Method for impurity removal and quality improvement of ilmenite concentrate
By adjusting the pH value of the ilmenite concentrate and performing reverse flotation, the problem of high calcium and magnesium impurity content in the ilmenite concentrate was solved, and the calcium and magnesium impurities in the ilmenite concentrate were effectively reduced to meet the requirements of titanium chloride method. White quality requirements improve the sorting efficiency and product quality.
Patent Information
- Application Number
- CN202411132795.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-10-22
AI Technical Summary
The existing ilmenite concentrate has a high content of calcium and magnesium impurities, which cannot meet the quality requirements of ilmenite concentrate by the chloride method titanium dioxide, resulting in low separation efficiency and products that do not meet the requirements of high titanium slag.
A method of impurity removal and upgrading of ilmenite concentrate is adopted, which includes making ilmenite concentrate into slurry, adjusting its pH value to alkaline, stirring and solid-liquid separation, followed by reverse flotation, and using chemicals to coarse Select and sweep to reduce acid consumption and improve impurity removal efficiency.
It effectively reduces the content of calcium and magnesium impurities in the ilmenite concentrate, ensuring that the total content of CaO+MgO in the ilmenite concentrate is ≤5%, meeting the requirements of the boiling chlorination process for high titanium slag, and improving the separation efficiency and product quality.
Smart Images

Figure CN118807986A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of mineral impurity removal, and in particular to a method for removing impurities and improving the quality of ilmenite concentrate. Background Art
[0002] Among the existing titanium resources, most are low-grade symbiotic rock ores, and the associated minerals are mainly calcium-magnesium silicate minerals. The titanium concentrate obtained by sorting such ores usually has high CaO and MgO contents, which seriously restricts the preparation of chloride-rich titanium materials from such ilmenite concentrates. How to reduce the calcium and magnesium contents in ilmenite concentrates is a current research hotspot.
[0003] The sulfuric acid method and the chlorination method are the mainstream processes for the current production of titanium dioxide. Compared with the sulfuric acid method, the chlorination method has the advantages of short process, better environmental friendliness, high degree of equipment automation and good product quality. However, the chlorination method has strict requirements on the quality of ilmenite concentrate. In addition to improving the grade of TiO2 in the feed, it also requires low impurity content, especially requiring CaO to be less than 0.15% and MgO to be less than 1.5%. Although the traditional positive flotation process can obtain a higher-grade ilmenite concentrate, the floatability of the gangue minerals is close to that of ilmenite, resulting in a high content of calcium and magnesium impurities in the ilmenite concentrate, which cannot meet the raw material requirements of subsequent chlorination titanium dioxide.
[0004] In the process of ilmenite selection, a strong magnetic-flotation combined process is usually used. Olivine, amphibole and chlorite, the gangue minerals associated with ilmenite, have good floatability, and their floatability during flotation is equivalent to that of ilmenite. The gangue mineral inhibitors used in the current flotation process are not targeted, resulting in low selection efficiency, serious inclusion of gangue minerals, high calcium and magnesium content in titanium concentrate, and the sum of impurities CaO+MgO in the titanium slag obtained from titanium concentrate smelting ≥5%. The obtained product cannot meet the requirements of boiling chlorination process for high titanium slag. To this end, reducing the calcium and magnesium content in titanium concentrate will help improve the development of my country's chloride titanium dioxide and sponge titanium technology and the level of efficient and large-scale utilization of titanium resources. Therefore, how to reduce the content of calcium and magnesium impurities in ilmenite concentrate to meet the demand of chloride titanium dioxide for ilmenite concentrate and realize efficient and environmentally friendly utilization of titanium resources is an urgent problem to be solved. Summary of the invention
[0005] The purpose of this application is to provide a method for removing impurities and improving the quality of ilmenite concentrate to solve the above problems.
[0006] To achieve the above objectives, this application adopts the following technical solutions:
[0007] A method for removing impurities and improving the quality of ilmenite concentrate, comprising:
[0008] The ilmenite concentrate is made into ilmenite concentrate slurry, the pH value of the ilmenite concentrate slurry is adjusted to alkaline, and the solid-liquid separation and washing are carried out after stirring to obtain the dedoped ilmenite concentrate; the ilmenite concentrate is obtained from the ilmenite ore by positive flotation;
[0009] Mixing the dedoped ilmenite concentrate with water to obtain dedoped ilmenite concentrate slurry;
[0010] A reagent is added to the dedoped ilmenite concentrate slurry to carry out roughing by reverse flotation to obtain titanium concentrate.
