Preparation method of heavy oil hydrodemetallization catalyst

Through rolling ball molding and hydrothermal treatment technology, a catalyst with gradient distribution of spherical cavities and flaky alumina structures was prepared, which solved the problems of poor gradient distribution of existing catalyst pore channels and insufficient anti-carbon deposition ability, and improved the reaction activity of the catalyst. and stability.

CN118807764AActive Publication Date: 2024-10-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310417855.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-22
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

Existing heavy oil hydrodemetallization catalysts have deficiencies in pore gradient distribution and carbon deposition resistance, making it difficult to effectively accommodate metal impurities and improve catalytic activity stability.

Method used

Rolling ball forming technology is used to prepare spherical alumina carriers. Micron spherical activated carbon is impregnated with aluminum nitrate solutions and active metal components of different concentrations, combined with sealing heat treatment of propylene oxide aqueous solution to form gradient distribution of spherical cavities and flaky alumina crystals. particles to improve the pore structure of the catalyst and the directional distribution of active metals.

Benefits of technology

It achieves the opening of large pores on the surface of the catalyst, enhances the diffusion ability of reactants, improves the hydrodemetallization, desulfurization activity and carbon deposition resistance of the catalyst, and ensures activity stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807764A_ABST
    Figure CN118807764A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a heavy oil hydrotreating catalyst, which comprises the following steps: (1) uniformly mixing pseudo-boehmite P1 and a physical pore-enlarging agent, and rolling to obtain a spherical precursor S0; (2) uniformly mixing pseudo-boehmite P2 and activated carbon Q1 impregnated with aluminum nitrate and active metal components to obtain W1, mixing W1 with S0, and rolling to obtain a spherical precursor S1; (3) uniformly mixing pseudo-boehmite P3 and activated carbon Q2 impregnated with a proper amount of aluminum nitrate and active metal components to obtain W2, mixing W2 with S1, and rolling to obtain a precursor S2; and (4) immersing the S2 into an epoxy propane aqueous solution, carrying out sealed heat treatment, carrying out solid-liquid separation, drying and roasting to obtain an alumina carrier, and loading a hydrogenation active component to obtain a catalyst product. The catalyst is rich in spherical cavities, macropores are in gradient distribution from outside to inside, the spherical cavities are high in catalytic activity, and the catalyst is suitable for the field of heavy oil hydrotreatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst preparation, and specifically relates to a method for preparing a heavy oil hydrodemetallization catalyst. Background Art

[0002] The fixed bed residue oil hydrogenation process technology is mature and widely used. It is an effective means to achieve efficient conversion of heavy oil. Residue oil is enriched with most of the sulfur, nitrogen, metals (mainly nickel and vanadium) in crude oil. Residue oil hydrogenation removes impurities such as metals, sulfur, and nitrogen under high temperature and high pressure conditions through the action of catalysts, providing high-quality raw materials for downstream catalytic cracking. At present, residue oil hydroprocessing catalysts usually include protective catalysts, demetallization catalysts, desulfurization catalysts, and denitrification catalysts. Among them, the role of the residue oil hydrogenation demetallization catalyst is to remove metals such as Ni and V in the residue oil, and at the same time protect the desulfurization catalyst. It not only removes metal impurities in the feed, but also must accommodate as many of these metals and coke impurities as possible.

[0003] CN104646008A discloses a catalyst for demetallization of inferior heavy oil by hydrodesulfurization and a preparation method thereof. The catalyst uses alumina as a carrier, and group VIII and VIB elements, especially Ni-Mo, as active components. The catalyst has a pore volume of 0.61-0.70 mL / g and a specific surface area of ​​155-200 m 2 / g, and the average pore diameter is 13.0-18.0nm. The preparation method of the catalyst is to treat the carrier particles after forming and calcining with an acid solution with continuously increasing concentration. Although this method can make the average pore diameter of the final catalyst gradually increase along the radial direction of the catalyst particles from the center to the outer surface, this treatment method is difficult to form larger pores on the carrier surface.

