High manganese steel bimetallic lining plate and preparation method thereof

By embedding high carbon chromium bearing steel rods in high manganese steel lining plates and performing specific heat treatment, a bimetallic lining plate with high hardness and high wear resistance is formed, which solves the problem of insufficient wear resistance of traditional lining plates and significantly improves the wear resistance of traditional lining plates. longevity and performance.

CN118807913AInactive Publication Date: 2024-10-22SHANDONG TIANLI MASCH FOUNDRY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410807256.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional high manganese steel lining plates have insufficient wear resistance under actual working conditions, short service life, and are prone to deformation and wear during long-term use.

Method used

It adopts a bimetallic liner structure of high manganese steel substrate and vertically embedded high-carbon chromium bearing steel rods. The overall structure is formed through metallurgical bonding, and water glass quartz sand molding, quenching and tempering are performed to ensure the high hardness and high hardness of the liner. Wear resistance.

Benefits of technology

The tensile strength, yield strength, impact energy absorption and hardness of the liner are improved, the wear resistance, corrosion resistance, impact resistance and fatigue resistance are enhanced, and the service life is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807913A_ABST
    Figure CN118807913A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wear-resistant materials, and discloses a high-manganese steel bimetal lining plate which comprises a high-manganese steel base body and a plurality of high-carbon-chromium bearing steel bars vertically embedded in the high-manganese steel base body. According to the method, the surface of the high-carbon-chromium bearing steel bar is melted and the inner layer is not melted through high-manganese steel water poured at a high temperature, so that a metallurgical bonding transition area is formed, and no gap exists; meanwhile, the high-carbon-chromium bearing steel bar plays a role of chilling iron in the high-manganese molten steel under the action of high-temperature pouring, so that grains of the high-manganese molten steel are refined and do not grow up in the solidification process; the high-carbon chromium bearing steel bar cannot be completely melted, the double metals cannot be mixed, and the high-manganese steel base body and the high-carbon chromium bearing steel bar form the whole high-manganese steel double-metal lining plate through the metallurgical bonding transition area; the high-manganese steel bimetallic lining plate has excellent tensile strength, yield strength and impact absorption energy and relatively high hardness, so that the wear resistance, corrosion resistance, impact resistance and fatigue resistance of the high-manganese steel bimetallic lining plate are improved, and the service life of the high-manganese steel bimetallic lining plate is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wear-resistant materials, in particular to a high manganese steel bimetal lining plate and a preparation method thereof. Background Art

[0002] Ball mill is the main equipment in the production process of ferrous metal mines, non-ferrous metal mines, cement building materials, water conservancy and electricity, etc. The cylinder of the ball mill is equipped with a liner to protect the cylinder when crushing materials. When the ball mill is rotating, the ball mill medium crushes the materials and the liner is also worn and consumed. Therefore, it needs to be replaced after a certain period of time and is the main easily worn part. This requires the liner to be unbreakable, impact-resistant, wear-resistant, corrosion-resistant, and fatigue-resistant.

[0003] The traditional lining material is high manganese steel, also known as austenitic manganese steel; its main feature is excellent toughness; but under actual working conditions, it has the disadvantages of insufficient wear resistance and short service life; therefore, with the progress of social science and technology and the development of new quality productivity, new material linings are constantly emerging.

[0004] For example, a Chinese patent discloses a composite ball mill liner and a preparation method thereof (authorization announcement number CN101884948B). This patented technology compounds a layer of ceramic particles on the wear surface of the ball mill liner to form a wear-resistant hard phase, and the gaps between the ceramic particles are filled with matrix metal. Therefore, the composite surface has both the wear resistance of the ceramic particles and the plasticity, toughness and fatigue resistance of the matrix metal. The hard phase is not easy to fall off, the process parameters are highly controllable, there are no defects such as slag inclusions in the organization, the processing operation is convenient, and it is convenient for industrial mass production. In addition, the service life of the liner is 5 to 8 times longer than that of an ordinary metal liner. However, its hardness is poor, and it is prone to deformation and wear during long-term use. Summary of the invention

