Homogeneous-heterojunction bismuth-based photocatalyst and preparation method thereof

By combining the molten salt method and the liquid phase method, the homo-heterojunction bismuth photocatalyst is prepared, which solves the problems of limited performance and complicated preparation process of the bismuth photocatalyst in the existing technology, and achieves efficient degradation of wastewater. Refractory pollutants and simplified preparation process are suitable for industrial production.

CN118807791APending Publication Date: 2024-10-22SHAANXI UNIV OF SCI & TECH

Patent Information

Application Number
CN202410828507.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing bismuth-based photocatalysts have limited performance in degrading refractory pollutants in sewage. In particular, single pure phase bismuth silicate powder performs poorly in photocatalytic reactions, and common preparation methods such as high-temperature solid phase method, solvent Thermal methods and sol-gel methods have problems such as long preparation cycles, unsafe equipment, and expensive equipment, making them difficult to industrialize.

Method used

The homo-heterojunction bismuth photocatalyst is prepared by combining the molten salt method and the liquid phase method. Through the joint action of surfactant and halide salt solution, the crystal phase transformation of bismuth silicate and the generation of bismuth oxychloride are promoted. Form a three-dimensional hierarchical structure, increase surface area and active sites, and improve photocatalytic performance.

Benefits of technology

The photocatalytic performance of the bismuth-based photocatalyst is improved, and it can effectively degrade refractory organic matter in sewage, such as rhodamine B, with a degradation rate of 99.9%. It also simplifies the preparation process and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807791A_ABST
    Figure CN118807791A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a homogeneous-heterojunction bismuth-based photocatalyst. The preparation method comprises the following steps: preparing bismuth silicate powder by a molten salt method; the homogeneous-heterojunction bismuth-based photocatalyst is prepared from a surfactant and a halogen salt solution. In the method, the surface of the bismuth silicate is activated by the fused salt, the internal crystal phase is controlled, the forbidden band width is adjusted, and subsequent halogenation is facilitated. The surfactant and the halide salt are added to synergistically promote transformation of a bismuth silicate crystal phase, non-polar long carbon chain CTA < + > and Cl <-> of the halide salt are in mutual electrostatic attraction, generation of a new phase is regulated and controlled, and a homogeneous-heterostructure is formed in a system. Meanwhile, the surfactant affects the growth preferred orientation of bismuth oxychloride and mediates the hierarchical stacking of nanosheet layers, so that the microstructure of the powder forms a structure which is large in surface area and multiple in active site and is beneficial to the photocatalytic reaction. According to the method, the yield of the powder can be improved by using the fused salt, and the defects of powder prepared by a solid phase method can be improved by a subsequent liquid phase method, so that the photocatalyst has more excellent photocatalytic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocatalyst materials, and particularly relates to a homogeneous-heterogeneous junction bismuth-based photocatalyst and a preparation method thereof. Background Art

[0002] As one of the narrow-bandgap photocatalysts that has been studied more, bismuth-based photocatalysts have significant effects in degrading bismuth-based dye compounds, so bismuth-based photocatalysts have received attention in the treatment of difficult-to-degrade pollutants in sewage. As a common bismuth-based photocatalyst, the performance of a single pure phase catalytic powder is limited. Methods to improve performance are often sought by inhibiting the recombination of photogenerated carriers and increasing active sites. Common methods for preparing bismuth silicate include high-temperature solid-phase method, solvothermal method, and sol-gel method. However, each method has its own advantages and disadvantages. The powder prepared by the solid-phase method is a large particle agglomerate, which is not conducive to the photocatalytic reaction. The powder prepared by the solvothermal method and the sol-gel method has the advantages of good dispersibility and high purity, but these methods have the pain points of long preparation cycle, unsafe and expensive production equipment, etc., which cannot be industrialized. Summary of the invention

[0003] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a homogeneous-heterogeneous junction bismuth-based photocatalyst and a preparation method thereof. The preparation process of the method is simple and convenient, and the molten salt method and the liquid phase method are combined to prepare a bismuth-based photocatalyst containing multiple heterojunctions at the same time. The use of the liquid phase method makes up for the agglomeration shortcomings of the solid phase method in preparing the powder. The surfactant added in the combination process promotes the phase and crystal phase transformation, forms a heterojunction, improves the microscopic morphology of the powder, forms a three-dimensional hierarchical structure, increases the surface area and active sites, and improves the photocatalytic performance of the bismuth-based photocatalyst.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is:

[0005] A method for preparing a homogeneous-heterogeneous junction bismuth-based photocatalyst comprises the following steps:

[0006] Step 1, preparing bismuth silicate powder by a molten salt method;

[0007] Step 2, using a surfactant, a halide solution and the bismuth silicate powder to prepare a homogeneous-heterojunction bismuth-based photocatalyst.