[0004] CN106669853A discloses a method for preparing a spherical modified alumina carrier. The spherical modified alumina carrier has the following properties: it has a dual pore distribution, with pore diameters of 10-15nm and 15-30nm; wherein the pore distribution of 10-15nm accounts for 35%-40% of the total pore volume, and the pore distribution of 15-30nm accounts for 30%-35% of the total pore volume; based on the weight of the carrier, the additive accounts for 2%-5% in terms of elemental amount, and the additive concentration gradually increases from the center of the carrier particle to the outer surface, wherein the additive content at 1 / 4R is 0.5wt%-1.0wt%, the additive content at 1 / 2R is 1.5wt%-2.0wt%, and the additive content at R is 2.5%wt-3.0wt%, wherein R is the radius of the carrier particle with the center of the spherical modified alumina carrier as the initial point; wherein the additive is one of the following combinations of I, II and III: I-fluorine and phosphorus, II-fluorine and boron, III-fluorine, phosphorus and boron. The alumina carrier additive prepared by this method has a gradient distribution, but the pore gradient distribution is poor, which is not conducive to the diffusion of macromolecular reactants.

[0005] CN110935461A discloses a method for preparing a heavy oil hydrogenation demetallization catalyst. The method for preparing the catalyst comprises: (1) kneading a physical pore expander, pseudo-boehmite and an active metal component, drying and calcining to obtain a modified alumina carrier SI; (2) spraying SI with an unsaturated impregnation solution I for the hydrogenation active component, and then drying and calcining to obtain a modified alumina carrier SII; (3) mixing SII, ammonium bicarbonate and water, and then performing a sealed heat treatment, and drying and calcining the material after the heat treatment to obtain a carrier SIII; (4) supersaturating the hydrogenation active component impregnation solution II for the carrier SIII, and then drying and calcining to obtain a catalyst. The surface of the catalyst prepared by this method has a rod-like structure, and the formed pores are open, which improves the catalyst's resistance to metal deposition and carbon deposition, but the rod-like alumina grown on the surface is easy to fall off, and the firmness of the bond with the main alumina needs to be further improved. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing a heavy oil hydroprocessing catalyst. The catalyst is rich in spherical cavities, and the macropores are distributed in a gradient from the surface to the inside, which is beneficial for the diffusion of reactant molecules into the interior of the catalyst. The spherical cavities have high catalytic activity, and are strong in accommodating metal impurities and resisting carbon deposition. The catalyst has high hydrodemetallization and desulfurization activity and activity stability, and is suitable for the field of heavy oil hydroprocessing.

[0007] The preparation method of the heavy oil hydroprocessing catalyst of the present invention comprises the following contents: (1) pseudo-boehmite P1 and a physical pore-enlarging agent are mixed evenly, and a spherical precursor S0 is obtained by rolling and forming; (2) pseudo-boehmite P2 and a proper amount of micron spherical activated carbon Q1 impregnated with aluminum nitrate solution A and active metal component solution I are mixed evenly to obtain material W1, and material W1 is mixed with spherical precursor S0, and a spherical precursor S1 is obtained by rolling and forming; (3) pseudo-boehmite P3 and The micron spherical activated carbon Q2 impregnated with appropriate amounts of aluminum nitrate solution B and active metal component solution II is mixed evenly to obtain material W2, and the material W2 is mixed with the spherical precursor S1, and rolled into a ball, and then dried and calcined to obtain the precursor S2; (4) the precursor S2 of step (3) is immersed in a propylene oxide aqueous solution for sealed heat treatment, and the material after treatment is subjected to solid-liquid separation, and the solid phase material is dried and calcined to obtain an alumina carrier, which is then loaded with the hydrogenation active component to obtain a catalyst product.

[0008] In the method of the present invention, the ball forming is carried out in a turntable forming machine, and the rotation operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70º, the rotation speed of the turntable is 10-30rpm; the forming time of the material in the turntable is 5-120min. The radius of the spherical precursor S0 is 0.2r-0.6r, and the radius of the spherical precursor S1 is 0.5r-0.8r, wherein r is the radius of the final spherical alumina material, that is, the straight-line distance from the center of the sphere to the outer surface. During the forming process, an aqueous solution containing a gelling agent is sprayed into the material; the aqueous solution containing a gelling agent is one or a mixture of aqueous solutions of nitric acid, phosphoric acid, oxalic acid, and acetic acid, and the mass concentration of the solution is 1%-3%, preferably an aqueous solution of acetic acid.