[0005] The object of the present invention is to provide a high manganese steel bimetallic liner and a preparation method thereof to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A high manganese steel bimetallic liner, comprising a high manganese steel substrate, and a plurality of high carbon chromium bearing steel rods vertically embedded in the high manganese steel substrate, wherein one end of the high carbon chromium bearing steel rod is flush with the front surface of the high manganese steel substrate, and the other end of the high carbon chromium bearing steel rod is located at 1 / 3 of the back surface of the high manganese steel substrate, that is, one end of the high carbon chromium bearing steel rod is flush with the working surface of the liner, and the length of the high carbon chromium bearing steel rod embedded in the high manganese steel substrate is 2 / 3 of the thickness of the high manganese steel substrate; a semicircular groove and a trapezoidal groove for reducing the thickness are provided on the back surface of the high manganese steel substrate, and the length of the high carbon chromium bearing steel rod is shortened according to the groove surface curve;

[0008] For example, the diameter of the high carbon chromium bearing steel rod is 8.3 mm, and the distance between the high carbon chromium bearing steel rod and the high manganese steel substrate is 20 to 30 mm; the outer diameter distance between two adjacent high carbon chromium bearing steel rods is 15 to 16 mm, and they are evenly distributed and staggered along the working surface of the liner; the high manganese steel substrate and the high carbon chromium bearing steel rods are metallurgically combined to form an integral structure.

[0009] As a further solution of the present invention: the chemical composition of the high manganese steel matrix is ​​as follows: w(c)=0.9~1.35%, w[Si)=0.3~0.9%, w(Mn)=11~14%, w(p)≤0.06%, w(s)≤0.04%, w(Cr)=0~2.5%; for example, the three grades of ZG100Mn13, ZG120Mn13, and ZG120Mn13Cr2 in the national standard GB / T5680 are selected; these three grades of high manganese steel are also commonly used grades for ball mill liners.

[0010] As a further solution of the present invention: the chemical composition of the high carbon chromium bearing steel bar is as follows: w(c)=0.95-1.10%, w(Si)=0.15-0.35%, w(Mn)=0.25-0.45%, w(Cr)=1.40-1.65%, w(Ni)≤0.3%, w(Cu)≤0.25%, w(Mo)=0.1%, w(Ni+Cu)≤0.5%, w(p)≤0.025%, w(s)≤0.025%; for example, the GCr15 grade in the national standard GB / T18254 is selected.

[0011] A preparation method of a high manganese steel bimetallic liner, wherein the molding process of the preparation method adopts water glass quartz sand molding, and the specific steps are as follows:

[0012] S1. Weld an iron nail, such as a 1.5-inch iron nail, at the center of one end of the high-carbon chromium bearing steel rod, and then insert the high-carbon chromium bearing steel rod into the cavity wall of the casting box in sequence according to the design layout and fix it to make a casting system. After closing the casting box, pour high-manganese molten steel into the casting box. After the high-manganese molten steel is cooled and solidified, a high-manganese steel matrix is ​​formed, so that the high-manganese steel matrix and the high-carbon chromium bearing steel rod are combined together to form a high-manganese steel bimetallic liner;

[0013] S2. Take out the high manganese steel bimetallic lining from the casting box, put it into the heat treatment furnace, and perform quenching and tempering treatment in sequence.

[0014] As a further solution of the present invention: in the S1 step, the pouring temperature of the high manganese molten steel is 1510-1570°C. Since the melting point of GCr15 is 1395-1460°C, during the pouring process, the surface of the high carbon chromium bearing steel rod melts while the inner layer does not melt, forming a metallurgical bonding transition zone with no gaps; at the same time, the high carbon chromium bearing steel rod acts as a chiller in the high manganese molten steel under the action of high temperature pouring, so that the grains of the high manganese molten steel are refined and will not grow during the solidification process; the high carbon chromium bearing steel rod will not be completely melted, the bimetal will not be mixed, and the high manganese steel matrix and the high carbon chromium bearing steel rod will form a whole liner through the metallurgical bonding transition zone.