[0011] Preferably, the concentration of the ilmenite concentrate slurry is 15wt% to 30wt%.
[0012] Preferably, the reagent used to adjust the pH value of the ilmenite concentrate slurry includes NaOH and Na2CO3;
[0013] The mass ratio of the NaOH to the Na2CO3 is 1 to 3:1;
[0014] The dosage of the agent used to adjust the pH value of the ilmenite concentrate slurry is 1000g to 2000g per ton of the ilmenite ore;
[0015] The pH value corresponding to the alkalinity is 9-11.
[0016] Preferably, the concentration of the dedoped ilmenite concentrate slurry is 25wt% to 40wt%.
[0017] Preferably, the reagents include a pH adjuster, a dispersant, an ilmenite inhibitor, and a gangue mineral collector.
[0018] Preferably, the pH adjuster comprises NaOH and / or Na2CO3;
[0019] The pH adjuster is used in an amount of 600 g to 1000 g per ton of the ilmenite ore.
[0020] Preferably, the dispersant includes at least one of sodium hexametaphosphate, sodium pyrophosphate, water glass and acidified water glass;
[0021] The dosage of the dispersant is 800 g to 1600 g per ton of the ilmenite ore.
[0022] Preferably, the ilmenite inhibitor comprises at least one of corn starch, phosphate starch, and sodium polyacrylate grafted starch;
[0023] The dosage of the ilmenite inhibitor is 1000 g to 1500 g per ton of the ilmenite ore.
[0024] Preferably, the gangue mineral collector comprises at least one of a primary amine compound, an ether amine compound and a quaternary ammonium salt compound;
[0025] The amount of the gangue mineral collector used is 200 g to 500 g per ton of the ilmenite ore.
[0026] Preferably, the roughing process of reverse flotation further includes scavenging process of reverse flotation;
[0027] The dosage of the reagent used in the reverse flotation sweep is halved.
[0028] Compared with the prior art, the beneficial effects of this application include:
[0029] (1) The method for removing impurities and improving the quality of ilmenite concentrate provided in the present application has a simple process flow. By adding reverse flotation, on the one hand, it solves the technical problem that the impurity content of calcium and magnesium in the ilmenite concentrate is high when only direct flotation is used, and it is difficult to meet the requirements of chloride titanium dioxide for ilmenite concentrate. On the other hand, it avoids the need to add a large amount of acid when only direct flotation is used, thereby significantly reducing acid consumption.
[0030] (2) By adding a de-agent process between forward flotation and reverse flotation, the mutual cancellation of the effects of forward flotation reagents and reverse flotation reagents can be avoided, thereby improving the efficiency of reverse flotation and promoting the effect of reverse flotation on impurity removal and quality improvement of ilmenite concentrate.
[0031] In summary, the present application solves the technical problems in the prior art of low separation efficiency of ilmenite concentrate, serious inclusion of gangue minerals, and high calcium and magnesium content in titanium concentrate, so that the sum of impurities CaO+MgO in the titanium slag obtained from the smelting of titanium concentrate is ≤5%, and the obtained product can meet the requirements of the boiling chlorination process for high titanium slag. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0033] Figure 1 The present invention is a schematic diagram of the process flow of the method for removing impurities and improving the quality of ilmenite concentrate by dedoping-reverse flotation provided in the embodiment. DETAILED DESCRIPTION
[0034] As used herein:
[0035] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0036] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0037] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0038] In these examples, parts and percentages are by mass unless otherwise indicated.
[0039] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0040] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0041] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0042] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows:
[0043] The ilmenite concentrate is made into pulp, the pH value of the ilmenite concentrate pulp is adjusted to alkaline, and after stirring, the solid-liquid separation and washing are carried out to obtain the de-doped ilmenite concentrate; the ilmenite concentrate is obtained by direct flotation of the ilmenite ore. The de-doped ilmenite concentrate is mixed with water to obtain the de-doped ilmenite concentrate pulp. A reagent is added to the de-doped ilmenite concentrate pulp for reverse flotation roughing to obtain the ilmenite concentrate.
[0044] In the ilmenite impurity removal and quality improvement method of the present application, the drug removal is first performed on the basis of the positive flotation. The drug removal can avoid the mutual cancellation of the effects between the positive flotation agent and the reverse flotation agent. After the drug removal process, the efficiency of the subsequent reverse flotation will be improved, thereby improving the impurity removal and quality improvement effect of the reverse flotation. In addition, reverse flotation can avoid the problem of incomplete separation on the one hand, and avoid adding a large amount of acid on the other hand. In this way, the acid consumption can be significantly reduced to ensure economy and environmental protection, and the corrosion of the acid to the equipment can be reduced, which is beneficial to equipment maintenance.