[0009] In the method of the present invention, the pseudo-boehmite P1 particles described in step (1) are in granular form and can be a commercially available product or pseudo-boehmite prepared by methods such as acid precipitation, alkali precipitation, alcohol aluminum hydrolysis, etc., preferably pseudo-boehmite with a pore size of 8.5-10 nm.

[0010] In the method of the present invention, the physical pore expanding agent in step (1) is one or more of activated carbon, sawdust, carbon black, urea, propylene glycol glycerol, triethylene glycol, melamine, polyethylene glycol, polyethylene oxide, methyl cellulose, polyoxyethylene, polyacrylamide and starch. The mass ratio of the physical pore expanding agent to the pseudo-boehmite P1 is 1:20-1:10.

[0011] In the method of the present invention, the concentration of the aluminum nitrate solution A in step (2) is 10wt%-20wt%, and the amount of the solution is such that the micron-shaped spherical activated carbon is adsorbed saturatedly.

[0012] In the method of the present invention, the active metal component solution I described in step (2) is a solution containing molybdenum and nickel, the concentration of molybdenum in the solution is 1.5-3 g / 100 mL in the form of molybdenum oxide, and the concentration of nickel in the form of nickel oxide is 0.4-1 g / 100 mL, and the amount of solution used is such that the micron-shaped spherical activated carbon is adsorbed saturatedly.

[0013] In the method of the present invention, there is no special requirement for the impregnation order of the aluminum nitrate solution A and the active metal component solution I in step (2). The aluminum nitrate solution A can be impregnated first and then the active metal component solution I, or the active metal component solution I can be impregnated first and then the aluminum nitrate solution A. After each impregnation, the micron spherical activated carbon generally needs to be dried at a drying temperature of 60-160° C. and a drying time of 1-5 hours.

[0014] In the method of the present invention, the pseudo-boehmite P2 particles in step (2) are in granular form, preferably with a pore size of 10-15 nm, and the diameter of the micron spherical activated carbon Q1 is 1-5 microns. The micron spherical activated carbon can be prepared by existing methods or purchased, and the mass ratio of the micron spherical activated carbon to the pseudo-boehmite P2 is 1:6.7-1:12.5.

[0015] In the method of the present invention, the pseudo-boehmite P3 particles in step (3) are in granular form, preferably pseudo-boehmite with a pore size greater than 15 nm, and the pseudo-boehmite can be prepared using existing technology or purchased.

[0016] In the method of the present invention, the concentration of the aluminum nitrate solution B in step (3) is 20wt%-30wt%, and the amount of the solution is such that the micron-shaped spherical activated carbon is saturated with adsorption.

[0017] In the method of the present invention, the active metal component solution II described in step (3) is a solution containing molybdenum and nickel, the concentration of molybdenum oxide in the solution is 3-4.5 g / 100 mL, the concentration of nickel oxide is 0.8-1.2 g / 100 mL, and the amount of solution used is to saturate the adsorption of the micron-shaped spherical activated carbon.

[0018] In the method of the present invention, there is no special requirement for the impregnation order of the aluminum nitrate solution B and the active metal component solution II in step (3). The aluminum nitrate solution B can be impregnated first and then the active metal component solution II, or the active metal component solution II can be impregnated first and then the aluminum nitrate solution B. After each impregnation, the micron spherical activated carbon generally needs to be dried at a drying temperature of 60-160° C. and a drying time of 1-5 hours.

[0019] In the method of the present invention, the diameter of the micron spherical activated carbon Q2 in step (3) is 5-10 microns. The micron spherical activated carbon can be prepared by existing methods or purchased. The mass ratio of the micron spherical activated carbon to pseudo-boehmite P3 is 1:5-1:10.

[0020] In the method of the present invention, the drying temperature in step (3) is 100-160° C., the drying time is 2-8 hours, and the calcination is carried out in an oxygen atmosphere, the calcination temperature is 450-600° C., and the calcination time is 4-8 hours.

[0021] In the method of the present invention, the mass percentage concentration of the propylene oxide aqueous solution in step (4) is 2.5%-12%, preferably 4%-8%, and the mass ratio of the propylene oxide aqueous solution to the alumina carrier precursor is 3:1-10:1, preferably 4:1-8:1.