[0008] In one embodiment, in step 1, K2CO3-KCl composite molten salt is weighed according to the molar ratio to achieve the lowest eutectic point, and mixed with Bi2O3 and SiO2 for ball milling, wherein the composite molten salt occupies 30%-50% of the total mass, and the ball-milled mixture is calcined at 660°C-720°C for 0.5h-2h, and the obtained block is ground, cleaned, and dried to obtain the bismuth silicate powder.

[0009] In one embodiment, the molar ratio of Bi2O3 to SiO2 is 1:1-9:1.

[0010] In one embodiment, the mixing ball milling time is 4h-6h, the ball milled mixture is heated to 660℃-720℃ at a heating rate of 5℃ / min-10℃ / min, and then calcined for 0.5h-2h.

[0011] In one embodiment, in step 2, bismuth silicate powder is evenly dispersed in deionized water, and the pH is adjusted to maintain at 1-2, then a surfactant is added to react, and then a halide solution is added to react, and after the reaction is complete, the obtained powder is washed and dried to obtain the homo-heterojunction bismuth-based photocatalyst.

[0012] In one embodiment, the concentration of the halide salt solution is 1 g / L-2 g / L, and the ratio of the amount of the bismuth silicate powder, the surfactant and the halide salt solution is (0.1-0.5) g: (0.005-0.060) g: (5-50) mL.

[0013] In one embodiment, after the bismuth silicate powder is evenly dispersed, the pH of the solution is adjusted in a stable environment at 25° C.-35° C., and stirred for 20 min-30 min; a surfactant is added and reacted for 20 min-40 min.

[0014] In one embodiment, the surfactant is a cationic surfactant, an anionic surfactant or a nonionic surfactant.

[0015] In one embodiment, the cationic surfactant is cetyltrimethylammonium bromide (CTAB) or cetyltrimethylammonium chloride (CTAC); the anionic surfactant is sodium dodecylbenzene sulfonate (SDBS); and the nonionic surfactant is polyvinylpyrrolidone (PVP) or dopamine hydrochloride (DA).

[0016] The present invention also claims to protect a homogeneous-heterogeneous junction bismuth-based photocatalyst obtained by the preparation method of the homogeneous-heterogeneous junction bismuth-based photocatalyst.

[0017] The homogeneous-heterogeneous junction bismuth-based photocatalyst can be used to degrade refractory organic matter in sewage, which mainly includes dyes, antibiotics, etc. Experiments have shown that the degradation rate of organic dyes such as rhodamine B reaches 99.9%.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. Surfactants and halide solutions jointly participate in the introduction process of bismuth oxychloride. The addition of surfactants affects the phase transformation of bismuth silicate crystals and promotes the mutual transformation between bismuth oxychloride and surfactants. Non-polar long carbon chains attached to the surface of bismuth silicate, such as CTA in CTAC and CTAB + The group can react with the subsequently added halide Cl due to electrostatic interaction - Mutual attraction promotes the formation of new phases, interferes with the growth orientation of crystals, and forms a good heterogeneous interface in the process. Surfactants also guide the assembly of nanosheets, making the photocatalytic powder have more active sites and improving the photocatalytic performance.