[0045] In an optional embodiment, the concentration of the ilmenite concentrate slurry is 15 wt% to 30 wt%, which is conducive to the full reaction of the residual reagent in the positive flotation between minerals during the de-drug process.
[0046] Optionally, the concentration of the ilmenite concentrate slurry can be 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt% or any value between 15wt% and 30wt%.
[0047] In an optional embodiment, the reagents used to adjust the pH value of the ilmenite concentrate slurry include NaOH and Na2CO3; the mass ratio of the NaOH to the Na2CO3 is 1 to 3:1, the pH value is adjusted to 9 to 11, and the amount of the reagent for adjusting the pH value of the ilmenite concentrate slurry is 1000g to 2000g per ton of the ilmenite ore.
[0048] Optionally, the mass ratio of the NaOH to the Na2CO3 can be 1:1, 2:1, 3:1 or any value between 1-3:1; the pH value can be adjusted to 9, 10, 11 or any value between 9 and 11; the dosage of the agent for adjusting the pH value of the ilmenite concentrate slurry can be 1000g per ton of the ilmenite ore, 1100g per ton of the ilmenite ore, 1200g per ton of the ilmenite ore, 1300g per ton of the ilmenite ore, 1400g per ton of the ilmenite ore, 1500g per ton of the ilmenite ore, 1600g per ton of the ilmenite ore, 1700g per ton of the ilmenite ore, 1800g per ton of the ilmenite ore, 1900g per ton of the ilmenite ore, 2000g per ton of the ilmenite ore or any value between 1000g and 2000g per ton of the ilmenite ore.
[0049] In an optional embodiment, the concentration of the dedoped ilmenite concentrate slurry is 25wt% to 40wt%, which is conducive to the contact and reaction of the reagent and the mineral during the reverse flotation process and can ensure sufficient contact between the reagent and the mineral.
[0050] Optionally, the concentration of the dedoped ilmenite concentrate slurry can be 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt% or any value between 25wt% and 40wt%.
[0051] In an optional embodiment, the reagents include a pH adjuster, a dispersant, an ilmenite inhibitor, and a gangue mineral collector.
[0052] In an optional embodiment, the pH adjuster includes NaOH and / or Na2CO3. The amount of the pH adjuster used is 600g to 1000g per ton of the ilmenite ore.
[0053] Optionally, the amount of the pH adjuster can be 600 g per ton of the ilmenite ore, 700 g per ton of the ilmenite ore, 800 g per ton of the ilmenite ore, 900 g per ton of the ilmenite ore, 1000 g per ton of the ilmenite ore, or any value between 600 g and 1000 g per ton of the ilmenite ore.
[0054] In an optional embodiment, the dispersant includes at least one of sodium hexametaphosphate, sodium pyrophosphate, water glass and acidified water glass. The amount of the dispersant is 800g to 1600g per ton of the ilmenite ore. After the dispersant is added, the electrostatic repulsion between particles can be utilized to significantly improve the dispersibility of the mineral, so that the mineral particles are evenly distributed in the flotation tank, and the particle agglomeration is avoided, thereby improving the efficiency of reverse flotation.
[0055] Optionally, the amount of the dispersant used can be 800g per ton of the ilmenite ore, 900g per ton of the ilmenite ore, 1000g per ton of the ilmenite ore, 1100g per ton of the ilmenite ore, 1200g per ton of the ilmenite ore, 1300g per ton of the ilmenite ore, 1400g per ton of the ilmenite ore, 1500g per ton of the ilmenite ore, 1600g per ton of the ilmenite ore or any value between 800g and 1600g per ton of the ilmenite ore.
[0056] In an optional embodiment, the ilmenite inhibitor includes at least one of corn starch, phosphate starch, and sodium polyacrylate grafted starch. The dosage of the ilmenite inhibitor is 1000 g to 1500 g per ton of the ilmenite ore. The ilmenite inhibitor can be selectively adsorbed on the surface of the ilmenite concentrate during the reverse flotation process, thereby inhibiting the flotation of the ilmenite concentrate, so that the ilmenite can be effectively separated from the gangue minerals during the reverse flotation process. And under the synergistic effect with the dispersant, the inhibitor will be more selective for ilmenite.
