Mineral recovery method of high-phosphorus vanadium titano-magnetite tailings
Through strong magnetic separation, cyclone classification, interference bed separation, fine screen classification and spiral chute gravity separation, combined with flotation desulfurization and dephosphorization steps, the problem of fine particles in high-phosphorus vanadium titanium magnetite tailings has been solved. The problem of ilmenite recycling has improved the recovery rate and quality of titanium ore and achieved efficient use of resources.
Patent Information
- Application Number
- CN202411208911.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The existing vanadium-titanium magnetite beneficiation process cannot effectively recover the fine ilmenite in high-phosphorus vanadium-titanium magnetite tailings, resulting in waste of resources and reduction of titanium ore quality, and increasing the difficulty of recycling titanium flotation.
After a stage of strong magnetic roughing, the coarse concentrate is divided into underflow ore and overflow ore through cyclone classification and interference bed separation. After fine screening and classification, a second stage of strong magnetic separation is performed to obtain fine-grained concentrate as Flotation raw materials, combined with spiral chute gravity separation and flotation desulfurization and dephosphorization processes, can improve the recovery rate and quality of titanium ore.
It improves the recovery rate and quality of titanium ore in high-phosphorus vanadium titanium magnetite tailings, enhances resource utilization, reduces the impact of sulfur and phosphorus impurities in the flotation process, and improves the grade and recovery rate of titanium concentrate.
Smart Images

Figure CN118807964A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of vanadium-titanium magnetite beneficiation, in particular to a mineral recovery method for high-phosphorus vanadium-titanium magnetite tailings. Background Art
[0002] The total reserves of vanadium-titanium magnetite resources in my country are over 20.1 billion tons, and are mainly distributed in Panxi area of Sichuan, Chengde area of Hebei, Chaoyang area of Liaoning and Hami area of Xinjiang. Among them, the reserves of vanadium-titanium magnetite resources, TiO2 and V2O5 in Panxi area of Sichuan account for 75.95%, 95.61% and 97.14% of the national reserves respectively, which is an important large-scale energy resource base in my country.
[0003] At present, the conventional beneficiation technology of vanadium-titanium magnetite in Panzhihua area is the "step grinding and step selection - magnetic separation for iron - flotation separation for titanium" process flow, which can realize the efficient development and utilization of vanadium-titanium magnetite. Although the step grinding and step selection can reduce the grinding time as much as possible, over-grinding is still inevitable, resulting in a large amount of fine ilmenite mixed in the high-phosphorus vanadium-titanium magnetite tailings. With this kind of beneficiation technology, the fine ilmenite minerals in the tailings cannot be recycled, which causes a certain degree of waste of resources.
[0004] In addition, a large amount of extremely fine calcite or titanite is filled in the interstitial spaces between the particles of anatase aggregate. The density of fine-grained gangue such as calcite or titanite is relatively high, and the particle size is usually less than five microns. It is difficult to separate them by fine grinding using the current mineral processing technology. Calcite or titanite is easy to enter the titanium ore along with the titanium ore, which is not conducive to the flotation recovery of ilmenite, resulting in reduced quality of the titanium ore after flotation.
[0005] In addition, the phosphorus content of vanadium-titanium magnetite in the current mining area shows a trend of increasing. Using the current mineral recovery process, sulfur phosphate ore and the like are not fully recovered and exist in the titanium tailings, which makes the recovery of flotation titanium ore more difficult and aggravates the loss of titanium ore resources. Therefore, it is necessary to explore a suitable mineral recovery method for high-phosphorus vanadium-titanium magnetite tailings to improve the recovery rate of titanium ore in the tailings. Summary of the invention
[0006] The purpose of the present invention is to provide a method for recovering minerals from high-phosphorus vanadium titanium magnetite tailings, which includes the following steps:
[0007] S1: After a period of strong magnetic roughing, the tailings of high phosphorus vanadium titanium magnetite are subjected to strong magnetic rough concentrate and the first strong magnetic tailings; the strong magnetic rough concentrate is subjected to cyclone classification and interference bed separation in turn to obtain underflow ore and overflow ore;
[0008] S2: The overflow ore is subjected to fine screening and classification to obtain oversize ore and undersize ore;
[0009] S3: After the undersize ore is concentrated, it is subjected to two-stage strong magnetic concentration to obtain fine-grained concentrate and a second strong magnetic tailings; the fine-grained concentrate is concentrated to form flotation raw material; the TiO2 grade of the second strong magnetic tailings is lower than 3.31%; the TiO2 grade of the flotation raw material is greater than 15%.
[0010] Compared with the ore-dressing process of the traditional process of only performing one-stage strong magnetic and two-stage strong magnetic combined with fine screening classification, the mineral recovery method of the high-phosphorus vanadium titanium magnetite tailings of the present invention is that after the first stage of strong magnetic roughing, the coarse concentrate is subjected to cyclone classification and interference bed separation respectively, so that the coarse concentrate can be divided into underflow ore with larger particle size and overflow ore with smaller particle size; the overflow ore with smaller particle size is further subjected to fine screening classification to obtain under-screen ore with smaller particle size and uniform particle size, and the under-screen ore with smaller particle size and uniform particle size is further subjected to two-stage strong magnetic separation to obtain micro-fine particle concentrate; and the fine concentrate is then separated into the fine concentrate by step S3. After concentration, it is used as a flotation raw material for flotation of titanium ore, and the fine-grained titanium ore in the high-phosphorus vanadium titanium magnetite tailings can be recovered, so that the slurry concentration of the flotation raw material is 45%, the TiO2 grade is 18.53%, and the grade of titanium dioxide in the fine-grained concentrate is greater than 15%, thereby improving the resource recovery rate; and, after cyclone classification and interference bed separation, the coarse-grained gangue that has not been finely ground and dissociated is separated into the bottom flow, and will not follow the fine-grained concentrate into the flotation titanium, and will not affect the quality of the titanium ore after flotation, thereby improving the beneficiation quality of the selected titanium ore.
[0011] Preferably, in the mineral recovery method of high-phosphorus vanadium titanium magnetite tailings described in the present invention, the particle size control value of the fine screening classification is selected to be 0.045 mm.