[0015] As a further solution of the present invention: in the step S2, the quenching temperature of the high manganese steel bimetallic lining is 1050-1100°C, the quenching method is water quenching, during the quenching process, the furnace entry temperature of the high manganese steel bimetallic lining is ≤200°C, the heating rate is ≤100°C / h, it is kept at a constant temperature of 650°C for 1h, then heated to 1050-1100°C, kept warm for 5h, and then quenched into water; the running time of the high manganese steel bimetallic lining from opening the furnace door to being hoisted into the water is less than 50s, and the water temperature in the quenching tank is less than 50°C; after the high manganese steel bimetallic lining enters the water, it is shaken and cooled to the water temperature before exiting the water; by heating at a temperature of 1050-1100°C The steel rods are quenched at 160℃ to completely transform the microstructure of the high manganese steel matrix into austenite, and meet the tempering requirements of the high carbon chromium bearing steel rods. The tempering temperature is 160℃ and the temperature is kept for 10 hours. The microstructure and mechanical properties of the high manganese steel matrix do not change by tempering at 160℃. Only when tempered at above 230℃, the carbides in the microstructure of the high manganese steel matrix will precipitate, resulting in changes in the microstructure and mechanical properties. The high carbon chromium bearing steel rods wrapped in the high manganese steel matrix have their internal stress removed and the martensite microstructure stabilized after tempering at 160℃. The hardness is HRC≥62, and high hardness and high wear resistance are obtained.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] The present invention uses high-temperature poured high manganese steel water to melt the surface of the high carbon chromium bearing steel rod while the inner layer does not melt, thereby forming a metallurgical bonding transition zone with no gaps; at the same time, the high carbon chromium bearing steel rod acts as a chiller in the high manganese steel water under the action of high temperature pouring, so that the grains of the high manganese steel water are refined and do not grow during the solidification process; the high carbon chromium bearing steel rod will not be completely melted, and the bimetal will not be mixed, and the high manganese steel matrix and the high carbon chromium bearing steel rod will form a whole high manganese steel bimetal lining plate through the metallurgical bonding transition zone; the high manganese steel bimetal lining plate has excellent tensile strength, yield strength, impact absorption energy and high hardness, thereby improving its wear resistance, corrosion resistance, impact resistance and fatigue resistance, and increasing its service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic diagram of the main view of a high manganese steel bimetallic liner;

[0019] Figure 2 It is a side view schematic diagram of a high manganese steel bimetallic liner.

[0020] In the figure: 1. High manganese steel substrate; 2. High carbon chromium bearing steel rod. DETAILED DESCRIPTION

[0021] Example 1

[0022] See also Figures 1-2 In an embodiment of the present invention, a high manganese steel bimetallic liner includes a high manganese steel substrate 1, and a plurality of high carbon chromium bearing steel rods 2 vertically embedded in the high manganese steel substrate 1, one end of the high carbon chromium bearing steel rod 2 is flush with the front surface of the high manganese steel substrate 1, and the other end of the high carbon chromium bearing steel rod 2 is located at 1 / 3 of the back surface of the high manganese steel substrate 1, and the high manganese steel substrate 1 and the high carbon chromium bearing steel rod 2 are metallurgically bonded to form an integral structure.

[0023] The diameter of the high carbon chromium bearing steel rod 2 is selected to be 8.3 mm, and the distance between the high carbon chromium bearing steel rod 2 and the high manganese steel substrate 1 is set to 20 mm; the outer diameter distance between two adjacent high carbon chromium bearing steel rods 2 is set to 15 mm, and they are evenly distributed and staggered along the working surface of the liner;

[0024] The high manganese steel substrate 1 is made of ZG120Mn13 grade in the national standard GB / T5680, and its chemical composition is as follows after chemical analysis: w(c)=1.17%, w[Si)=0.6%, w(Mn)=12.1%, w(p)=0.04%, w(s)=0.02%;

[0025] The high carbon chromium bearing steel bar 2 uses the GCr15 grade in the national standard GB / T18254. The chemical composition obtained by chemical analysis is as follows: w(c)=1.03%, w(Si)=0.27%, w(Mn)=0.34%, w(Cr)=1.51%, w(Ni)=0.1%, w(Cu)=0.13%, w(Mo)=0.1%, w(p)≤0.018%, w(s)≤0.011%.

