Carbon-based supported low-temperature section denitration catalyst suitable for biomass combustion flue gas, preparation method and application

By loading carbon-based catalysts with Mn, Cu and Nb components on coconut shell carbon carriers, the problems of high NOx and alkaline earth metal poisoning in biomass boiler flue gas are solved, and efficient nitrogen oxide removal and resistance in the low-temperature section are achieved. Alkaline, meeting the denitrification needs of biomass combustion flue gas.

CN118807771AInactive Publication Date: 2024-10-22DONGYING URBAN CONSTRUCTION DEVELOPMENT GROUP CO LTD +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410943068.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The high NOx content and high alkaline earth metal content in the flue gas of biomass boilers make the existing catalysts inefficient and prone to poisoning during the denitration process, making it difficult to meet the demand for efficient denitration of biomass combustion flue gas.

Method used

Coconut shell carbon is used as a carrier to load Mn, Cu and Nb active components. A carbon-based supported low-temperature denitrification catalyst is prepared through a specific process. The low-temperature denitrification performance of Mn and Cu and the alkaline resistance of Nb are used to improve the denitrification of the catalyst. Efficiency and resistance to alkali.

Benefits of technology

It achieves efficient removal of NOx in biomass flue gas under low temperature conditions. It has good alkali resistance and high nitrogen oxide removal rate in the low temperature section. The process is simple and low-cost. The recycling of used catalysts does not produce secondary pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807771A_ABST
    Figure CN118807771A_ABST
Patent Text Reader

Abstract

The invention provides a carbon-based supported low-temperature section denitration catalyst suitable for biomass combustion flue gas as well as a preparation method and application thereof, belongs to the technical field of flue gas denitration catalysts, and can solve the problems that the content of alkaline earth metal in the flue gas of a biomass boiler is relatively high, the components of the flue gas are variable and the content of NOx is relatively high. According to the carbon-based supported low-temperature section denitration catalyst suitable for the biomass combustion flue gas, coconut shell charcoal serves as a carrier, manganese-copper-niobium composite oxide serves as an active substance, a precursor of manganese oxide is manganous nitrate, a precursor of copper oxide is copper sulfate pentahydrate, a precursor of niobium oxide is niobium nitrate hexahydrate, and a precursor of carbon-based supported low-temperature section denitration catalyst suitable for the biomass combustion flue gas serves as an active substance. And the molar ratio of manganese to copper to niobium in the precursor is 7: 3: 0.05. The catalyst can be applied to biomass fuel combustion smoke dust purification, the effect in SCR application is outstanding, the removal rate of nitrogen oxide in the low-temperature section is high, the manufacturing process is simple and convenient, the cost is low, and secondary pollution cannot be generated in waste catalyst recovery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of flue gas denitration catalysts, and in particular relates to a carbon-based loaded low-temperature denitration catalyst specially suitable for biomass boiler flue gas and suitable for biomass combustion flue gas, a preparation method and an application thereof. Background Art

[0002] Biomass energy is one of the important energy sources for human survival. It is the fourth largest energy source after coal, oil and natural gas, and occupies an important position in the entire energy system. The use of biomass energy can effectively reduce carbon emissions, but due to the high content of nitrogen in biomass fuel, it produces more nitrogen oxides during combustion. NOx emissions during biomass fuel combustion depend largely on the type of fuel, combustion equipment and technology, and emission control measures. When biomass fuel is burned under high temperature conditions, such as in some industrial combustion equipment or high-temperature combustion furnaces, the generation of NOx may increase; the structural design and operation of the combustion equipment will also affect the emission level of NOx. If the combustion equipment is not efficient or improperly controlled, it may lead to increased NOx emissions. With the popularization and application of large-scale biomass boilers, the NOx emission problem of biomass combustion flue gas has received more and more attention. At present, the NOx emissions during biomass combustion are effectively reduced and the environmental friendliness of the combustion process is improved mainly through the adoption of advanced combustion technology, optimization design of combustion equipment, selection of low-nitrogen combustion technology, use of NOx adsorbents and selection of appropriate NOx emission control equipment.