[0020] 2. After molten salt treatment, bismuth silicate is activated and undergoes a crystal phase transformation, which results in the formation of a homogeneous heterojunction in the material system, and then forms a heterojunction with the new phase generated subsequently, thereby constructing a homogeneous-heterojunction photocatalyst. After molten salt activation, the bandgap width of bismuth silicate is significantly reduced, which is helpful for the separation of carriers in the catalyst. Molten salt can control the crystal phase composition inside bismuth silicate to achieve the purpose of forming an effective homogeneous-heterojunction. At the same time, the addition of surfactants can also effectively adjust the bandgap width of the photocatalyst, reduce the widening bandgap changes caused by the introduction of new phases into the system, and make it easier for photogenerated carriers to separate. The built-in electric field formed between the homogeneous and heterojunctions inside bismuth silicate can accelerate the migration of photogenerated carriers, and the heterostructure formed between bismuth silicate and bismuth oxychloride helps to shunt photogenerated carriers and helps photogenerated electrons and holes to undergo redox reactions respectively.

[0021] 3. The surfactant and the halide solution act together on the group exchange reaction to improve the problem of serious agglomeration and few active sites of the original bismuth silicate powder, and transform the original agglomerated powder into a three-dimensional hierarchical structure self-assembled by nanosheets. This method has a simple preparation process and adopts a solid-liquid method. The yield is greatly improved compared with other methods, and the degradation performance of the photocatalyst is greatly improved, which is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a photocatalytic degradation diagram of Rhodamine B degraded by a homogeneous-heterojunction bismuth-based photocatalyst. DETAILED DESCRIPTION

[0023] The embodiments of the present invention are described in detail below with reference to the accompanying drawings and examples.

[0024] A homogeneous-heterogeneous junction bismuth photocatalyst and a preparation method thereof are disclosed. The homogeneous-heterogeneous junction bismuth photocatalyst is prepared by a solid-liquid combination method, wherein a trace amount of surfactant and a halide solution added in a liquid phase method act together on the generation of bismuth oxychloride, while promoting the partial transformation of the crystal phase in bismuth silicate, thereby generating a homogeneous-heterogeneous junction bismuth photocatalyst with more active sites.

[0025] Specifically, the steps may include:

[0026] Step 1), weigh the K2CO3-KCl composite molten salt according to the molar ratio to achieve the lowest eutectic point, and then ball mill it with Bi2O3 and SiO2 in a molar ratio of 1:1-9:1, wherein the mixed molten salt occupies 30%-50% of the total mass, and zirconium oxide is used as the grinding ball, and the ball milling time is 4h-6h. Weigh 4g-6g of the mixture for calcination, and heat it to 660℃-720℃ at a heating rate of 5℃ / min-10℃ / min for 0.5h-2h. Grind, clean and dry the calcined block.

[0027] Step 2), weigh 0.1g-0.5g bismuth silicate powder and add it into 20mL-50mL deionized water to make it dispersed evenly. Add dilute acid to adjust the solution pH to 1-2 in a stable environment of 25℃-35℃, stir for 20min-30min, then add 5mg-60mg surfactant to react for 20min-40min, then add 5mL-50mL 1g / L-2g / L NaCl solution, and wash and dry the powder after the reaction is complete.

[0028] Among them, the surfactants are: cationic surfactants (cetyltrimethylammonium bromide (CTAB), cetyltrimethylammonium chloride (CTAC), etc.), anionic surfactants (sodium dodecylbenzene sulfonate (SDBS), etc.), and non-ionic surfactants (polyvinylpyrrolidone (PVP), dopamine hydrochloride (DA), etc.).

[0029] The present invention is based on bismuth silicate, and a trace amount of surfactant is added to work together with halide salt to prepare bismuth-based photocatalytic powder containing homogeneous-heterogeneous junctions. Molten salt activates the surface of bismuth silicate and controls the internal crystal phase, adjusts the band gap, and facilitates subsequent halogenation. The addition of surfactant and halide salt synergistically promotes the transformation of bismuth silicate crystal phase, wherein non-polar long carbon chain CTA + Cl with halogen salts - Mutual electrostatic attraction regulates the generation of new phases and forms a homogeneous-heterogeneous structure in the system. At the same time, the surfactant affects the growth orientation of bismuth oxychloride, mediates the hierarchical stacking of nanosheets, and makes the microstructure of the powder form a structure with a large surface area and multiple active sites that is beneficial to the photocatalytic reaction. This method can improve the yield of the powder by using molten salt, and the subsequent liquid phase method can improve the shortcomings of the solid phase method for preparing powders, so that the photocatalyst has better photocatalytic performance.