[0022] In the method of the present invention, the sealed heat treatment in step (4) is preferably carried out in a closed autoclave, and the sealed heat treatment is preferably a two-step sealed heat treatment, i.e., firstly a low-temperature sealed heat treatment at 60-100°C for 1-4 hours, and then a sealed heat treatment at 110-180°C, preferably 120-160°C, for 14-20 hours.

[0023] In the method of the present invention, the drying temperature in step (4) is 100-160°C, the drying time is 2-8 hours, the calcination temperature is 500-750°C, the calcination time is 4-8 hours, and the calcination is carried out in an oxygen-containing atmosphere, preferably in an air atmosphere.

[0024] In the method of the present invention, the loading method in step (4) can be an impregnation method, and the Mo content in the hydrogenation active component impregnation solution is 7.5%-13.5 g / 100 mL as metal oxide, and the Ni content is 2.1-4.5 g / 100 mL as metal oxide.

[0025] In the method of the present invention, the drying temperature in step (4) is 100-160° C., the drying time is 2-8 hours, the roasting temperature is 450-550° C., and the roasting time is 4-6 hours.

[0026] Compared with the prior art, the present invention has the following advantages: (1) In the process of rolling balls, the present invention adjusts the composition of the mixed material to obtain an alumina carrier precursor with micron-sized spherical cavities in a gradient distribution. The alumina carrier precursor is placed in a propylene oxide aqueous solution for sealed hydrothermal treatment. During the low-temperature sealed hydrothermal treatment, the propylene oxide is hydrolyzed to form an alcohol solution, and the solution is weakly alkaline; during the high-temperature sealed hydrothermal treatment, the alumina carrier surface, the alumina grains on the surface of the micron-sized cavity, and the aluminum oxide compound formed after the aluminum nitrate is roasted in the micron-sized cavity grow in situ to form flaky alumina grains in an alkaline and alcohol solution environment. The flaky alumina on the outer surface of the carrier accumulates to form open channels of 40-300nm, and the flaky alumina in the micron-sized cavity accumulates to form through channels of 50-100nm. This channel structure is conducive to the diffusion of macromolecular reactants into the interior of the carrier.

[0027] (2) The present invention uses aluminum nitrate solutions and solutions containing active metal components of different concentrations to impregnate micron-sized spherical activated carbons. During calcination, aluminum nitrate decomposes to form corresponding aluminum oxide compounds and active metal components, which are anchored in the micron-sized spherical cavities of the carrier. During in-situ growth by hydrothermal treatment, the active metal components cooperate with the rehydration process of alumina grains, thereby improving the interaction between the active metal components and the alumina carrier and enhancing the activity of the catalyst.

[0028] (3) Through the directional regulation of active metal components and flaky alumina, the active metal content in the pores formed by the accumulation of flaky particles in the spherical cavity of the catalyst is increased. The active metal components are highly matched with the catalyst pore structure, making the catalyst have higher activity and higher resistance to metal deposition. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the SEM image of the outer surface of the alumina carrier prepared in Example 1.

[0030] Figure 2 This is the SEM image of the cross section of the alumina support prepared in Example 1.

[0031] Figure 3 This is the SEM image of the outer surface of the alumina support prepared in Comparative Example 2.

[0032] Figure 4 This is the SEM image of the cross section of the alumina support prepared in Comparative Example 2. DETAILED DESCRIPTION

[0033] The technical scheme and technical effect of the present invention are further described below in conjunction with the embodiments, but are not limited to the following embodiments. In the present invention, wt% represents mass fraction.

[0034] Scanning electron microscopy was used to characterize the microstructure of the alumina carrier. The specific operation was as follows: a JSM-7500F scanning electron microscope was used to characterize the microstructure of the carrier, with an accelerating voltage of 5 KV, an accelerating current of 20 µA, and a working distance of 8 mm.