[0003] Flue gas denitrification technology mainly includes post-denitrification treatment of flue gas and combustion process control, and the selective catalytic reduction (SCR) method is currently the most widely used, mature technology and excellent denitrification performance method. At present, the commercial catalyst is mainly vanadium-titanium catalyst. For coal-fired equipment in large power plants, vanadium-titanium catalysts can play a good catalytic role. However, since the flue gas of biomass boilers is different from that of coal-fired boilers, the N content of biomass fuels is closely related to the type of biomass. For example, the NOx emission of wood pellet fuel is 337.4mg / Nm 3 Corn straw pellet fuel is 601.3mg / Nm 3 Therefore, biomass boiler flue gas has higher requirements for catalysts and requires high denitrification efficiency within different NOx content ranges; moreover, elements such as K and Ca with high alkaline earth metal content in biomass enter the flue gas during the combustion process and will adhere to the surface of the catalyst, causing alkaline earth metal poisoning of the catalyst. Therefore, the poisoning effect of alkaline earth metals on the catalyst must also be considered during the denitrification process of biomass boiler flue gas. Summary of the invention

[0004] The present invention aims at the technical problems in the prior art that the flue gas of the biomass boiler has a high alkaline earth metal content, variable flue gas components and a high NOx content, and proposes a carbon-based loaded low-temperature denitrification catalyst suitable for biomass combustion flue gas, a preparation method and an application. The catalyst uses coconut shell charcoal as a carrier, and is first loaded with Mn and Cu ions, and then loaded with Nb active components in combination with a specific process. The obtained catalyst has outstanding effects in SCR applications, a high nitrogen oxide removal rate in the low-temperature stage, a simple manufacturing process, low cost, and the recycling of waste catalysts will not cause secondary pollution, and can be used for the purification of smoke from the combustion of biomass fuels.

[0005] In order to achieve the above-mentioned purpose, the present invention provides a carbon-based supported low-temperature denitrification catalyst suitable for biomass combustion flue gas, with coconut shell charcoal as a carrier and manganese, copper and niobium composite oxide as an active substance, wherein the precursor of manganese oxide is manganese nitrate, the precursor of copper oxide is copper sulfate pentahydrate, and the precursor of niobium oxide is niobium nitrate hexahydrate, and the molar ratio of manganese, copper and niobium elements in the precursor is 7:3:0.05.

[0006] Coconut shell charcoal has a high specific surface area and good chemical stability under low temperature conditions. The active substances Mn and Cu oxides have excellent low-temperature denitrification performance, and Nb has a significant optimization performance on the alkali resistance of the catalyst. The reactive substance Mn has good performance in the low temperature section. Due to the rich valence of Mn, it will exist on the carrier surface in the form of a variety of different oxides, providing a wealth of active sites on the carrier surface; Cu has excellent denitrification performance in the medium and low temperature sections. The co-loading of Mn and Cu can achieve the diversification of surface active components. The multi-component mixed loading can achieve the electron migration transformation between components to adjust the surface metal valence and enhance the surface redox performance; Nb is a substance with strong alkali resistance. The loading of Nb will achieve synergistic catalysis with the surface Mn and Cu while improving the surface alkali resistance. By adsorbing alkaline earth metals and regulating the surface reaction process, Nb can effectively improve the denitrification efficiency of alkaline flue gas; Therefore, loading the three components of Mn, Cu, and Nb on the surface of the carbon-based catalyst can meet the denitrification needs of biomass flue gas under low temperature conditions, and at the same time have good alkali resistance.

[0007] Preferably, the loading amount of active substances such as manganese and copper is 5% to 10%.