[0012] As a preferred embodiment of the present invention, by selecting the value of the particle size control selected by the fine screening classification as 0.045mm, the undersize ore with a particle size of ≤0.045mm obtained by fine screening classification is concentrated-two-stage strong magnetic-re-concentration, and the mineral with a slurry concentration of 45% and a TiO2 grade of 18.50% can be obtained as a flotation raw material, the grade of titanium dioxide in the fine concentrate is greater than 15%, and the fine-grained titanium ore in the high-phosphorus vanadium titanium magnetite tailings is recovered at a high recovery rate, further improving the resource recovery rate; and the oversize ore with a particle size ≥0.045mm will not follow the fine concentrate into the flotation titanium, and will not affect the quality of the titanium ore after flotation, thereby further improving the beneficiation quality of the selected titanium ore.
[0013] Preferably, in the mineral recovery method of high-phosphorus vanadium titanium magnetite tailings described in the present invention, the magnetic field strength of the first stage of strong magnetism is 10000 GS, and the magnetic field strength of the second stage of strong magnetism is 5000 GS.
[0014] As a preferred solution of the present invention, by performing a stage of strong magnetization before cyclone classification, interference bed separation and fine screen classification, not only can the high-phosphorus vanadium titanium magnetite tailings be magnetically separated once, but also according to the specificity of the material used in the present invention, the high-phosphorus vanadium titanium magnetite is selected, and the magnetic field strength of the first stage of strong magnetization is selected to be 10000GS, which can improve the efficiency of magnetic separation; and then by performing a second stage of strong magnetization after cyclone classification, interference bed separation and fine screen classification, the magnetic field strength of the second stage of strong magnetization is preferably 5000GS, and the overflow ore after fine screen classification is used for the second stage of magnetic separation. Since the medium box with a smaller gap is more conducive to improving the concentrate grade in the strong magnetic separation stage, the unclassified strong magnetic coarse concentrate is easy to block the medium box when entering the strong magnetic concentration operation, resulting in a poor strong magnetic separation process. Therefore, the magnetic field strength of the strong magnetic is adjusted by two stages, and coordinated with the order of cyclone classification, interference bed separation and fine screen classification, the classification particle size and the strong magnetic operation are balanced in terms of recovery rate and operation efficiency, and the recovery rate and production efficiency are further optimized.
[0015] Preferably, the mineral recovery method of high-phosphorus vanadium-titanium magnetite tailings of the present invention, said S1 specifically comprises the following steps:
[0016] S11: The strong magnetic coarse concentrate is classified by a cyclone into a first underflow ore and a first overflow ore;
[0017] S12: The first underflow ore is sorted through an interference bed to obtain a second underflow ore and a second overflow ore.
[0018] As a preferred embodiment of the present invention, the strong magnetic coarse concentrate is classified by cyclone classification, and the coarse concentrate after the first stage of strong magnetization is classified into a first underflow ore with larger particle size and a first overflow ore with smaller particle size. The first underflow ore with larger particle size is sorted into a second underflow ore with larger particle size and higher density through an interference bed. Classification is performed before sorting, and the properties of the titanium ore body filled with fine-grained gangue are fully considered. Since the coarse-grained concentrate with lower density but larger particle size enters the fine screen classification, the efficiency of the fine screen classification will be reduced and the medium box of the second stage of strong magnetism will be easily blocked, so as to avoid the coarse-grained concentrate that has not been classified and sorted from entering the second stage of strong magnetism to block the medium box, so that the fine screen classification and the second stage of strong magnetism operation are smoother, thereby improving the ore dressing efficiency. On the other hand, uniform fine-grained minerals enter the second stage of strong magnetism operation, which reduces the processing volume of strong magnetism, reduces electricity consumption, and improves production efficiency.
[0019] Preferably, in the mineral recovery method of high-phosphorus vanadium-titanium magnetite tailings of the present invention, S3 further comprises the following steps:
[0020] S31: The underflow ore and the overscreen ore are roughly separated through a spiral chute at least once to obtain a gravity separation rough concentrate and a gravity separation rough tailings;
[0021] S32: The gravity-selected coarse concentrate is recovered by at least three times of superposition of the spiral chute, and the gravity-selected ore is obtained; the TiO2 grade of the gravity-selected ore is greater than 25%; the recovered gravity-selected ore is subjected to ore grinding operation, and then enters the titanium selection process of the beneficiation plant again to start beneficiation;
[0022] S33: The coarse tailings from the gravity separation are recovered by at least one sweeping through a spiral chute to obtain gravity separation tailings; the TiO2 grade of the gravity separation tailings is lower than 2.00%.
[0023] As a preferred embodiment of the present invention, the fine-grained gangue that has not been dissociated by fine grinding is sorted into the underflow, and can be re-selected in a spiral chute together with the ore on the screen, thereby obtaining re-selected ore and re-selected tailings. With the action of S1 and S2, there are fewer fine particles in the underflow, which is more conducive to the subsequent spiral chute sorting to pre-enrich the coarse-grained ilmenite, so that the titanium dioxide grade of the re-selected ore is greater than 25%; after the re-selected ore is ground, the titanium dioxide grade of the concentrator is carried out again, so that the ore with larger particle size in the tailings is re-ground and sorted, so that the titanium ore contained in the re-selected ore can be recovered as much as possible, and the TiO2 grade of the re-selected tailings is lower than 2.00%, thereby reducing the titanium ore grade in the re-selected tailings, indicating that the titanium ore is further recovered, thereby further improving the final titanium ore grade.
[0024] Preferably, the mineral recovery method of high-phosphorus vanadium-titanium magnetite tailings of the present invention further comprises step S4: flotation desulfurization of the flotation raw material, specifically comprising the following steps:
[0025] S42: 600 g / t sulfuric acid is added to the first sulfur ore, and after a concentration, the obtained minerals include the second sulfur ore and the third sulfur ore;
[0026] S43: After adding 300g / t sulfuric acid to the second sulfur ore and performing secondary concentration, the first intermediate ore obtained is returned to the primary concentration and the concentrate obtained is added with 200g / t sulfuric acid for tertiary concentration. The minerals obtained by the tertiary concentration include sulfur-cobalt concentrate and the second intermediate ore, and the second intermediate ore is returned to the secondary concentration; the S grade of the sulfur-cobalt concentrate is 30.79%;
[0027] S44: 100 g / t sulfuric acid is added to the third sulfur ore and scavenged, and the obtained minerals are returned to the primary concentration and form floating sulfur tailings.