[0035] The micro-region composition of the sample was characterized by using a scanning electron microscope-energy spectrometer. The specific operation was as follows: a JSM-7500F scanning electron microscope equipped with an EDAX energy spectrometer was used, with an accelerating voltage of 30 kV, a probe current of 11µA, and a working distance of 8mm. During the measurement, the catalyst particles were cut and adhered to the scanning electron microscope sample stage so that the cross section of the catalyst particles was perpendicular to the electron beam direction of the scanning electron microscope. In the experiment, 20 granular particle micro-regions and spherical cavity micro-regions were selected as the measurement areas, and the contents of molybdenum oxide and nickel oxide in the corresponding areas were measured and the average values ​​were taken.

[0036] The molybdenum and nickel content of the catalyst bulk phase was determined according to the method described in the literature ICP-AES determination of the content of metal elements in molybdenum-nickel series hydrogenation catalysts, Guangzhou Chemical Industry, 2021, 49, (17): 129-130.

[0037] Preparation of micron spherical activated carbon: The micron spherical activated carbon used in the method of the present invention is according to the literature: Dai Linlin, Li Wei, Wu Qiong, et al. Hydrothermal carbonization of carboxymethyl cellulose-CO 2 Preparation of micron-shaped spherical activated carbon by activation [J]. Chemistry and Industry of Forest Products, 2015, 35 (4): 21-27. The prepared micron-shaped spherical activated carbon has a diameter of 1-5 microns and 5-10 microns. Example 1

[0038] Mix 32 g of methyl cellulose and 200 g of pseudo-boehmite (pore size 10 nm) evenly. The mixed material was placed in a rotating disk molding machine for full mixing, the inclination angle of the rotating disk was adjusted to 45°, and the rotating speed of the rotating disk was 15 rpm; an acetic acid aqueous solution with a mass concentration of 1% was sprayed onto the material in the rotating disk through a sprayer for mixed contact, and the molding time of the material in the rotating disk was 25 minutes to obtain a spherical precursor S0; (2) Weigh 20 grams of spherical activated carbon with a diameter of 1-5 microns, impregnate it with a 16.5wt% aluminum nitrate solution to saturate the activated carbon adsorption, and dry the material at 80°C for 4 hours after adsorption; then impregnate the spherical activated carbon with a Mo-Ni-P solution with a molybdenum oxide concentration of 2.1g / 100mL and a nickel oxide concentration of 0.5g / 100mL to saturate the adsorption, and dry the material at 80°C for 4 hours after adsorption. Mix the dried micron spherical activated carbon with 200 grams of pseudo-boehmite (pore size 15nm), place the mixed material and the spherical precursor S0 prepared in step (1) in a turntable molding machine for thorough mixing, adjust the inclination angle of the turntable to 45º, the speed of the turntable to 15rpm, spray an acetic acid aqueous solution with a mass concentration of 1% on the material in the turntable through a sprayer, and after mixing and contacting, the material is molded in the turntable for 25min to obtain a spherical precursor S1; (3) Weigh 29g of activated carbon with a diameter of 5-10 microns, impregnate it with a 27.5wt% aluminum nitrate solution to saturate the activated carbon with adsorption, and dry the material at 80°C for 4 hours after adsorption; then impregnate the spherical activated carbon with a Mo-Ni-P solution with a molybdenum oxide concentration of 4.2g / 100mL and a nickel oxide concentration of 1.1g / 100mL to saturate the adsorption, and dry the material at 80°C for 4 hours after adsorption. The dried micron spherical activated carbon is mixed with 200g of pseudo-boehmite (pore size 17.5nm), and the mixed material and the spherical precursor S1 prepared in step (2) are placed in a turntable molding machine for full mixing. The inclination angle of the turntable is adjusted to 45°, and the rotation speed of the turntable is adjusted to 15rpm. A 1% mass concentration of acetic acid aqueous solution is sprayed onto the material in the turntable through a sprayer. After mixing and contacting, the material is molded in the turntable for 20min to obtain a spherical precursor S2. The obtained spherical precursor S2 was dried at 140°C for 6 hours and calcined at 550°C in an oxygen atmosphere for 6 hours to obtain an alumina carrier precursor.