[0008] Another aspect of the present invention provides a method for preparing the above-mentioned carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas, comprising the following steps:

[0009] S1, activating the coconut shell charcoal with nitric acid to obtain a nitric acid-modified biocarbon-based carrier;

[0010] S2, fully dissolving Mn(NO3)2 and CuSO4·5H2O in deionized water, then immersing the biocarbon-based carrier modified by nitric acid in the above solution, ultrasonically treating at room temperature, heating in a water bath and stirring until the solvent is completely evaporated, and then drying and calcining in anoxic condition to obtain a catalyst loaded with Mn and Cu components;

[0011] S3. Fully dissolve Nb(NO3)2·6H2O in deionized water, and then immerse the catalyst loaded with Mn and Cu components in the above solution. After ultrasonic treatment at room temperature, heat in a water bath and stir until all the solvent evaporates. Then, dry, calcine in anoxic conditions, crush, and screen to obtain a carbon-based loaded low-temperature denitrification catalyst suitable for biomass combustion flue gas.

[0012] Preferably, step S1 comprises the following specific steps: crushing the coconut shell charcoal into particles of 20-40 mesh, washing and drying, pouring into a nitric acid solution with a concentration of 15-20% and stirring evenly, and soaking it in a water bath at 70-80°C for 4-5 hours, and then repeatedly washing the obtained acid-soaked sample with deionized water until it is neutral, and drying it at 100-105°C for 10-12 hours. In step S1, a certain concentration of nitric acid is used to acidify and expand the coconut shell charcoal to enhance its activity.

[0013] Preferably, the ultrasonic treatment time in step S2 and step S3 is 30 min.

[0014] Preferably, the water bath in step S2 and step S3 is carried out in a constant temperature magnetic heating stirrer, the water bath temperature is 70-80° C., and the stirring time is 4-5 h.

[0015] Preferably, the drying temperature in step S2 and step S3 is 100-105° C., and the drying time is 10-12 h.

[0016] Preferably, the anaerobic calcination in step S2 and step S3 is carried out in a tubular furnace in a N2 atmosphere, starting from room temperature, with a heating rate of 10°C / min, a maximum calcination temperature of 400-450°C, a maximum calcination time of 3-4h, and a total calcination time of 4-5h.

[0017] Preferably, the carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas obtained in step S3 has a particle size of 20 to 40 meshes.

[0018] The present invention discloses an application of the carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas in the purification of biomass fuel combustion smoke.

[0019] Compared with the prior art, the advantages and positive effects of the present invention are as follows: the carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas of the present invention adopts coconut shell charcoal as a carrier, which has a large specific surface area and strong adsorption performance, and has a wide source of raw materials, low price, and is suitable for large-scale industrial production; Mn and Cu are used as the main active substances, and are prepared by impregnation, which can meet the denitration requirements of biomass flue gas under low temperature conditions, and at the same time, the activity is modified by adding Nb to improve the alkali resistance; the carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas of the present invention can be used for smoke purification of biomass fuel combustion, has outstanding effects in SCR applications, has a high nitrogen oxide removal rate in the low temperature section, has a simple manufacturing process, low cost, and the recovery of waste catalysts will not cause secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a schematic structural diagram of a catalyst activity testing device according to an embodiment of the present invention;

[0021] Figure 2 It is a line graph of NOx conversion rate of the catalysts prepared in the examples and comparative examples at different temperatures when testing catalytic activity;

[0022] Figure 3 It is a line graph of NOx conversion rate at different temperatures of the catalyst K poisoned by the examples and comparative examples when testing the catalytic activity;

[0023] In the attached figure: 11, NO / N2 mixed gas, 12, O2 / N2 mixed gas, 13, high-purity nitrogen, 14, NH3 / N2 mixed gas, 2, pressure gauge, 3, pressure reducing valve, 4, gas flow meter, 5, mixer, 6, tubular furnace, 7, insulation layer, 8, catalyst layer, 9, filter, 10, flue gas analyzer. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] In order to more clearly and in detail introduce the carbon-based supported low-temperature denitrification catalyst suitable for biomass combustion flue gas, preparation method and application provided in the embodiments of the present invention, the following description will be made in conjunction with specific embodiments, wherein % in the following embodiments are all mass percentage symbols unless otherwise specified.