[0028] As a preferred embodiment of the present invention, the mineral recovery method of the high-phosphorus vanadium titanium magnetite tailings can obtain a sulfur-cobalt concentrate with an S grade of 30.79% and an S recovery rate of 83.04% through a flotation desulfurization process, which can be sold as a product to generate economic benefits. In addition, the S grades in the generated floating sulfur tailings and floating phosphorus raw materials are 0.139% and 0.053%, respectively, indicating that combined with the classification effect of S1-S3, the sulfur recovery and separation effects are better, and the S content in the floating sulfur tailings and floating phosphorus raw materials is further reduced, and the negative impact of the co-existing sulfur element on the subsequent titanium resource recovery is eliminated to a certain extent, and a higher grade of sulfur-cobalt concentrate is recovered; all under neutral conditions and after roughing, the pH value is adjusted to carry out floating sulfur selection and floating phosphorus selection, which greatly reduces the amount of adjusting agent used in the flotation process, and reduces the negative impact on the flotation titanium selection process, thereby promoting the acquisition of high-quality titanium concentrate.
[0029] Phosphorus is a harmful impurity in titanium concentrate, and the industry generally requires that the phosphorus content in titanium concentrate is less than 0.05%. For ordinary low-phosphorus vanadium titanium magnetite, the phosphorus content in the titanium concentrate can be reduced by adding inhibitors; however, when the phosphorus content in the floating raw material is greater than 0.3%, such as the phosphorus content of the high-phosphorus vanadium titanium magnetite tailings of the present invention is 1%, it affects the acquisition of titanium concentrate products with higher titanium ore grades; therefore, the mineral recovery method of the high-phosphorus vanadium titanium magnetite tailings of the present invention is further improved, and the floating phosphorus raw material is subjected to flotation dephosphorization after flotation desulfurization, and the flotation dephosphorization specifically includes the following steps:
[0030] S45: Select the floating phosphorus raw material for flotation dephosphorization test, add 200g / t collector and perform rough selection once, and the obtained minerals include the first phosphate ore and floating titanium raw material; the collector is a composite agent composed of oxidized paraffin soap and MES in a ratio of 9:1; the MES is sodium fatty acid methyl ester sulfonate, which is an anionic collector; the TiO2 grade in the floating titanium raw material is 18.53%;
[0031] S46: The first phosphate ore is concentrated and recovered at least once to obtain phosphorus-containing tailings; the recovered second phosphate ore is returned to S45 for rough selection again.
[0032] As a preferred embodiment of the present invention, on the basis of obtaining floating phosphorus raw materials after flotation desulfurization, the floating phosphorus raw materials are further subjected to flotation dephosphorization to obtain phosphorus-containing tailings with a P grade of 6.60% and a P recovery rate of 60.56%. Not only the phosphorus tailings are recovered, but also qualified phosphorus concentrate products are obtained by further enrichment, thereby improving the recovery rate of phosphorus ore in high-phosphorus vanadium titanium magnetite tailings, thereby improving the economic benefits; and, after combining S1-S3, flotation desulfurization and flotation dephosphorization, the flotation titanium material is obtained for flotation titanium ore, eliminating the influence of sulfur ore and phosphate ore on the flotation titanium ore, so that the grade of titanium ore in the floating titanium raw material is increased to 18.53%, which is convenient for the recovery of titanium in the flotation titanium selection stage, reduces the difficulty of flotation titanium selection, and further realizes the efficient separation and recovery of titanium ore; all under neutral conditions and after roughing, the pH value is adjusted to carry out floating sulfur selection and floating phosphorus selection, which greatly reduces the amount of adjusting agent used in the flotation process, reduces the negative impact on the flotation titanium selection process, and promotes the acquisition of high-quality titanium concentrate.
[0033] Preferably, the mineral recovery method of the high-phosphorus vanadium-titanium magnetite tailings of the present invention comprises flotation of titanium ore on the titanium flotation raw material after flotation dephosphorization, and the flotation of titanium ore specifically comprises the following steps:
[0034] S47: Selecting a floating titanium raw material for a flotation titanium selection test, adding 1500 g / t of sulfuric acid, 1000 g / t of a depressant, 2500 g / t of a collector and 300 g / t of diesel and performing a rough selection once, to obtain a first titanium concentrate and a first titanium tailings;
[0035] 1200 g / t of sulfuric acid and 500 g / t of collector are added to the first titanium concentrate and subjected to primary concentration to obtain the second titanium concentrate and the first titanium middlings, and the first titanium middlings are returned to the roughing separation for further separation;
[0036] After adding 800 g / t of sulfuric acid and 300 g / t of collector to the second titanium concentrate and performing secondary concentration, the third titanium concentrate and the second titanium middlings are obtained, and the second titanium middlings are returned to the primary concentration for further separation;
[0037] 400 g / t of sulfuric acid and 200 g / t of collector are added to the third titanium concentrate and the concentrate is refined three times to obtain the fourth titanium concentrate and the third titanium middlings. The third titanium middlings are returned to the secondary refinement for further separation.
[0038] After adding 400 g / t of sulfuric acid to the fourth titanium concentrate and performing the fourth concentration, titanium concentrate and the fourth titanium middlings are obtained, and the fourth titanium middlings are returned to the third concentration for further separation;
[0039] After adding 300g / t of sulfuric acid and 200g / t of collector to the first titanium tailings and scavenging, the fifth titanium middlings and flotation tailings are obtained, and the fifth titanium middlings are returned to the roughing separation for further sorting; the TiO2 grade of the titanium concentrate reaches 47.50%; the TiO2 grade of the flotation tailings is lower than 2.50%.
[0040] As a preferred solution of the present invention, the titanium ore with finer particle size is recycled by sequentially undergoing cyclone classification, interference bed separation and fine screen separation, or sequentially undergoing cyclone classification, interference bed separation and fine screen separation, spiral chute re-selection, desulfurization and dephosphorization processes; or the tailings with higher density such as fine-grained gangue such as calcite or titanite are classified and recycled after re-grinding; and the influence of sulfur and phosphate ore on the flotation of titanium ore is eliminated, thereby achieving an increase in the grade of titanium concentrate for flotation of titanium to 47.50%, an increase in the recovery rate of titanium ore to 91.46%, and a TiO2 grade of only 2.46% in the flotation tailings.