[0030] Several embodiments of the present invention are as follows.

[0031] Example 1

[0032] Step 1), preparation of bismuth silicate powder: weigh the K2CO3-KCl composite molten salt according to the molar ratio to achieve the lowest eutectic point, and then ball mill it with Bi2O3 and SiO2 in a molar ratio of 3:1, wherein the mixed molten salt occupies 30% of the total mass, and zirconium oxide is used as the grinding ball, and the ball milling time is 4h. Weigh 4.5g of the mixture for calcination, and heat it to 660℃ at a heating rate of 10℃ / min for 0.5h. Grind, clean and dry the calcined block.

[0033] Step 2), preparation of homogeneous-heterogeneous junction bismuth-based photocatalyst: weigh 0.3g of bismuth silicate powder and add it into 20mL of deionized water to make it dispersed evenly. Add dilute acid to adjust the solution pH to 1 in a stable environment at 25°C, stir for 20min, then add 20mg of CTAB to react for 40min, then add 5mL of 1.5g / L NaCl solution, and wash and dry the powder after the reaction is complete.

[0034] refer to Figure 1 The homogeneous-heterogeneous bismuth-based photocatalytic powder obtained can degrade 15 mg / L of rhodamine B by 99.9% within 30 minutes. The performance of the modified powder has been greatly improved, thanks to the addition of CTA in CTAB. + Bismuth oxychloride is introduced in combination with halide salts. The formation of various heterojunctions greatly improves the migration and separation of photogenerated carriers. The active groups of CTAB present in the reaction medium further mediate the assembly process of the newly generated nanosheets, forming a three-dimensional hierarchical microstructure with a large surface area and active sites, which is easy to increase the reaction sites for redox during the photocatalytic reaction.

[0035] The concentration of Rhodamine B in this example is 15 mg / L. Photocatalytic degradation test process time 30 mL of Rhodamine B solution and 30 mg of powder were first placed in dark conditions and stirred for 60 minutes to achieve adsorption and desorption equilibrium. Then a 500W xenon lamp was used as the light source for 30 minutes. Samples were taken at regular intervals, 3 ml each time, the suspension was centrifuged to obtain the upper clear liquid, and the pollutant concentration during the reaction was tested using a UV-visible spectrophotometer. The dark reaction was sampled every 30 minutes, and the light reaction was sampled every 5 minutes.

[0036] Example 2

[0037] Step 1), preparation of bismuth silicate powder: weigh the K2CO3-KCl composite molten salt according to the molar ratio to achieve the lowest eutectic point, and then ball mill it with Bi2O3 and SiO2 in a molar ratio of 6:1, wherein the mixed molten salt occupies 30% of the total mass, and zirconium oxide is used as the grinding ball, and the ball milling time is 5h. Weigh 3g of the mixture for calcination, and heat it to 720℃ at a heating rate of 10℃ / min for 0.5h. Grind, clean and dry the calcined block.

[0038] Step 2), preparation of homogeneous-heterogeneous junction bismuth-based photocatalyst: weigh 0.25g bismuth silicate powder and add it into 30mL deionized water to make it dispersed evenly. Add dilute acid to adjust the solution pH to 1 in a stable environment at 25°C, stir for 30min, then add 40mg PVP to react for 20min, then add 10mL 1g / L NaCl solution, and wash and dry the powder after the reaction is complete.

[0039] In more embodiments of the present invention, the aforementioned parameters are combined in different types. For example, in step 1), the ratio of Bi2O3 and SiO2 is selected as 3:1, 6:1, 9:1, and the calcination temperature and holding time are selected as a combination of 660°C / 1h and 690°C / 0.5h, etc. The results all prove that bismuth silicate powder can be prepared.

[0040] Similarly, in step 2), the actual amount of bismuth silicate powder was also selected as 0.2g, 0.3g, and 0.4g, the water bath temperature was selected as 25°C, 30°C, and 35°C, the surfactant was selected as CTAB, CTAC, PVP, SDBS, etc., the amount of the surfactant was 10mg, 20mg, 30mg, 40mg, etc., the reaction time was 20min, 30min, 40min, etc., the concentration of NaCl used was 1g / L, 1.2g / L, 1.6g / L, etc., the amount added was 5mL, 10mL, 15mL, etc., and the results all proved that homogeneous-heterojunction bismuth-based photocatalysts can be prepared.