[0026] Example 1

[0027] The preparation method of the carbon-based supported low-temperature denitration catalyst for biomass combustion flue gas in this embodiment specifically comprises the following steps:

[0028] 30g of coconut shell charcoal was poured into 20% nitric acid for activation, and then placed in a water bath at 80°C for 4h, and then the acid-soaked sample was repeatedly washed with deionized water until neutral, and then dried at 105°C for 12h;

[0029] Dissolve 6.5g Mn(NO3)2 and 3.9g CuSO4·5H2O in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ and treat for 30min to fully dissolve the solute; put the treated coconut shell charcoal into the above solution, raise the water bath temperature to 80℃, and adjust the rotor speed to 450r / min until all the solvent in the beaker evaporates; then place it in a drying oven for drying at 105℃ for 12h; after drying, a solid catalyst is obtained, the catalyst block is crushed, ground and screened out particles of 20-40 mesh for standby use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature 25℃ at a rate of 10℃ / min. After reaching 400℃, the calcination is carried out at a constant temperature for 4h to obtain a catalyst loaded with Mn and Cu components;

[0030] Weigh 0.55gNb(NO3)2·6H2O and dissolve it in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ for 30min to fully dissolve the solute; put the catalyst loaded with Mn and Cu components into the above solution, and at the same time increase the water bath temperature to 80℃, and adjust the rotor speed to 450r / min until all the solvent in the beaker evaporates; then place it in a drying oven for drying at 105℃ for 12h; after drying, a solid catalyst is obtained, the catalyst block is crushed, ground and screened to obtain particles of 20-40 mesh for standby use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature 25℃ at a rate of 10℃ / min. After reaching 400℃, they are calcined at a constant temperature for 4h, and after crushing and screening, a low-temperature SCR denitration catalyst loaded with Mn, Cu and Nb is obtained;

[0031] In terms of metal content, in the catalyst prepared in this example, the mass ratio of the active material to the coconut shell carbon carrier is 1:10.

[0032] Example 2

[0033] The preparation method of the carbon-based supported low-temperature denitration catalyst for biomass combustion flue gas in this embodiment specifically comprises the following steps:

[0034] 30g of coconut shell charcoal was poured into 20% nitric acid for activation, and then placed in a water bath at 80°C for 4h, and then the acid-soaked sample was repeatedly washed with deionized water until neutral, and then dried at 105°C for 12h;

[0035] Dissolve 13gMn(NO3)2 and 7.8gCuSO4·5H2O in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ and treat for 30min to fully dissolve the solute; put the treated coconut shell charcoal into the above solution, raise the water bath temperature to 80℃, and adjust the rotor speed to 450r / min until all the solvent in the beaker evaporates; then place it in a drying oven for drying at 105℃ for 12h; after drying, a solid catalyst is obtained, the catalyst block is crushed, ground and screened out particles of 20-40 mesh for standby use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature 25℃ at a rate of 10℃ / min. After reaching 400℃, the charcoal is calcined at a constant temperature for 4h to obtain a catalyst loaded with Mn and Cu components;

[0036] Weigh 1.1g Nb(NO3)2·6H2O and dissolve it in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ for 30min to fully dissolve the solute; put the catalyst loaded with Mn and Cu components into the above solution, and at the same time increase the water bath temperature to 80℃, and adjust the rotor speed to 450r / min until all the solution in the beaker evaporates; then place it in a drying oven for drying at a temperature of 105℃ for 12h; after drying, a solid catalyst is obtained, the catalyst block is crushed, ground and screened to obtain particles of 20 to 40 mesh for standby use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature of 25℃ at a rate of 10℃ / min. After reaching 400℃, the catalyst is calcined at a constant temperature for 4h, and a low-temperature SCR denitration catalyst loaded with Mn, Cu and Nb is obtained after crushing and screening;

[0037] In terms of metal content, in the catalyst prepared in this example, the mass ratio of the active material to the coconut shell carbon carrier is 2:10.