[0041] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0042] 1. The present invention can separate the strong magnetic rough concentrate into underflow ore with larger particle size and overflow ore with smaller particle size by subjecting the rough concentrate to cyclone classification and interference bed separation after a stage of strong magnetic rough separation; the overflow ore with smaller particle size is further subjected to fine screening classification to obtain undersize ore with smaller and uniform particle size, and the undersize ore with smaller and uniform particle size is further subjected to a second stage of strong magnetic separation to obtain a fine-grained concentrate; the fine-grained concentrate is then concentrated in step S3 and used as a flotation raw material, thereby recovering the fine-grained titanium ore in the high-phosphorus vanadium titanium magnetite tailings, so that the slurry concentration of the flotation raw material is 45%, the TiO2 grade is 18.53%, and the grade of titanium dioxide in the fine concentrate is greater than 15%, thereby improving the resource recovery rate;
[0043] 2. After cyclone classification and interference bed separation, the coarse-grained gangue that has not been finely ground and dissociated is separated into the bottom flow and will not follow the fine-grained concentrate into the flotation titanium, and will not affect the quality of the titanium ore after flotation, thereby improving the beneficiation quality of the selected titanium ore. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is a schematic flow diagram of the mineral recovery method of high-phosphorus vanadium titanium magnetite tailings of the present invention;
[0045] Figure 2 It is a schematic diagram of the flotation desulfurization process of the present invention;
[0046] Figure 3 It is a schematic diagram of the flotation dephosphorization process of the present invention;
[0047] Figure 4 It is a schematic diagram of the process of flotation separation of titanium according to the present invention. DETAILED DESCRIPTION
[0048] The present invention will be described in detail below in conjunction with the accompanying drawings.
[0049] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0050] It should be noted that the high-phosphorus vanadium titanium magnetite tailings described in the present invention come from the ore dressing plant of Chongqing Iron and Steel Xichang Mining Co., Ltd. Before the mineral recovery of the present invention, the TiO2 grade of the high-phosphorus vanadium titanium magnetite tailings is 5.06%, the S grade is 0.33%, and the P content is 1%.
[0051] Example 1
[0052] This embodiment provides a method for recovering minerals from high-phosphorus vanadium-titanium magnetite tailings. Figure 1 The process shown includes the following steps:
[0053] S1: After a period of strong magnetic roughing, the tailings of high phosphorus vanadium titanium magnetite are subjected to strong magnetic rough concentrate and the first strong magnetic tailings; the strong magnetic rough concentrate is subjected to cyclone classification and interference bed separation respectively to obtain underflow ore and overflow ore; the particle size of the underflow ore is larger than that of the overflow ore;
[0054] S2: The overflow ore is finely screened and classified to obtain oversize ore and undersize ore. The particle size of the oversize ore is larger than that of the undersize ore.
[0055] S3: After the undersize ore is concentrated, it is subjected to two-stage strong magnetic concentration to obtain fine-grained concentrate and the second strong magnetic tailings; the fine-grained concentrate is concentrated to form flotation raw materials; the TiO2 grade of the second strong magnetic tailings is lower than 3.31%; the TiO2 grade of the flotation raw materials is greater than 15%.
[0056] Specifically, the mineral recovery method of high-phosphorus vanadium-titanium magnetite tailings described in this embodiment can recover titanium ore or other minerals from the classified fine-grained ore. After step S1, the vanadium-titanium magnetite strong magnetic separation titanium tailings are subjected to strong magnetic separation roughing to obtain strong magnetic rough concentrate, the first strong magnetic tailings are discarded, and the strong magnetic rough concentrate is then graded and sorted respectively through a cyclone and an interference bed.
[0057] In this embodiment, the magnetic field strength of the magnetic field is selected according to the actual needs of mineral processing. The magnetic field strength of the first stage magnetic field can be selected from 8000GS to 12000GS, and the magnetic field strength of the second stage strong magnet can be selected from 4000Gs to 8000Gs. It is also preferred that the magnetic field strength of the first stage strong magnet is 10000GS, and the magnetic field strength of the second stage strong magnet is 5000GS. Combined with the control of the grading particle size of the cyclone and the grading particle size of the fine screen, the concentrated bottom flow concentration of the underscreen ore is 30%, the concentrated bottom flow concentration after the second stage strong magnet is 45%, and the TiO2 grade of the second stage strong magnetic concentrate is greater than 15%.
[0058] Specifically, refer to Figure 1 In the process flow shown in the figure, the particle size of the cyclone classification and the interference bed separation is controlled in the range of -0.15mm to +0.075mm; for example, the overflow ore with a particle size of ≤0.075mm enters the fine screen classification, and then is concentrated and subjected to the second stage of strong magnetic separation, or the overflow ore with a particle size of ≤0.15mm enters the fine screen classification, and then is concentrated and subjected to the second stage of strong magnetic separation to form a flotation raw material; more specifically, the value of the fine screen classification is preferably selected to be 0.045mm; a mineral with a pulp concentration of 45% and a TiO2 grade of 18.53% can be obtained as a flotation raw material, the grade of titanium dioxide in the fine concentrate is greater than 15%, and the TiO2 grade of the second strong magnetic tailings after fine screen classification is less than 3.31%. The test results are shown in Table 1.
[0059] Table 1: Test results of Example 1
[0060] Product Name Yield (%) <![CDATA[TiO2 grade (%)]]> <![CDATA[Recovery rate of TiO2(%)]]> Flotation raw materials 13.65 18.53 49.99 Coarse concentrate 9.47 10.63 19.89 The second strongest magnetic tailings 11.83 3.31 7.76 The first strong magnetic tailings 65.02 1.74 22.36 total 100.00 5.06 100.00
[0061] It should be noted that the cyclone classification principle is: the mixture enters the cyclone along the tangential direction under the action of external pressure to obtain an external vortex; the particles with higher density, heavier weight and larger particle size are finally discharged from the bottom flow port, and the components with lower density, lighter weight and smaller particle size move toward the central axis to form an internal vortex and are discharged through the overflow port to achieve the separation of two phases with different densities; It should be noted that the interference layer bed convection sorting principle is: the slurry is fed tangentially into the feed well of the equipment, and an upward disturbed water flow is formed through the turbulence plate. The particles with higher density will sink to the bottom of the bed to form an underflow; while the particles with lower density float on the upper layer to form an overflow.
[0062] It should be noted that the grading principle of the interference bed separator is as follows: the slurry is fed tangentially into the feed well of the equipment, and water is pumped into the distributor at the bottom of the separator by a pump at a predetermined pressure and flow rate, and is evenly distributed to the bottom of the interference bed separator through the turbulence plate, forming an upward disturbed water flow. The descending material meets the rising water flow to form an interference layer or boiling bed. The particles in the feed perform interference sedimentation movement in the separator. Due to the different densities between the particles, there are differences in the interference sedimentation speed, which provides a basis for sorting. When a stable state is reached, particles in the feed with a density higher than the average density of the interference bed will enter the bed into the sedimentation flow and be discharged through the discharge port at the bottom, and particles with a density lower than the average density of the interference bed will be discharged through the top overflow port.