[0057] Optionally, the dosage of the ilmenite inhibitor can be 1000g per ton of the ilmenite ore, 1100g per ton of the ilmenite ore, 1200g per ton of the ilmenite ore, 1300g per ton of the ilmenite ore, 1400g per ton of the ilmenite ore, 1500g per ton of the ilmenite ore or any value between 1000g and 1500g per ton of the ilmenite ore.
[0058] In an optional embodiment, the gangue mineral collector includes at least one of a primary amine compound, an ether amine compound and a quaternary ammonium salt compound. The gangue mineral inhibitor is used in an amount of 200 g to 500 g per ton of the ilmenite ore. The gangue mineral collector can be specifically adsorbed on the surface of the gangue mineral, causing changes in its surface properties, thereby enhancing the floatability of the gangue mineral and more effectively separating the ilmenite concentrate from the gangue mineral. In addition, in combination with a dispersant, the gangue mineral collector will be more selective for the gangue mineral.
[0059] In an optional embodiment, the reverse flotation comprises roughing and scavenging performed sequentially, and the dosage of the reagent is halved during the scavenging.
[0060] Example 1
[0061] A method for removing impurities and improving the quality of ilmenite concentrate, using a ilmenite concentrate from Panxi (the ilmenite concentrate is obtained from ilmenite ore after positive flotation), with a TiO2 grade of 46.86%, a CaO+MgO content of 5.0% to 6.0%, and gangue minerals mainly feldspar, chlorite, and forsterite. The residual reagent after positive flotation is mainly sodium oleate, and the residual amount is 1000 to 1500g per ton of ilmenite ore. Figure 1 As shown, water is added to the ilmenite concentrate to adjust the concentration to about 20wt%, 1800g of a mixture of NaOH and Na2CO3 is added per ton of ilmenite ore, and the mixture is stirred for 20 minutes to strengthen the dedoping process. After the stirring, the slurry is filtered to obtain the dedoped ilmenite concentrate; clean water is added to the dedoped ilmenite concentrate to ensure that the slurry concentration is 33wt%, 700g of the pH adjuster NaOH is added per ton of ilmenite ore, and the slurry is stirred for 2 minutes; 1200g of sodium pyrophosphate dispersant is added per ton of ilmenite ore, and the slurry is stirred for 2 minutes; 1000g of the inhibitor phosphate starch (purchased from Nantong Gaofeng Biotechnology Co., Ltd., product model: GF-A101) is added per ton of ilmenite ore, and the slurry is stirred for 2 minutes; 300g of the collector dodecylamine acetate is added per ton of ilmenite ore, and the slurry is stirred for 3 minutes, and a roughing operation is carried out, and the amount of reagents used in the scavenging operation is halved, and the gangue minerals are removed by reverse flotation, and the bottom product of the tank is a high-quality ilmenite concentrate. The grade of TiO2 in high-quality titanium concentrate is 50.07%, of which the grade of CaO is 0.13% and the grade of MgO is 1.34%.
[0062] Example 2
[0063] A method for removing impurities and improving the quality of ilmenite concentrate, using a ilmenite concentrate from Hebei (the ilmenite concentrate is obtained from ilmenite ore after positive flotation), the grade of TiO2 is 45.31%, the grade of CaO is 1.30%, the grade of MgO is 4.23%, the gangue minerals are mainly calcite, chlorite, and amphibole, and the residual reagent after positive flotation is mainly sodium oleate, and the residual amount is 800g to 1300g per ton of ilmenite ore. Figure 1As shown, water is added to the ilmenite concentrate to adjust the concentration to about 15wt%, 1400g of a mixture of NaOH and Na2CO3 is added per ton of ilmenite ore, and the mixture is stirred for 25 minutes to strengthen the dedoping process. After the stirring, the slurry is filtered to obtain the dedoped titanium concentrate; clean water is added to the dedoped titanium concentrate to ensure that the slurry concentration is 28wt%, 800g of a pH adjuster NaOH is added per ton of ilmenite ore, and the slurry is stirred for 2 minutes; 1200g of a dispersant water glass is added per ton of ilmenite ore, and the slurry is stirred for 2 minutes; 1400g of an inhibitor of corn starch is added per ton of ilmenite ore, and the slurry is stirred for 2 minutes; 200g of a collector hexadecyltrimethylammonium chloride is added per ton of ilmenite ore, and the slurry is stirred for 3 minutes, and a roughing operation is carried out, and the amount of reagents used in the scavenging operation is halved, and the gangue minerals are removed by reverse flotation, and the bottom product of the tank is a high-quality titanium concentrate. The grade of TiO2 in high-quality titanium concentrate is 48.52%, of which the grade of CaO is 0.11% and the grade of MgO is 1.29%.