[0038] Example 3

[0039] The preparation method of the carbon-based supported low-temperature denitration catalyst for biomass combustion flue gas in this embodiment specifically comprises the following steps:

[0040] 30g of coconut shell charcoal was poured into 20% nitric acid for activation, and then placed in a water bath at 80°C for 4h, and then the acid-soaked sample was repeatedly washed with deionized water until neutral, and then dried at 105°C for 12h;

[0041] Dissolve 17.5g Mn(NO3)2 and 10.7g CuSO4·5H2O in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ and treat for 30min to fully dissolve the solute; put the treated coconut shell charcoal into the above solution, raise the water bath temperature to 80℃, and adjust the rotor speed to 450r / min until all the solvent in the beaker evaporates; then place it in a drying oven for drying at 105℃ for 12h; after drying, a solid catalyst is obtained, the catalyst block is crushed, ground and screened out particles of 20-40 mesh for standby use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature 25℃ at a rate of 10℃ / min. After reaching 400℃, the calcination is carried out at a constant temperature for 4h to obtain a catalyst loaded with Mn and Cu components;

[0042] Weigh 1.65g Nb(NO3)2·6H2O and dissolve it in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ for 30min to fully dissolve the solute; put the catalyst loaded with Mn and Cu components into the above solution, and at the same time increase the water bath temperature to 80℃, and adjust the rotor speed to 450r / min until all the solvent in the beaker evaporates; then place it in a drying oven for drying at 105℃ for 12h; after drying, a solid catalyst is obtained, the catalyst block is crushed, ground and screened to obtain particles of 20-40 mesh for standby use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature 25℃ at a rate of 10℃ / min. After reaching 400℃, they are calcined at a constant temperature for 4h, and after crushing and screening, a low-temperature SCR denitration catalyst loaded with Mn, Cu and Nb is obtained;

[0043] In terms of metal content, in the catalyst prepared in this example, the mass ratio of the active material to the coconut shell carbon carrier is 3:10.

[0044] Comparative Example 1

[0045] The preparation method of the denitration catalyst in this comparative example specifically comprises the following steps:

[0046] 30g of bamboo charcoal was poured into 20% nitric acid for activation, and then soaked in a water bath at 80℃ for 4h, and then the acid-soaked sample was repeatedly washed with deionized water until it was neutral, and then dried at 105℃ for 12h;

[0047] Dissolve 6.5g Mn(NO3)2 and 3.9g CuSO4·5H2O in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ and treat for 30min to fully dissolve the solute; put the treated bamboo charcoal into the above solution, raise the water bath temperature to 80℃, and adjust the rotor speed to 450r / min until all the solvent in the beaker evaporates; then place it in a drying oven for drying at 105℃ for 12h; after drying, a solid catalyst is obtained, and the catalyst block is crushed, ground and screened to obtain particles of 20-40 mesh for later use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature 25℃ at a rate of 10℃ / min. After reaching 400℃, the catalyst is calcined at a constant temperature for 4h to obtain a catalyst loaded with Mn and Cu components;

[0048] Weigh 0.55gNb(NO3)2·6H2O and dissolve it in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ for 30min to fully dissolve the solute; put the catalyst loaded with Mn and Cu components into the above solution, and at the same time increase the water bath temperature to 80℃, and adjust the rotor speed to 450r / min until all the solvent in the beaker evaporates; then place it in a drying oven for drying at 105℃ for 12h; after drying, a solid catalyst is obtained, the catalyst block is crushed, ground and screened to obtain particles of 20-40 mesh for standby use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature 25℃ at a rate of 10℃ / min. After reaching 400℃, they are calcined at a constant temperature for 4h, and after crushing and screening, a low-temperature SCR denitration catalyst loaded with Mn, Cu and Nb is obtained;

[0049] Calculated by metal content, in the catalyst prepared in this comparative example, the mass ratio of the active substance to the bamboo charcoal carrier is 1:10.