[0026] A preparation method of a high manganese steel bimetallic liner, wherein the molding process of the preparation method adopts water glass quartz sand molding, and the specific steps are as follows:

[0027] S1. Weld a 1.5-inch iron nail at the center of one end of the high-carbon chromium bearing steel rod 2, and then insert the high-carbon chromium bearing steel rod 2 into the cavity wall of the casting box in sequence according to the design layout and fix it, so as to make a casting system. After closing the casting box, pour high manganese molten steel into the casting box at a casting temperature of 1510° C. The high manganese molten steel is cooled and solidified to form a high manganese steel matrix 1, so that the high manganese steel matrix 1 and the high carbon chromium bearing steel rod 2 are combined together to form a high manganese steel bimetallic liner;

[0028] S2. Take the high manganese steel bimetallic lining plate out of the casting box and put it into the heat treatment furnace for quenching and tempering. First, quenching is performed at a temperature of 1050°C by water quenching, and then tempering is performed at a temperature of 160°C.

[0029] Example 2

[0030] See also Figures 1-2 In an embodiment of the present invention, a high manganese steel bimetallic liner includes a high manganese steel substrate 1, and a plurality of high carbon chromium bearing steel rods 2 vertically embedded in the high manganese steel substrate 1, one end of the high carbon chromium bearing steel rod 2 is flush with the front surface of the high manganese steel substrate 1, and the other end of the high carbon chromium bearing steel rod 2 is located at 1 / 3 of the back surface of the high manganese steel substrate 1, and the high manganese steel substrate 1 and the high carbon chromium bearing steel rod 2 are metallurgically bonded to form an integral structure.

[0031] The diameter of the high carbon chromium bearing steel rod 2 is selected to be 8.3 mm, and the distance between the high carbon chromium bearing steel rod 2 and the high manganese steel substrate 1 is set to 30 mm; the outer diameter distance between two adjacent high carbon chromium bearing steel rods 2 is set to 16 mm, and they are evenly distributed and staggered along the working surface of the liner;

[0032] The high manganese steel substrate 1 uses the ZG120Mn13Cr2 grade in the national standard GB / T5680, and its chemical composition is as follows after chemical analysis: w(c)=1.07%, w[Si)=0.6%, w(Mn)=11.8%, w(p)=0.03%, w(s)=0.02%, w(Cr)=1.9%;

[0033] The high carbon chromium bearing steel bar 2 is of the GCr15 grade in Example 1, and its chemical composition is the same as that in Example 1.

[0034] A preparation method of a high manganese steel bimetallic liner, wherein the molding process of the preparation method adopts water glass quartz sand molding, and the specific steps are as follows:

[0035] S1. Weld a 1.5-inch iron nail at the center of one end of the high-carbon chromium bearing steel rod 2, and then insert the high-carbon chromium bearing steel rod 2 into the cavity wall of the casting box in sequence according to the design layout and fix it, so as to make a casting system. After closing the casting box, pour high manganese molten steel into the casting box at a casting temperature of 1570° C. The high manganese molten steel is cooled and solidified to form a high manganese steel matrix 1, so that the high manganese steel matrix 1 and the high carbon chromium bearing steel rod 2 are combined together to form a high manganese steel bimetallic liner;

[0036] S2. Take the high manganese steel bimetallic lining plate out of the casting box and put it into the heat treatment furnace for quenching and tempering. First, quenching is performed at a temperature of 1100°C by water quenching, and then tempering is performed at a temperature of 160°C.

[0037] In order to better illustrate the technical effect of the present invention, the following experiments are used to illustrate:

[0038] The microstructure and mechanical properties of the high manganese steel bimetallic liner prepared in Example 1 and Example 2 were analyzed respectively;

[0039] 1. Through microstructure analysis, it is found that the microstructure of the high manganese steel matrix in the high manganese steel bimetallic liner prepared in Example 1 and Example 2 is all austenite; the microstructure of the high carbon chromium bearing steel rod is all martensite;