[0039] (4) Weigh 100 g of the alumina carrier precursor prepared in step (3), add 580 g of a 6.6% propylene oxide aqueous solution, transfer the mixture into an autoclave, seal the autoclave and place it in an oven, first seal it at 80° C. for 3 hours, then heat it to 140° C. for 17.5 hours, wash and filter the material after cooling, dry the solid material at 140° C. for 6 hours, and calcine it at 650° C. in an air atmosphere for 6 hours to obtain an alumina carrier A1. The properties of the carrier are shown in Table 1, and the scanning electron microscope image of the outer surface of the carrier is shown in Table 1. Figure 1 , cross-sectional SEM images are shown in Figure 2 .

[0040] (5) Weigh 100 g of the alumina carrier prepared in step (4) and place it in a spray pot. Spray the alumina carrier with an active component impregnation solution having a molybdenum oxide concentration of 9.3 g / 100 mL and a nickel oxide concentration of 2.4 g / 100 mL in a saturated impregnation manner. The impregnated material is dried at 120° C. for 4 hours and calcined at 500° C. for 5 hours to obtain the hydrodemetallization catalyst Cat-1 of the present invention. The catalyst properties are shown in Table 1. Example 2

[0041] The same as Example 1, except that the amount of methyl cellulose added in step (1) is 28 grams; the concentration of aluminum nitrate solution in step (2) is 10.5wt%, the concentration of molybdenum oxide in Mo-Ni-P solution is 1.8g / 100mL, the concentration of nickel oxide is 0.5g / 100mL, and the amount of micron spherical activated carbon added is 23 grams; the concentration of aluminum nitrate solution in step (3) is 29wt%, the concentration of molybdenum oxide in Mo-Ni-P solution is 4.4g / 100mL, the concentration of nickel oxide is 1.2g / 100mL, and the amount of micron spherical activated carbon added is 33 grams. In step (4), the concentration of propylene oxide is 5.2%, the amount of solution is 660 grams, and during hydrothermal treatment, it is first sealed and treated at 90°C for 2 hours, then heated to 150°C, and the treatment time is 16.5 hours to obtain the hydrodemetallization catalyst Cat-2 of the present invention. The catalyst properties are shown in Table 1. Example 3

[0042] The same as Example 1, except that the amount of methyl cellulose added in step (1) is 36 grams; the concentration of aluminum nitrate solution in step (2) is 13.5wt%, the concentration of molybdenum oxide in Mo-Ni-P solution is 2.5g / 100mL, the concentration of nickel oxide is 0.6g / 100mL, and the amount of micron spherical activated carbon added is 18 grams; the concentration of aluminum nitrate solution in step (3) is 25wt%, the concentration of molybdenum oxide in Mo-Ni-P solution is 3.9g / 100mL, the concentration of nickel oxide is 1.0g / 100mL, and the amount of micron spherical activated carbon added is 38 grams. In step (4), the concentration of propylene oxide is 7.4%, the amount of solution is 480 grams, and during the hydrothermal treatment, it is first sealed at 70°C for 3.5 hours, then heated to 130°C, and the treatment time is 18.5 hours to obtain the hydrodemetallization catalyst Cat-3 of the present invention. The catalyst properties are shown in Table 1. Example 4

[0043] The same as Example 1, except that the amount of methyl cellulose added in step (1) is 24 grams; the concentration of aluminum nitrate solution in step (2) is 19.5wt%, the concentration of molybdenum oxide in Mo-Ni-P solution is 2.8g / 100mL, the concentration of nickel oxide is 0.7g / 100mL, and the amount of micron spherical activated carbon added is 26 grams; the concentration of aluminum nitrate solution in step (3) is 22.5wt%, the concentration of molybdenum oxide in Mo-Ni-P solution is 3.5g / 100mL, the concentration of nickel oxide is 0.9g / 100mL, and the amount of micron spherical activated carbon added is 25 grams. In step (4), the concentration of propylene oxide is 4.6%, the amount of solution is 710 grams, and during the hydrothermal treatment, it is first sealed at 100°C for 1.5 hours, then heated to 160°C, and the treatment time is 15.5 hours to obtain the hydrodemetallization catalyst Cat-4 of the present invention. The catalyst properties are shown in Table 1.

[0044] Comparative Example 1 The same method as Example 1 was used, except that the aqueous solution of propylene oxide in step (4) was replaced with an aqueous solution of ammonia of the same mass concentration to prepare comparative hydrodemetallization Cat-5. The catalyst properties are shown in Table 1.