[0050] Comparative Example 2

[0051] The preparation method of the denitration catalyst in this comparative example specifically comprises the following steps:

[0052] 30g of coconut shell charcoal was poured into 20% nitric acid for activation, and then placed in a water bath at 80°C for 4h, and then the acid-soaked sample was repeatedly washed with deionized water until neutral, and then dried at 105°C for 12h;

[0053] Dissolve 8.78g Fe(NO3)3 and 3.9g CuSO4·5H2O in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ and treat for 30min to fully dissolve the solute; put the treated coconut shell charcoal into the above solution, raise the water bath temperature to 80℃, and adjust the rotor speed to 450r / min until all the solvent in the beaker evaporates; then place it in a drying oven for drying at 105℃ for 12h; after drying, a solid catalyst is obtained, the catalyst block is crushed, ground and screened out particles of 20-40 mesh for standby use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature 25℃ at a rate of 10℃ / min. After reaching 400℃, the catalyst is calcined at a constant temperature for 4h to obtain a catalyst loaded with Fe and Cu components;

[0054] Weigh 0.55gNb(NO3)2·6H2O and dissolve it in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ for 30min to fully dissolve the solute; put the catalyst loaded with Mn and Cu components into the above solution, and at the same time increase the water bath temperature to 80℃, adjust the rotor speed to 450r / min, until all the solvent in the beaker evaporates; then place it in a drying oven for drying at 105℃ for 12h; after drying, a solid catalyst is obtained, the catalyst block is crushed, ground and screened to obtain particles of 20-40 mesh for standby use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature 25℃ at a rate of 10℃ / min. After reaching 400℃, they are calcined at a constant temperature for 4h, and after crushing and screening, a low-temperature SCR denitration catalyst loaded with Fe, Cu and Nb is obtained;

[0055] Calculated by metal content, in the catalyst prepared in this comparative example, the mass ratio of the active material to the coconut shell carbon carrier is 1:10.

[0056] Comparative Example 3

[0057] The preparation method of the denitration catalyst in this comparative example specifically comprises the following steps:

[0058] 30g of coconut shell charcoal was poured into 20% nitric acid for activation, and then placed in a water bath at 80°C for 4h, and then the acid-soaked sample was repeatedly washed with deionized water until neutral, and then dried at 105°C for 12h;

[0059] Dissolve 0.55g Nb(NO3)2·6H2O in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ for 30min to fully dissolve the solute; put the treated coconut shell charcoal into the above solution, raise the water bath temperature to 80℃, and adjust the rotor speed to 450r / min until all the solvent in the beaker evaporates; then place it in a drying oven for drying at 105℃ for 12h; after drying, a solid catalyst is obtained, the catalyst block is crushed, ground and screened out 20-40 mesh particles for standby use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature 25℃ at a rate of 10℃ / min. After reaching 400℃, it is calcined at a constant temperature for 4h to obtain a catalyst loaded with Nb component;

[0060] Weigh 6.5g Mn(NO3)2 and 3.9g CuSO4·5H2O, and dissolve them in a beaker filled with 50ml deionized water; place the beaker in a constant temperature magnetic stirrer, adjust the water bath temperature to 30℃ for 30min, and fully dissolve the solute; put the catalyst loaded with Nb component into the above solution, and at the same time increase the water bath temperature to 80℃, and adjust the rotor speed to 450r / min, until all the solvent in the beaker evaporates; then place it in a drying oven for drying at 105℃ for 12h; after drying, a solid catalyst is obtained, and the catalyst block is crushed, ground and screened to obtain particles of 20-40 mesh for standby use; the screened particles are calcined in a nitrogen atmosphere, and the temperature is programmed to rise from room temperature 25℃ at a rate of 10℃ / min. After reaching 400℃, they are calcined at a constant temperature for 4h, and after crushing and screening, a low-temperature SCR denitration catalyst loaded with Mn, Cu, and Nb is obtained;

[0061] Calculated by metal content, in the catalyst prepared in this comparative example, the mass ratio of the active material to the coconut shell carbon carrier is 1:10.