[0064] Example 3
[0065] A method for removing impurities and improving the quality of ilmenite concentrate, using a ilmenite concentrate from Shaanxi (the ilmenite concentrate is obtained from ilmenite ore after positive flotation), the grade of TiO2 is 46.14%, the grade of CaO is 0.79%, the grade of MgO is 4.48%, the gangue minerals are mainly amphibole, pyroxene, plagioclase, chlorite and mica, and the residual reagent after positive flotation is mainly sodium oleate, and the residual amount is 700g to 1200g per ton of ilmenite ore. Figure 1 As shown, water is added to the ilmenite concentrate to adjust the concentration to about 25wt%, 1000g of a mixture of NaOH and Na2CO3 is added per ton of ilmenite ore, and the mixture is stirred for 20 minutes to strengthen the dedoping process. After the stirring, the slurry is filtered to obtain the dedoped ilmenite concentrate; clean water is added to the dedoped ilmenite concentrate to ensure that the slurry concentration is 33wt%, 900g of the pH adjuster NaOH is added per ton of ilmenite ore, and the slurry is stirred for 2 minutes; 800g of sodium hexametaphosphate as a dispersant is added per ton of ilmenite ore, and the slurry is stirred for 2 minutes; 800g of the inhibitor sodium polyacrylate grafted starch (purchased from Guangzhou Baiyu Biotechnology Co., Ltd.) is added per ton of ilmenite ore, and the slurry is stirred for 2 minutes; 250g of the collector decyl ether amine acetate is added per ton of ilmenite ore, and the slurry is stirred for 3 minutes, and a roughing operation is carried out, and the amount of reagents used in the scavenging operation is halved, and the gangue minerals are removed by reverse flotation, and the bottom product of the tank is a high-quality ilmenite concentrate. The grade of TiO2 in high-quality titanium concentrate is 49.17%, of which the grade of CaO is 0.12% and the grade of MgO is 1.16%.
[0066] Comparative Example 1
[0067] A method for removing impurities and upgrading the quality of ilmenite concentrate by removing drugs and reverse flotation. The ilmenite concentrate feeding and reverse flotation process are the same as those in Example 1, except that no removal of drugs is performed in the test. As a result, the grade of the titanium concentrate finally obtained is 47.59%, wherein the grade of CaO is 1.21%, and the grade of MgO is 2.34%. The impurity content of calcium and magnesium in the ilmenite exceeds the standard and does not meet the raw material requirements of the titanium dioxide chloride process.
[0068] Comparative Example 2
[0069] A method for removing impurities and improving the quality of ilmenite concentrate by drug removal and reverse flotation. The ilmenite concentrate feeding and method process are the same as those in Example 1, except that the dispersant sodium pyrophosphate is not added in the reverse flotation operation. As a result, the grade of the titanium concentrate finally obtained is 48.07%, of which the grade of CaO is 0.92% and the grade of MgO is 1.71%. The impurity content of calcium and magnesium in the ilmenite exceeds the standard and does not meet the raw material requirements of the titanium dioxide chloride process.
[0070] Comparative Example 3
[0071] A method for removing impurities and improving the quality of ilmenite concentrate by drug removal and reverse flotation. The ilmenite concentrate feeding and reverse flotation process are the same as those in Example 2, except that no drug removal operation is performed in the test. As a result, the grade of the titanium concentrate finally obtained is 46.16%, wherein the grade of CaO is 1.17%, and the grade of MgO is 2.29%. The impurity content of calcium and magnesium in the ilmenite exceeds the standard and does not meet the raw material requirements of the titanium dioxide chloride process.
[0072] Comparative Example 4
[0073] A method for removing drugs from ilmenite concentrate and improving its quality by reverse flotation. The ilmenite concentrate feeding and the method process are the same as those in Example 2, except that no dispersant water glass is added in the reverse flotation operation. As a result, the grade of the titanium concentrate finally obtained is 47.57%, wherein the grade of CaO is 0.79% and the grade of MgO is 1.92%. The impurity content of calcium and magnesium in the ilmenite exceeds the standard and does not meet the raw material requirements of the titanium dioxide chloride process.