[0045] Comparative Example 2 The same as Example 1, except that the propylene oxide aqueous solution in step (4) was replaced with an ethylene oxide solution of the same concentration, to prepare a comparative hydrodemetallization catalyst Cat-6. The catalyst properties are shown in Table 1. The morphology of the corresponding carrier is similar to that of the carrier precursor in Example 1, and no flaky structure is observed. The specific scanning electron microscopy image is shown in Figure 3 , cross-sectional SEM images are shown in Figure 4 .

[0046] Comparative Example 3 The same method as Example 1, except that the concentration of propylene oxide in step (4) was 1%, was used to prepare a comparative hydrodemetallization catalyst Cat-7. The catalyst properties are shown in Table 1.

[0047] Comparative Example 4 The same as Example 1, except that the micron spherical activated carbon is not impregnated with active metal components in step (2) and step (3), but the active metal components are loaded onto the carrier for the first time in step (5) to obtain a comparative hydrodemetallization agent catalyst Cat-8 with the same active metal content. The catalyst properties are shown in Table 1.

[0048] Table 1 Catalyst properties

[0049] From the data in Table 1 and Figure 1-4 It can be seen that compared with the comparative example, the hydrodemetallization catalyst prepared by the method of the present invention has a high content of macropores on the surface and wide pores. The flaky particles accumulate in the micron-sized spherical cavities inside the catalyst to form more pores of 50-100 nm, and the content of active metal components in the catalyst is well matched with the catalyst pores. Example

[0050] The hydrodemetallization catalysts Cat-1 to Cat-4 prepared by the present invention and the hydrodemetallization catalysts Cat-5 to Cat-8 prepared by the comparative example were respectively loaded into a fixed bed hydrogenation reactor, and the treated raw materials (see Table 2) were subjected to the following experimental conditions: reaction temperature 375°C, hydrogen to oil volume ratio 700, liquid hourly volume space velocity 0.8h -1 , hydrogen partial pressure 14.5MPa, continuous operation 2000 hours, impurity removal properties are shown in Table 3.

[0051] Table 2 Raw material properties

[0052] Table 3 Evaluation results of catalysts Hydrogenation protection catalyst Cat-1 Cat-2 Cat-3 Cat-4 Cat-5 Cat-6 Cat-7 Cat-8 Relative Ni+V removal rate, % 131 126 129 127 100 103 98 120 Relative S removal rate, % 126 129 124 125 100 99 105 115 From the results in Table 3, it can be seen that the hydrodemetallization catalyst prepared by the method of the present invention has high Ni and V demetallization activity, high desulfurization activity and good activity stability.

Claims

1. A preparation method of a heavy oil hydroprocessing catalyst, comprising the following contents: (1) pseudo-boehmite P1 and a physical pore-enlarging agent are mixed uniformly, and the mixture is subjected to ball rolling to obtain a spherical precursor S0; (2) pseudo-boehmite P2 and a proper amount of micron-shaped spherical activated carbon Q1 impregnated with aluminum nitrate solution A and active metal component solution I are mixed uniformly to obtain material W1, and material W1 is mixed with spherical precursor S0, and ball rolling is performed to obtain spherical precursor S1; (3) pseudo-boehmite P3 and The micron spherical activated carbon Q2 impregnated with appropriate amounts of aluminum nitrate solution B and active metal component solution II is mixed evenly to obtain material W2, and the material W2 is mixed with the spherical precursor S1, and rolled into a ball, and then dried and calcined to obtain the precursor S2; (4) the precursor S2 of step (3) is immersed in a propylene oxide aqueous solution for sealed heat treatment, and the material after treatment is subjected to solid-liquid separation, and the solid phase material is dried and calcined to obtain an alumina carrier, which is then loaded with the hydrogenation active component to obtain a catalyst product.

2. The method according to claim 1, characterized in that: The pseudo-boehmite P1 particles in step (1) are in the form of granules, preferably pseudo-boehmite with a pore size of 8.5-10 nm.

3. The method according to claim 1, characterized in that: The physical pore-enlarging agent in step (1) is one or more of activated carbon, sawdust, carbon black, urea, propylene glycol, glycerol, triethylene glycol, melamine, polyethylene glycol, polyethylene oxide, methyl cellulose, polyoxyethylene, polyacrylamide and starch. The mass ratio of the physical pore-enlarging agent to the pseudo-boehmite P1 is 1:20-1:

10.