[0062] Performance Testing

[0063] use Figure 1 The catalyst activity test device shown in the figure measures the activity of the catalysts prepared in Examples 1-3 and Comparative Examples 1-3, and the test conditions are:

[0064] Airspeed: 7500h -1 ; O2 intake content: 3%; NO intake content: 500ppm; SO2 intake content: 100ppm; H2O intake content: 1%; NH3 / NO=1:1; Temperature: 75℃, 100℃, 125℃, 150℃, 175℃, 200℃, 225℃, 250℃, 275℃;

[0065] The specific test method includes the following steps:

[0066] (1) Loading the catalyst: Weigh the catalyst with a measuring cylinder and load it into a quartz tube;

[0067] (2) Preheating of flue gas analyzer: After the experimental device is powered on, turn on the flue gas analyzer and preheat it for 20 minutes to allow it to reach a stable working state;

[0068] (3) Tube furnace temperature program setting: Turn on the power of the experimental bench thermostat, set the tube furnace temperature rise rate, reaction temperature and dwell time of each reaction temperature, open the N2 gas valve, and when the temperature rises to the set reaction temperature, the thermostat will perform the insulation-heating-insulation stage according to the preset program;

[0069] (4) Reaction gas introduction: Open the NOx valve and introduce gas. The gas flow is controlled and adjusted by the gas distribution system. When the NOx concentration at the reactor outlet is stable, record the NOx inlet concentration c at this time. NO进口 ;

[0070] (5) NOx outlet concentration detection: When reaching each temperature measurement point, the heating program will enter a constant temperature state. When the NOx reading in the flue gas analyzer is stable, the NOx outlet concentration c at this time is recorded. NO出口 ;

[0071] (6) Program heating: follow the preset heating program to the next temperature range and repeat steps (4) and (5);

[0072] (7) When the temperature is adjusted to the test temperature and the catalytic denitrification efficiency is stable for 100 minutes, open the SO2 valve and introduce H2O, and record the NOx outlet concentration c every 10 minutes. NO出口 , continue to flow for 400 minutes to cut off SO2 and H2O, then record the NOx outlet concentration, and continue the test for 100 minutes;

[0073] (8) Calculate the NOx conversion rate.

[0074] Component analysis: The denitrification performance of the catalyst and its alkaline resistance were studied based on a 0.5% K2O loading.

[0075] The NO concentration in the sample was measured using a flue gas analyzer, and the NO conversion rate was calculated as follows:

[0076]

[0077] Where η NO is NO conversion rate; c NO进口 is the inlet concentration of NO; ​​c NO出口 is the NO outlet concentration; for trace reaction, the volume change is negligible. The measurement results are shown in Table 1 below. The line graph obtained by drawing Table 1 is shown in Figure 2 shown.

[0078] Table 1 NOx conversion rate (%) of the denitration catalysts prepared in Examples 1-3 and Comparative Examples 1-3 at different temperatures

[0079]

[0080] As can be seen from Table 1, the NOx conversion rate of the catalyst prepared in Comparative Example 1 is lower than 80%, and the maximum efficiency is 78% at around 200°C, and the temperature range for maintaining above 70% is only 200-250°C. Comparative Example 2 uses Fe as the active substance, and Comparative Example 3 first adds Nb and then adds Mn and Cu. The carbon-based loaded low-temperature section denitration catalyst suitable for biomass combustion flue gas prepared in Examples 1-3 of the present invention has a NOx conversion rate of more than 80% at 150-275°C, and has a higher NOx conversion rate than Comparative Example 1 and Comparative Example 2 in the low-temperature section of 90-240°C, indicating that the carbon-based loaded low-temperature section denitration catalyst suitable for biomass combustion flue gas of the present invention has a better low-temperature catalytic effect, and the high activity temperature window of the catalyst is wider. In the low-temperature section, the present invention has a better denitration effect than bamboo charcoal-based catalysts and loaded Fe / Cu catalysts.

[0081] The NOx conversion rates of the denitration catalysts K poisoned at different temperatures prepared in Examples 1-3 and Comparative Examples 1-3 are shown in Table 2. The line graph obtained by plotting Table 2 is shown in Table 2. Figure 3 shown.

[0082] Table 2 NOx conversion rate (%) of denitration catalyst K poisoned at different temperatures prepared in Examples 1-3 and Comparative Examples 1-3

[0083]

[0084] As can be seen from Table 2, for Example 1, a certain amount of Nb is doped for modification. Under K poisoning conditions, its denitration efficiency is lower than that in Table 1, but it can still maintain a denitration efficiency of more than 80% in the range of 150-275°C, and its denitration efficiency can still reach 90% above 175°C. For Comparative Example 3, Nb is doped first and then Mn and Cu are doped, and its temperature window is greatly reduced. Therefore, for the present invention only, Nb doping can effectively improve the catalyst's alkaline earth metal resistance, and the doping order has a great influence on the reaction.