[0063] Specifically, in this embodiment, S1 specifically includes the following steps: S11: the coarse concentrate is classified by a cyclone to be divided into a first underflow ore and a first overflow ore, and the particle size of the first underflow ore is larger than that of the first overflow ore; S12: the first underflow ore is sorted by an interference bed to obtain a second underflow ore and a second overflow ore, and the density of the second underflow ore is larger than that of the second overflow ore.
[0064] It should be noted that the "coarse" and "fine" in the coarse concentrate or fine concentrate of the present invention are relative to each other and are mineral names defined only for the convenience of distinction. They can be distinguished according to the value of particle size control, and are not defined in a general sense.
[0065] The mineral recovery method of high-phosphorus vanadium titanium magnetite tailings described in this embodiment improves the grade of TiO2 in the flotation raw material. Then, the flotation raw material is used for titanium selection in the subsequent process. The general flotation titanium selection method can be used to float titanium ore, thereby improving the recovery rate of the final titanium ore.
[0066] Comparative Example 1
[0067] Comparative Example 1 uses high-phosphorus vanadium titanium magnetite tailings with a TiO2 grade of 5.06%, an S grade of 0.33%, and a P content of 1%. The difference between Comparative Example 1 and Example 1 is that in Comparative Example 1, only fine screening is used for classification after a first-stage strong magnetic roughing, and no cyclone classification and interference bed separation are performed; other parameters such as the magnetic field intensity, the value of the fine screen classification particle size control, etc. can be set with reference to the same conditions as Example 1. Specifically, in Comparative Example 1, the high-phosphorus vanadium titanium magnetite tailings are subjected to a first-stage strong magnetic roughing to obtain a coarse concentrate, and the first strong magnetic tailings are discarded, and then the coarse concentrate is screened for coarse and fine classification, and the classification particle size is controlled to be 0.045 mm. The part with a particle size less than 0.045 mm enters concentration-second-stage strong magnetic separation-concentration, and the bottom flow with a pulp concentration of 45% is obtained as a flotation raw material. The test results are shown in Table 2.
[0068] Table 2: Comparative Example 1 Test Results
[0069] Product Name Yield (%) <![CDATA[TiO2 grade (%)]]> <![CDATA[TiO2 recovery rate (%)]]> Flotation raw materials 11.68 16.39 37.83 Coarse concentrate 14.37 12.15 34.51 The second strongest magnetic tailings 8.00 3.86 6.10 The first strong magnetic tailings 65.95 1.65 21.56 total 100.00 5.06 100.00
[0070] Comparing Table 2 with Table 1, it can be seen that the titanium tailings of the vanadium-titanium magnetite strong magnetic separation were not subjected to cyclone classification and interference bed separation after a strong magnetic separation. After only fine screening and coarse separation, the TiO2 grade of the obtained flotation raw material was reduced to 16.39%, and the TiO2 recovery rate dropped significantly to only 37.83%. At the same time, the TiO2 grade in the second strong magnetic tailings was higher than that in Example 1, indicating that the separation effect of Comparative Example 1 was weaker than that of Example 1; in addition, the applicant found that during the test, the classification efficiency of Comparative Example 1 was only 50% of the classification efficiency of Example 1.
[0071] Example 2
[0072] On the basis of Example 1, the mineral recovery method of high phosphorus vanadium titanium magnetite tailings is further improved, referring to Figure 1 In the process flow shown, S3 further includes the following steps:
[0073] S31: The underflow ore and the ore on the screen pass through the spiral chute for at least one roughing to obtain the gravity separation rough concentrate and gravity separation rough tailings;
[0074] S32: The gravity-selected coarse concentrate is recovered through at least three times of superimposed concentration in a spiral chute, and a gravity-selected ore is obtained; the TiO2 grade of the gravity-selected ore is greater than 25%; the recovered gravity-selected ore is ground and then enters the titanium selection process of the beneficiation plant again to start beneficiation.
[0075] S33: The coarse tailings from the gravity separation are recovered by at least one sweeping through a spiral chute to obtain gravity separation tailings; the TiO2 grade of the gravity separation tailings is lower than 2.00%.
[0076] Specifically, refer to Figure 1 As shown, on the basis of Example 1, after a section of strong magnetic coarse concentrate is subjected to cyclone classification, interference bed separation and fine screen classification through the S1-S2 process steps, not only a fine concentrate with a smaller particle size is obtained as a flotation raw material, but also an underflow ore and an overscreen ore with a larger particle size than the underscreen ore are obtained, for example, an underflow ore with a particle size greater than 0.15 mm or greater than 0.075 mm and an overscreen ore with a particle size greater than 0.045 mm are obtained, and after at least one roughing separation through a spiral chute, at least three superimposed fine separations are respectively carried out, and at least one scavenging separation is carried out to recover the titanium ore in the coarse concentrate, and a gravity separation ore and a gravity separation tailings are obtained.
[0077] In this embodiment, the test conditions in the S1-S2 step are set to the test conditions selected in the embodiment, such as the magnetic field strength and the classification particle size setting, and the optional range provided in Example 1 is selected. The test results obtained are shown in Table 3. Through the coordination of S3 and S1-S2, and then through the spiral chute gravity separation, the TiO2 grade of the gravity separation ore is 28.53%, which can be returned to the original process of the concentrator for separation; the TiO2 grade of the gravity separation tailings is 1.56%, indicating that through the spiral chute gravity separation, the recovery of titanium ore is further increased, the titanium ore grade in the tailings is reduced, and the titanium resources are further recycled.
[0078] Table 3: Test results of Example 2
[0079]
[0080]
[0081] It should be noted that spiral chute gravity separation is understood as the use of the difference in specific gravity of different mineral particles to achieve separation. Although specific gravity is the main basis for sorting, the size and shape of the particles will also affect their behavior in the spiral chute; larger or irregularly shaped particles may settle more easily to form coarse ores, while smaller or spherical particles may move more easily with the water flow to form fine ores; mineral particles with higher density will slide down the slope faster due to gravity to form heavy ores, while particles with lower density will move slower or be discharged with the water flow to become light ores.