[0040] 2. The mechanical properties of the high manganese steel matrix in the high manganese steel bimetallic liner include tensile strength (σ b , MPa), yield strength (σ s , MPa), impact absorption energy (A KU , J, i.e. the impact absorbed energy of the U-notch specimen under the 2mm pendulum blade), residual stress (σ 5% , N, i.e. the stress corresponding to the specified non-proportional elongation of 0.05% obtained in the tensile test) and Brinell hardness (HB); the mechanical property index Rockwell hardness (HRC) of the high carbon chromium bearing steel bar in the high manganese steel bimetallic liner;

[0041] 1. The mechanical properties of the high manganese steel bimetallic liner prepared in Example 1 are shown in Table 1 below;

[0042] Table 1

[0043]

[0044] It can be concluded from Table 1 above that the high manganese steel bimetallic liner prepared by the present invention has excellent tensile strength, yield strength, impact absorption energy and high hardness.

[0045] 2. The mechanical properties of the high manganese steel bimetallic liner prepared in Example 2 are shown in Table 2 below;

[0046] Table 2

[0047]

[0048] It can be concluded from Table 2 above that the high manganese steel bimetallic liner prepared by the present invention has excellent tensile strength, yield strength, impact absorption energy and high hardness.

[0049] What is described above is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high manganese steel bimetallic liner, comprising a high manganese steel substrate (1), and a plurality of high carbon chromium bearing steel bars (2) vertically embedded in the high manganese steel substrate (1), It is characterized in that One end of the high carbon chromium bearing steel rod (2) is flush with the front side of the high manganese steel substrate (1), and the other end of the high carbon chromium bearing steel rod (2) is located at 1 / 3 of the back side of the high manganese steel substrate (1); the high manganese steel substrate (1) and the high carbon chromium bearing steel rod (2) are metallurgically bonded to form an integral structure.

2. A high manganese steel bimetallic liner according to claim 1, It is characterized in that The chemical composition of the high manganese steel substrate (1) is as follows: w(c)=0.9-1.35%, w[Si)=0.3-0.9%, w(Mn)=11-14%, w(p)≤0.06%, w(s)≤0.04%, w(Cr)=0-2.5%.

3. A high manganese steel bimetallic liner according to claim 1, It is characterized in that The chemical composition of the high carbon chromium bearing steel bar (2) is as follows: w(c)=0.95-1.10%, w(Si)=0.15-0.35%, w(Mn)=0.25-0.45%, w(Cr)=1.40-1.65%, w(Ni)≤0.3%, w(Cu)≤0.25%, w(Mo)=0.1%, w(Ni+Cu)≤0.5%, w(p)≤0.25%, w(s)≤0.025%.

4. A method for preparing the high manganese steel bimetallic liner according to claim 1, It is characterized in that The molding process of the preparation method adopts water glass quartz sand molding, and the specific steps are as follows: S1. Weld an iron nail at the center of one end of the high-carbon chromium bearing steel rod (2), and then insert the high-carbon chromium bearing steel rod (2) into the cavity wall of the casting box in sequence according to the design layout and fix it, so as to make a casting system. After closing the casting box, pour high-manganese molten steel into the casting box, and the high-manganese molten steel is cooled and solidified to form a high-manganese steel matrix (1), so that the high-manganese steel matrix (1) and the high-carbon chromium bearing steel rod (2) are combined together to form a high-manganese steel bimetallic liner; S2. Take out the high manganese steel bimetallic lining from the casting box, put it into the heat treatment furnace, and perform quenching and tempering treatment in sequence.

5. A method for preparing a high manganese steel bimetallic liner according to claim 4, It is characterized in that In the step S1, the pouring temperature of the high manganese molten steel is 1510-1570°C.

6. The method for preparing a high manganese steel bimetallic liner according to claim 4, It is characterized in that In the step S2, the quenching temperature of the high manganese steel bimetallic liner is 1050-1100°C, the quenching method is water quenching; the tempering temperature is 160°C.

Citation Information

Patent Citations

  • Preparation technique for alloy powder core tube thread in situ generating abrasion-proof composite material

    CN101239396A

  • Method for preparing composite abrasion-proof lining board

    CN101406950A

  • Grinding roller of vertical mill and preparation method of grinding roller

    CN115780025A

  • Wear-resisting compound liner board for ball mill

    CN2109910U

  • Improved ball mill lining plate structure

    CN212018018U