[0085] The above-described embodiments are merely descriptions of preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various deformations, modifications, evolutions, and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the scope of protection determined by the claims of the present invention.

Claims

1. A carbon-based supported low-temperature denitrification catalyst suitable for biomass combustion flue gas, It is characterized in that The catalyst uses coconut shell charcoal as a carrier and manganese, copper and niobium composite oxide as an active substance, wherein the precursor of manganese oxide is manganese nitrate, the precursor of copper oxide is copper sulfate pentahydrate, the precursor of niobium oxide is niobium nitrate hexahydrate, and the molar ratio of manganese, copper and niobium elements in the precursor is 7:3:0.

05.

2. The carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 1, It is characterized in that The loading amount of active substances manganese and copper is 5% to 10%.

3. The method for preparing a carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 1 or 2, It is characterized in that The following steps are involved: S1, activating the coconut shell charcoal with nitric acid to obtain a nitric acid-modified biocarbon-based carrier; S2, Mn(NO 3 ) 2 ,CuSO 4 ·5H 2 O is fully dissolved in deionized water, and then the biocarbon-based carrier modified by nitric acid is immersed in the above solution, and after ultrasonic treatment at room temperature, it is heated in a water bath and stirred until all the solvent evaporates, and then dried and calcined in anoxic condition to obtain a catalyst loaded with Mn and Cu components; S3. Put Nb(NO 3 ) 2 6H 2 O is fully dissolved in deionized water, and then the catalyst loaded with Mn and Cu components is immersed in the above solution. After ultrasonic treatment at room temperature, it is heated in a water bath and stirred until the solvent is completely evaporated. Then, it is dried, calcined in anoxic conditions, crushed, and screened to obtain a carbon-based loaded low-temperature denitrification catalyst suitable for biomass combustion flue gas.

4. The method for preparing a carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 3, It is characterized in that Step S1 includes the following specific steps: crushing the coconut shell charcoal into particles of 20-40 mesh, washing and drying, pouring into a nitric acid solution with a concentration of 15-20% and stirring evenly, and placing it in a water bath of 70-80° C. for 4-5 hours, and then repeatedly washing the obtained acid-soaked sample with deionized water until it is neutral, and drying it at 100-105° C. for 10-12 hours.

5. The method for preparing a carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 3, It is characterized in that The ultrasonic treatment time in step S2 and step S3 is 30 min.

6. The method for preparing a carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 3, It is characterized in that The water bath in step S2 and step S3 is carried out in a constant temperature magnetic heating stirrer, the water bath temperature is 70-80° C., and the stirring time is 4-5 h.

7. The method for preparing a carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 3, It is characterized in that In step S2 and step S3, the drying temperature is both 100-105° C., and the drying time is both 10-12 hours.

8. The method for preparing a carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 3, It is characterized in that In step S2 and step S3, the anaerobic calcination is carried out under N 2 The calcination is carried out in a tubular furnace with a temperature rising from room temperature at a rate of 10°C / min. The maximum calcination temperature is 400-450°C. The maximum calcination time is maintained for 3-4 hours and the total calcination time is 4-5 hours.

9. The method for preparing a carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas according to claim 3, It is characterized in that The carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas obtained in step S3 has a particle size of 20 to 40 meshes.

10. Use of the carbon-based supported low-temperature denitration catalyst suitable for biomass combustion flue gas as claimed in claim 1 or 2 in the purification of biomass fuel combustion smoke.

Citation Information

Patent Citations

  • Low-sulfur-resistant low-temperature carbon-based denitration catalyst as well as preparation method and application thereof

    CN112403488A

  • Anti-potassium poisoning SCR (Selective Catalytic Reduction) denitration catalyst and preparation method thereof

    CN115814783A

  • Sulfur dioxide-resistant low temperature manganese-iron oxide denitrification catalyst and preparation method thereof

    WO2016078292A1