[0041] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, substitutions, combinations, simplifications, etc. made based on the principles or spirit of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a homogeneous-heterojunction bismuth-based photocatalyst, It is characterized in that The steps include: Step 1, preparing bismuth silicate powder by a molten salt method; Step 2, using a surfactant, a halide solution and the bismuth silicate powder to prepare a homogeneous-heterojunction bismuth-based photocatalyst.

2. The method for preparing the homo-heterojunction bismuth-based photocatalyst according to claim 1, It is characterized in that In step 1, K is weighed according to the molar ratio to achieve the lowest eutectic point. 2 CO 3 -KCl composite molten salt, with Bi 2 O 3 and SiO 2 The mixed material is ball-milled, wherein the composite molten salt accounts for 30%-50% of the total mass, the ball-milled mixture is calcined at 660° C.-720° C. for 0.5 h-2 h, and the obtained block is ground, cleaned and dried to obtain the bismuth silicate powder.

3. The method for preparing the homo-heterojunction bismuth-based photocatalyst according to claim 2, It is characterized in that The Bi 2 O 3 and SiO 2 The molar ratio is 1:1-9:

1.

4. The method for preparing the homo-heterojunction bismuth-based photocatalyst according to claim 2, It is characterized in that The mixing ball milling time is 4h-6h, and the mixed material after ball milling is heated to 660°C-720°C at a heating rate of 5°C / min-10°C / min, and then calcined at this temperature for 0.5h-2h.

5. The method for preparing the homo-heterojunction bismuth-based photocatalyst according to claim 1, It is characterized in that In the step 2, bismuth silicate powder is dispersed evenly in deionized water, and the pH is adjusted to maintain at 1-2, then a surfactant is added to react, and then a halide solution is added to react, and after the reaction is complete, the obtained powder is washed and dried to obtain the homogeneous-heterojunction bismuth-based photocatalyst.

6. The method for preparing the homo-heterojunction bismuth-based photocatalyst according to claim 5, It is characterized in that The concentration of the halide salt solution is 1g / L-2g / L, and the ratio of the amount of the bismuth silicate powder, the surfactant and the halide salt solution is (0.1-0.5)g: (0.005-0.060)g: (5-50)mL.

7. The method for preparing the homo-heterojunction bismuth-based photocatalyst according to claim 5 or 6, It is characterized in that After the bismuth silicate powder is evenly dispersed, the pH of the solution is adjusted in a stable environment at 25° C.-35° C., and the solution is stirred for 20 min-30 min. After adding a surfactant, the solution is reacted for 20 min-40 min.

8. The method for preparing the homo-heterojunction bismuth-based photocatalyst according to claim 5 or 6, It is characterized in that The surfactant is a cationic surfactant, an anionic surfactant or a nonionic surfactant.

9. The method for preparing the homo-heterojunction bismuth-based photocatalyst according to claim 8, It is characterized in that The cationic surfactant is hexadecyltrimethylammonium bromide (CTAB) or hexadecyltrimethylammonium chloride (CTAC); the anionic surfactant is sodium dodecylbenzenesulfonate (SDBS); and the nonionic surfactant is polyvinylpyrrolidone (PVP) or dopamine hydrochloride (DA).

10. Use of the homo-heterojunction bismuth-based photocatalyst obtained by the preparation method of the homo-heterojunction bismuth-based photocatalyst according to any one of claims 1 to 9 for degrading refractory organic matter in sewage, wherein the refractory organic matter includes dyes and antibiotics.

Citation Information

Patent Citations

  • Nanosheet layer stacked controllable flower-like BSOCB photocatalyst and preparation method thereof

    CN117085744A

  • Three-dimensional peony-shaped composite photocatalyst and preparation method thereof

    CN117085745A

  • Bismuth colloidal solution and its manufacturing method

    JP2004099991A

Cited By

  • Composite photocatalytic material with (Bi2+ / Bi3 +)-VO-VN synergistic regulation effect and preparation method thereof

    CN120286048A