[0082] In this embodiment, after the spiral chute gravity separation, the coarse heavy ore with larger particles and heavier weight is subjected to at least three rounds of concentration to form the gravity separation medium, and the fine light ore with smaller particles and lighter weight is scavenged and recovered to form the gravity separation tailings. The lower the TiO2 grade in the gravity separation tailings, the better the separation effect of the titanium ore by using the present invention.
[0083] Comparative Example 2
[0084] The coarse-grained concentrate obtained in Comparative Example 1 was subjected to a spiral process gravity separation test. The process steps and process parameter settings of S3 in Example 2 were adopted. The spiral chute gravity separation was a traditional process of primary roughing, tertiary concentration and primary scavenging. The test results are shown in Table 4 below. The TiO2 grade of the gravity separation ore obtained in the comparative example 2 test was lower than that in Example 2, while the TiO2 grade of the gravity separation tailings was higher than that in Example 2, indicating that the effect of comparative example 2 is weaker than that of Example 2.
[0085] Table 4: Test results of comparative example 2
[0086]
[0087]
[0088] Example 3
[0089] In this embodiment, based on Example 1, Figure 2 In the process shown, the S4 comprises the following steps:
[0090] S41: Select flotation raw materials, add 600g / t of xanthate and 150g / t of frother and perform one-time roughing, and the obtained minerals include floating phosphorus raw materials and first sulfur ore; the S grade of the floating phosphorus raw materials is 0.053%;
[0091] S42: 600 g / t sulfuric acid is added to the first sulfur ore, and after a concentration, the obtained minerals include the second sulfur ore and the third sulfur ore;
[0092] S43: After adding 300g / t sulfuric acid to the second sulfur ore and performing secondary concentration, the first intermediate ore obtained is returned to the primary concentration and the concentrate obtained is added with 200g / t sulfuric acid for tertiary concentration, and the obtained minerals include sulfur-cobalt concentrate and the second intermediate ore; the S grade of the sulfur-cobalt concentrate is 30.79%;
[0093] S44: 100 g / t sulfuric acid is added to the third sulfur ore and scavenged, and the obtained minerals are returned to the primary concentration and form floating sulfur tailings.
[0094] Specifically, flotation desulfurization test: The flotation raw material obtained in Example 1 was subjected to a flotation desulfurization test. The dosage of each reagent was 600 g / t of xanthate, 150 g / t of frother, and 1200 g / t of sulfuric acid. The results of the flotation desulfurization test are shown in Table 5.
[0095] Table 5: Test results of flotation desulfurization using the flotation raw materials of Example 1
[0096] Product Name Yield (%) S grade (%) S recovery rate (%) Cobalt Sulfide Concentrate 0.89 30.79 83.04 Floating sulfur tailings 4.01 0.139 1.69 Floating phosphorus raw materials 95.10 0.053 15.27 total 100.00 0.33 100.00
[0097] The test results show that through Figure 2 The flotation desulfurization process shown can obtain a sulfur-cobalt concentrate with an S grade of 30.79% and an S recovery rate of 83.04%, which can be sold as a product to generate economic benefits; the S grades in the generated floating sulfur tailings and floating phosphorus raw materials are 0.139% and 0.053%, respectively, indicating that the desulfurization test is carried out in combination with the flotation raw materials obtained in Example 1, and the enrichment and separation effect of sulfur is better, which eliminates the negative impact of the co-existing sulfur element on the subsequent titanium resource recovery to a certain extent.
[0098] Comparative Example 3
[0099] The flotation raw material obtained in Comparative Example 1 was subjected to a flotation desulfurization test. The dosage of each reagent was 600 g / t of yellow medicine, 150 g / t of No. 2 oil, and 1200 g / t of sulfuric acid. For the specific process, refer to Figure 2 The test process of Example 3 is shown; the difference between Comparative Example 3 and Example 3 is that Comparative Example 3 uses flotation raw materials prepared from Comparative Example 1, and Example 3 uses flotation raw materials prepared from Example 1; Table 6 shows the flotation desulfurization test results of Comparative Example 3 using flotation raw materials from Comparative Example 1.
[0100] Table 6: Flotation desulfurization test results of Comparative Example 3 using flotation raw materials from Comparative Example 1
[0101] Product Name Yield (%) S grade (%) S recovery rate (%) Cobalt Sulfide Concentrate 0.84 30.180 76.82 Floating sulfur tailings 5.00 0.249 3.78 Floating phosphorus raw materials 94.16 0.068 19.40 total 100.00 0.330 100.00
[0102] From the comparison between Table 6 and Table 5, it can be seen that when only fine screening classification is used in the pre-enrichment process, the S grade in the obtained cobalt-sulfide concentrate is reduced to 30.180%, and the S recovery rate is reduced to 76.82%; the S grade and recovery rate in the floating phosphorus raw material change to 0.249% and 19.40%, indicating that the combined classification method has a promoting effect on the subsequent flotation effect.
[0103] Example 4
[0104] In Example 4, the floating phosphorus raw material obtained after flotation desulfurization using the flotation raw material in Example 1 is used in Example 3, that is, the floating phosphorus raw material used is the same as that in Example 3, and a flotation dephosphorization test is carried out. Figure 3 As shown, the flotation dephosphorization specifically includes the following steps:
[0105] S45: the floating phosphorus raw material is selected for flotation dephosphorization test, 200g / t collector is added and roughly selected once, and the obtained minerals include the first phosphate ore and the floating titanium raw material; the collector is a composite agent composed of oxidized paraffin soap and MES in a ratio of 9:1; the MES is sodium fatty acid methyl ester sulfonate, which is a typical anionic collector; the TiO2 grade in the floating titanium raw material is 18.53%;
[0106] S46: The first phosphate ore is recovered through at least one concentration and phosphorus-containing tailings are obtained; the recovered second phosphate ore is returned to S45 for rough selection again.
[0107] For details, please refer to the above process flow Figure 3 As shown, on the basis of completing the flotation desulfurization test, a flotation dephosphorization test was carried out: Example 4 selected Example 3 as the flotation raw material, and the obtained floating phosphorus raw material was subjected to a flotation dephosphorization test. The collector was a composite reagent composed of oxidized paraffin soap and MES in a ratio of 9:1, and the dosage was 200g / t of floating raw material. The results of the flotation dephosphorization test are shown in Table VII.