[0074] Comparative Example 5
[0075] A method for removing impurities and improving the quality of ilmenite concentrate by drug removal and reverse flotation. The ilmenite concentrate feeding and reverse flotation process are the same as those in Example 3, except that no drug removal operation is performed in the test. As a result, the grade of the titanium concentrate finally obtained is 47.23%, wherein the grade of CaO is 0.66%, and the grade of MgO is 1.79%. The impurity content of calcium and magnesium in the ilmenite exceeds the standard and does not meet the raw material requirements of the titanium dioxide chloride process.
[0076] Comparative Example 6
[0077] A method for removing impurities and improving the quality of ilmenite concentrate by drug removal and reverse flotation. The ilmenite concentrate feeding and method process are the same as those in Example 3, except that the dispersant sodium hexametaphosphate is not added in the reverse flotation operation. As a result, the grade of the titanium concentrate finally obtained is 48.61%, wherein the grade of CaO is 0.52%, and the grade of MgO is 1.54%. The impurity content of calcium and magnesium in the ilmenite exceeds the standard and does not meet the raw material requirements of the titanium dioxide chloride process.
[0078] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0079] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for removing impurities and improving the quality of ilmenite concentrate, It is characterized in that include: The ilmenite concentrate is made into ilmenite concentrate slurry, the pH value of the ilmenite concentrate slurry is adjusted to alkaline, and the solid-liquid separation and washing are carried out after stirring to obtain the dedoped ilmenite concentrate; the ilmenite concentrate is obtained from the ilmenite ore by positive flotation; Mixing the dedoped ilmenite concentrate with water to obtain dedoped ilmenite concentrate slurry; A reagent is added to the dedoped ilmenite concentrate slurry to carry out roughing by reverse flotation to obtain titanium concentrate.
2. The method for removing impurities and improving the quality of ilmenite concentrate according to claim 1, It is characterized in that The concentration of the ilmenite concentrate slurry is 15wt% to 30wt%.
3. The method for removing impurities and improving the quality of ilmenite concentrate according to claim 1, It is characterized in that The reagents used to adjust the pH value of the ilmenite concentrate slurry include NaOH and Na 2 CO 3 ; The NaOH and the Na 2 CO 3 The mass ratio is 1 to 3:1; The dosage of the agent used to adjust the pH value of the ilmenite concentrate slurry is 1000 g to 2000 g per ton of the ilmenite ore; The pH value corresponding to the alkalinity is 9-11.
4. The method for removing impurities and improving the quality of ilmenite concentrate according to claim 1, It is characterized in that The concentration of the dedoped ilmenite concentrate slurry is 25wt% to 40wt%.
5. The method for removing impurities and improving the quality of ilmenite concentrate according to claim 1, It is characterized in that The reagents include a pH adjuster, a dispersant, an ilmenite inhibitor, and a gangue mineral collector.
6. The method for removing impurities and improving the quality of ilmenite concentrate according to claim 5, It is characterized in that The pH adjuster includes NaOH and / or Na 2 CO 3 ; The pH adjuster is used in an amount of 600 g to 1000 g per ton of the ilmenite ore.
7. The method for removing impurities and improving the quality of ilmenite concentrate according to claim 5, It is characterized in that The dispersant includes at least one of sodium hexametaphosphate, sodium pyrophosphate, water glass and acidified water glass; The dosage of the dispersant is 800 g to 1600 g per ton of the ilmenite ore.
8. The method for removing impurities and improving the quality of ilmenite concentrate according to claim 5, It is characterized in that The ilmenite inhibitor comprises at least one of corn starch, phosphate starch, and sodium polyacrylate grafted starch; The dosage of the ilmenite inhibitor is 1000 g to 1500 g per ton of the ilmenite ore.
9. The method for removing impurities and improving the quality of ilmenite concentrate according to claim 5, It is characterized in that The gangue mineral collector comprises at least one of a primary amine compound, an ether amine compound and a quaternary ammonium salt compound; The amount of the gangue mineral collector used is 200 g to 500 g per ton of the ilmenite ore.
10. The method for removing impurities and improving the quality of ilmenite concentrate according to any one of claims 1 to 9, It is characterized in that The roughing process of reverse flotation also includes scavenging process of reverse flotation; The dosage of the reagent used in the reverse flotation sweep is halved.
Citation Information
Patent Citations
Olivine pyroxenite type ilmenite step-by-step flotation method
CN108927293A
Acid pretreatment-flotation separation method of olivine pyroxenite ilmenite
CN111744677A
Tungsten ore and rutile flotation co-enrichment method
CN117414940A
Flotation process for reinforced recovery of ilmenite and reagent system thereof
CN117563785A