4. The method according to claim 1, characterized in that: The radius of the spherical precursor S0 in step (1) is 0.2r-0.6r, and the radius of the spherical precursor S1 is 0.5r-0.8r, where r is the radius of the alumina carrier, that is, the straight-line distance from the center of the sphere to the outer surface.

5. The method according to claim 1, characterized in that: The concentration of the aluminum nitrate solution A in step (2) is 10wt%-20wt%, and the amount of the solution is such that the micron-shaped spherical activated carbon is adsorbed saturatedly.

6. The method according to claim 1, characterized in that: The active metal component solution I described in step (2) is a solution containing molybdenum and nickel, wherein the concentration of molybdenum in the solution is 1.5-3 g / 100 mL in the form of molybdenum oxide, and the concentration of nickel in the form of nickel oxide is 0.4-1 g / 100 mL, and the amount of the solution is such that the micron-shaped spherical activated carbon is adsorbed saturatedly.

7. The method according to claim 1, characterized in that: The pseudo-boehmite P2 particles in step (2) are granular, preferably with a pore size of 10-15 nm; the diameter of the micron spherical activated carbon Q1 is 1-5 microns, and the mass ratio of the micron spherical activated carbon to the pseudo-boehmite P2 is 1:6.7-1:12.

5.

8. The method according to claim 1, characterized in that: The pseudo-boehmite P3 particles in step (3) are in the form of granules, preferably pseudo-boehmite with a pore size greater than 15 nm.

9. The method according to claim 1, characterized in that: The concentration of the aluminum nitrate solution B in step (3) is 20wt%-30wt%, and the amount of the solution is such that the micron-shaped spherical activated carbon is adsorbed saturatedly.

10. The method according to claim 1, characterized in that: The active metal component solution II described in step (3) is a solution containing molybdenum and nickel, wherein the concentration of molybdenum oxide in the solution is 3-4.5 g / 100 mL, and the concentration of nickel oxide is 0.8-1.2 g / 100 mL. The amount of solution used is such that the micron-shaped spherical activated carbon is adsorbed saturatedly.

11. The method according to claim 1, characterized in that: The diameter of the micron spherical activated carbon Q2 in step (3) is 5-10 microns, and the mass ratio of the micron spherical activated carbon to the pseudo-boehmite P3 is 1:5-1:

10.

12. The method according to claim 1, characterized in that: The drying temperature in step (3) is 100-160°C, and the drying time is 2-8 hours; the calcination is carried out in an oxygen atmosphere, the calcination temperature is 450-600°C, and the calcination time is 4-8 hours.

13. The method according to claim 1, characterized in that: The mass percentage concentration of the propylene oxide aqueous solution in step (4) is 2.5%-12%; the mass ratio of the propylene oxide aqueous solution to the alumina carrier precursor is 3:1-10:

1.

14. The method according to claim 1, characterized in that: The sealing heat treatment process described in step (4) is: first, sealing heat treatment is performed at a low temperature of 60-100°C for 1-4 hours, and then sealing heat treatment is performed at 110-180°C for 14-20 hours.

15. The method according to claim 1, characterized in that: The loading method in step (4) is an impregnation method, and the Mo content in the impregnation solution of the hydrogenation active component is 7.5%-13.5 g / 100 mL as metal oxide, and the Ni content is 2.1-4.5 g / 100 mL as metal oxide.

16. The method according to claim 1, characterized in that: The drying temperature in step (4) is 100-160°C, the drying time is 2-8 hours, the roasting temperature is 450-550°C, and the roasting time is 4-6 hours.

Citation Information

Patent Citations

  • Hydrotreating catalyst as well as preparation method and application thereof

    CN103801314A

  • Hydrogenation catalyst as well as preparation method and application thereof

    CN104549430A

  • High-dispersion particle catalyst applied to synthesis of hydrogen peroxide as well as preparation method and application thereof

    CN107008492A

  • Hydro-denitrification catalyst and application thereof

    CN110404552A

  • Preparation method of spherical alumina carrier

    CN111822057A