[0108] Table 7: Example 4 flotation dephosphorization test results
[0109] Product Name Yield (%) P grade (%) P recovery rate (%) Phosphorus tailings 5.23 6.60 60.56 Floating titanium raw materials 94.77 0.24 39.44 total 100.00 0.57 100.00
[0110] The test results show that through the flotation dephosphorization test shown in Example 4, a phosphorus-containing tailings with a P grade of 6.60% and a P recovery rate of 60.56% can be obtained, the P grade in the floating titanium raw material is 0.24%, the sorting effect is good, and the phosphorus-containing tailings can be further enriched by flotation to obtain a qualified phosphate concentrate product.
[0111] Comparative Example 4
[0112] Comparative Example 4: Comparative Example 3 uses the flotation raw material in Comparative Example 1, and the floating phosphorus raw material obtained after flotation desulfurization, that is, the floating phosphorus raw material used is the same as that in Comparative Example 3, and a flotation dephosphorization test is carried out. The collector is a composite agent composed of oxidized paraffin soap and MES in a ratio of 9:1, and the dosage is 200g / t; this comparative example uses the following as shown in Example 4 Figure 3 The method and process shown, the test results are shown in Table 8; the difference between Comparative Example 4 and Example 4 is that the floating phosphorus raw material used in Comparative Example 4 is obtained from Comparative Example 3.
[0113] Table 8: Comparative Example 4 flotation dephosphorization test results
[0114] Product Name Yield (%) P grade (%) P recovery rate (%) Phosphorus tailings 5.15 6.05 54.66 Floating titanium raw materials 94.85 0.27 45.34 Floating phosphorus raw materials 100.00 0.57 100.00
[0115] By comparing Comparative Example 4 with Example 4, it can be seen that under the same reagent system and flotation process conditions, only the fine screening classification method has an inhibitory effect on the flotation dephosphorization process. The P grade and phosphorus recovery rate in the obtained phosphorus-containing tailings are lower than those in Example 4, which are 6.05% and 54.66% respectively. The P grade in the obtained floating titanium raw material increases to 0.27%, which will increase the difficulty of flotation titanium selection.
[0116] Example 5
[0117] On the basis of Example 4, the mineral recovery method of high-phosphorus vanadium-titanium magnetite tailings of the present invention is to flotate titanium ore on the floating titanium raw material after flotation dephosphorization. The specific process is referred to Figure 4 As shown, the flotation of titanium ore specifically includes the following steps:
[0118] S47: Selecting floating titanium raw materials for flotation titanium selection test, adding 1500g / t of sulfuric acid, 1000g / t of inhibitor, 2500g / t of collector and 300g / t of diesel and performing a roughing selection, a first titanium concentrate and a first titanium tailing are obtained; 1200g / t of sulfuric acid and 500g / t of collector are added to the first titanium concentrate and a first concentration is performed to obtain a second titanium concentrate and a first titanium middling, and the first titanium middling is returned to the roughing selection for reselection; 800g / t of sulfuric acid and 300g / t of collector are added to the second titanium concentrate and a second concentration is performed to obtain a third titanium concentrate and a second titanium middling, and the second titanium middling is returned to the first concentration for reselection; 4 00g / t of sulfuric acid and 200g / t of collector and after three concentrations, the fourth titanium concentrate and the third titanium middlings were obtained, and the third titanium middlings were returned to the secondary concentration for re-selection; 400g / t of sulfuric acid was added to the fourth titanium concentrate and after four concentrations, titanium concentrate and the fourth titanium middlings were obtained, and the fourth titanium middlings were returned to the tertiary concentration for re-selection; 300g / t of sulfuric acid and 200g / t of collector were added to the first titanium tailings and after scavenging, the fifth titanium middlings and flotation tailings were obtained, and the fifth titanium middlings were returned to the roughing for re-selection; the TiO2 grade of the titanium concentrate reached 47.50%; the TiO2 grade of the flotation tailings was lower than 6.06%; the test results obtained are shown in Table 9.
[0119] Table 9: Experimental results of titanium flotation in Example 5
[0120] Product Name Yield (%) <![CDATA[TiO2 grade (%)]]> <![CDATA[TiO2 recovery rate (%)]]> Titanium Concentrate 35.68 47.50 91.46 Flotation tailings 64.32 2.46 8.54 Floating titanium raw materials 100.00 18.53 100.00
[0121] The test results show that through Figure 4 The titanium flotation process shown in the figure was used for titanium separation test, and titanium concentrate with a TiO2 grade of 47.50% was obtained. The TiO2 recovery rate was 91.46%, and the TiO2 grade in the flotation tailings was only 2.46%, thus realizing the efficient separation and recycling of titanium resources.
[0122] Comparative Example 5
[0123] Comparative Example 5 The titanium flotation raw material obtained in Comparative Example 3 was subjected to a titanium flotation test. The process flow was as shown in Example 5. Figure 4 The process is as follows, and the dosage of each reagent is referenced to Example 5. Table 10 is the flotation test results of titanium in Comparative Example 5; the difference between Comparative Example 5 and Example 5 is that Comparative Example 5 uses the flotation raw material obtained from Comparative Example 4, and Example 5 uses the flotation raw material obtained from Example 4.
[0124] Table 10: Comparative Example 5 Flotation Titanium Selection Test Results
[0125] Product Name Yield (%) <![CDATA[TiO2 grade (%)]]> <![CDATA[TiO2 recovery rate (%)]]> Titanium Concentrate 30.46 45.83 85.17 Flotation tailings 69.54 3.49 14.83 Floating titanium raw materials 100.00 16.39 100.00
[0126] By comparing Comparative Example 5 with Example 5, it can be seen that only fine screening classification in the pre-enrichment process will not increase the TiO2 grade in the titanium concentrate, and may even reduce the grade of the titanium concentrate. It can be seen that the grade of the titanium concentrate obtained by flotation separation of titanium through cyclone classification, interference bed separation and fine screening classification, spiral chute gravity separation, desulfurization and dephosphorization processes is increased to 47.50%, thereby improving the recovery rate of titanium ore.
[0127] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A mineral recovery method for high-phosphorus vanadium-titanium magnetite tailings, characterized in that: The following steps are involved: S1: After a period of strong magnetic roughing, the tailings of high phosphorus vanadium titanium magnetite are subjected to strong magnetic rough concentrate and the first strong magnetic tailings; the strong magnetic rough concentrate is subjected to cyclone classification and interference bed separation in turn to obtain underflow ore and overflow ore; S2: The overflow ore is subjected to fine screening and classification to obtain oversize ore and undersize ore; S3: After the undersize ore is concentrated, it is subjected to two-stage strong magnetic concentration to obtain fine-grained concentrate and a second strong magnetic tailings; the fine-grained concentrate is concentrated to form flotation raw material; the TiO2 grade of the second strong magnetic tailings is lower than 3.31%; the TiO2 grade of the flotation raw material is greater than 15%.
2. The mineral recovery method of high-phosphorus vanadium-titanium magnetite tailings according to claim 1, characterized in that: The particle size control value of the fine screen classification is selected as 0.045 mm.
3. The mineral recovery method of high-phosphorus vanadium-titanium magnetite tailings according to claim 1, characterized in that: The magnetic field strength of the first stage of strong magnetism is 10000 GS, and the magnetic field strength of the second stage of strong magnetism is 5000 GS.
4. The mineral recovery method of high-phosphorus vanadium-titanium magnetite tailings according to claim 1, characterized in that: The S1 specifically includes the following steps: S11: The strong magnetic coarse concentrate is classified by a cyclone into a first underflow ore and a first overflow ore; S12: The first underflow ore is sorted through an interference bed to obtain a second underflow ore and a second overflow ore.
5. The mineral recovery method of high-phosphorus vanadium-titanium magnetite tailings according to claim 1, characterized in that: The S3 further comprises the following steps: S31: The underflow ore and the overscreen ore are roughly separated through a spiral chute at least once to obtain a gravity separation rough concentrate and a gravity separation rough tailings; S32: The gravity-selected coarse concentrate is recovered by at least three times of superposition of the spiral chute, and the gravity-selected ore is obtained; the TiO2 grade of the gravity-selected ore is greater than 25%; the recovered gravity-selected ore is subjected to ore grinding operation, and then enters the titanium selection process of the beneficiation plant again to start beneficiation; S33: The coarse tailings from the gravity separation are recovered by at least one sweeping through a spiral chute to obtain gravity separation tailings; the TiO2 grade of the gravity separation tailings is lower than 2.00%.
6. The mineral recovery method of high-phosphorus vanadium-titanium magnetite tailings according to claim 1 or 5, characterized in that: The step S4 is also included: flotation desulfurization of the flotation raw material, which specifically includes the following steps: S41: Select the flotation raw material, add 600g / t of xanthate and 150g / t of frother and perform one rough selection, and the obtained minerals include floating phosphorus raw material and first sulfur ore; the S grade of the floating phosphorus raw material is 0.053%; S42: 600 g / t sulfuric acid is added to the first sulfur ore, and after a concentration, the obtained minerals include the second sulfur ore and the third sulfur ore; S43: After adding 300g / t sulfuric acid to the second sulfur ore and performing secondary concentration, the first intermediate ore obtained is returned to the primary concentration and the concentrate obtained is added with 200g / t sulfuric acid for tertiary concentration. The minerals obtained by the tertiary concentration include sulfur-cobalt concentrate and the second intermediate ore, and the second intermediate ore is returned to the secondary concentration; the S grade of the sulfur-cobalt concentrate is 30.79%; S44: 100 g / t sulfuric acid is added to the third sulfur ore and scavenged, and the obtained minerals are returned to the primary concentration and form floating sulfur tailings.
7. The mineral recovery method of high-phosphorus vanadium titanium magnetite tailings according to claim 6, characterized in that: After flotation desulfurization, the floating phosphorus raw material is subjected to flotation dephosphorization, and the flotation dephosphorization specifically comprises the following steps: S45: Select the floating phosphorus raw material for flotation dephosphorization test, add 200g / t collector and perform rough selection once, and the obtained minerals include the first phosphate ore and floating titanium raw material; the collector is a composite agent composed of oxidized paraffin soap and MES in a ratio of 9:1; the MES is sodium fatty acid methyl ester sulfonate; the TiO2 grade in the floating titanium raw material is 18.53%; S46: The first phosphate ore is concentrated and recovered at least once to obtain phosphorus-containing tailings; the recovered second phosphate ore is returned to S45 for rough selection again.
8. The mineral recovery method of high-phosphorus vanadium titanium magnetite tailings according to claim 7, characterized in that: After flotation dephosphorization, the titanium flotation raw material is subjected to flotation titanium ore, and the flotation titanium ore specifically comprises the following steps: S47: Selecting a floating titanium raw material for a flotation titanium selection test, adding 1500 g / t of sulfuric acid, 1000 g / t of a depressant, 2500 g / t of a collector and 300 g / t of diesel and performing a rough selection once, to obtain a first titanium concentrate and a first titanium tailings; 1200 g / t of sulfuric acid and 500 g / t of collector are added to the first titanium concentrate and subjected to primary concentration to obtain the second titanium concentrate and the first titanium middlings, and the first titanium middlings are returned to the roughing separation for further separation; After adding 800 g / t of sulfuric acid and 300 g / t of collector to the second titanium concentrate and performing secondary concentration, the third titanium concentrate and the second titanium middlings are obtained, and the second titanium middlings are returned to the primary concentration for further separation; 400 g / t of sulfuric acid and 200 g / t of collector are added to the third titanium concentrate and the concentrate is refined three times to obtain the fourth titanium concentrate and the third titanium middlings. The third titanium middlings are returned to the secondary refinement for further separation. After adding 400 g / t of sulfuric acid to the fourth titanium concentrate and performing the fourth concentration, titanium concentrate and the fourth titanium middlings are obtained, and the fourth titanium middlings are returned to the third concentration for further separation; After adding 300g / t of sulfuric acid and 200g / t of collector to the first titanium tailings and scavenging, the fifth titanium middlings and flotation tailings are obtained, and the fifth titanium middlings are returned to the roughing separation for further sorting; the TiO2 grade of the titanium concentrate reaches 47.50%; the TiO2 grade of the flotation tailings is lower than 2.50%.
Citation Information
Patent Citations
Separation method for roughing slime through teetered bed separator (TBS) and concentrating coarse slime difficult to separate through slime dense medium cyclone
CN105080701A
Method for extracting titanium and reducing impurities from vanadium titano-magnetite iron ore dressing tailings
CN112076891A
Process for recovering coarse slime in qualified medium
CN112156885A
Method for reducing ilmenite flotation difficulty in process of recovering ilmenite from iron dressing tailings
CN112791848A
Method for recovering ilmenite from iron tailings of vanadium-titanium magnetite containing olivine or pyroxene
CN112892854A
Cited By
Iron-titanium separation method for high-iron and high-titanium type vanadium titano-magnetite
CN119565759A