White graphene modified high-performance aluminum foil as well as preparation method and application thereof

By using white graphene-doped water-based epoxy resin solution and acrylic resin solution to form a coating on the surface of the aluminum foil, the problem of performance degradation caused by the easy oxidation of the aluminum foil is solved, achieving high anti-corrosion, thermal conductivity and hydrophilicity, and extending the service life. longevity and optimized heat exchange efficiency.

CN118808094APending Publication Date: 2024-10-22ZHENJIANG JINTIANCHEN NEW MATERIAL +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410797262.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Aluminum foil is easily oxidized to form an oxide film during use, resulting in reduced anti-corrosion and thermal conductivity. Existing coating materials cannot meet the requirements for anti-corrosion, thermal conductivity and oxidation resistance at the same time.

Method used

A white graphene-doped water-based epoxy resin solution is used as the anti-corrosion thermal conductive layer, and an acrylic resin solution is used as the hydrophilic layer. A coating with high anti-corrosion, high thermal conductivity and hydrophilicity is formed on the surface of the aluminum foil by roller coating. .

Benefits of technology

It improves the anti-corrosion, thermal conductivity and anti-oxidation capabilities of the aluminum foil, reduces the condensation phenomenon of condensed water, increases the heat exchange area, accelerates the refrigeration rate, extends the service life and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808094A_ABST
    Figure CN118808094A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of corrosion prevention of aluminum foils, and particularly relates to a white graphene modified high-performance aluminum foil and a preparation method and application thereof. The anti-corrosion heat-conducting coating is prepared through white graphene modification, and the high-performance aluminum foil is prepared through simple coating in combination with the hydrophilic coating; as the white graphene doped epoxy resin solution is added as the prime coat paint, the corrosion resistance, heat conduction performance and oxidation resistance of the aluminum foil can be improved, the service life of the aluminum foil can be prolonged, the acrylic resin solution is adopted as the hydrophilic layer paint, the hydrophilic layer can reduce the condensation phenomenon of condensate water, increase the heat exchange area, accelerate the refrigeration rate and the like, and the service life of the aluminum foil is prolonged. And reduction of energy consumption is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of corrosion protection of aluminum foil, and specifically relates to a white graphene-modified high-performance aluminum foil and a preparation method and application thereof. Background Art

[0002] Aluminum foil is a metal with good ductility and thermal conductivity, and is often used to manufacture heat exchangers for air conditioners. However, during the use of aluminum foil, the aluminum foil itself is easily oxidized to form an oxide film, which reduces its anti-corrosion and thermal conductivity. The existing method is to use some materials to coat the aluminum foil. Commonly used coatings generally include anti-corrosion layer materials and hydrophilic layer materials. However, the current materials cannot simultaneously meet the current requirements of aluminum foil in terms of anti-corrosion, thermal conductivity, and antioxidant capacity.

[0003] Epoxy resin coatings are a water-based coating with extremely high adhesion, relatively high safety and certain corrosion resistance. They are widely used in daily life. However, pure epoxy resin coatings have poor hydrophilicity, electrical conductivity and thermal conductivity. Thermal conductive fillers (such as metals, carbon materials, etc.) are usually added to improve their electrical and thermal conductivity.

[0004] Boron nitride (BN) is a boron-nitrogen polymer compound composed of boron and nitrogen atoms in an orderly manner and with crystalline properties. It has high chemical stability, high heat resistance and high thermal conductivity, and is commonly known as white graphene. If the surface of aluminum foil can be modified by using white graphene doped with epoxy resin solution material to form an anti-corrosion and thermal conductive coating, and acrylic resin solution is used as a hydrophilic layer coating, it will be able to solve technical problems such as improving the service life and performance of aluminum foil, reducing the condensation of condensed water, increasing the heat exchange area, and accelerating the refrigeration rate. Summary of the invention

[0005] The purpose of the present invention is to solve some problems existing in the prior art, and to provide a high-performance aluminum foil modified with white graphene (BN), and a preparation method and application thereof, wherein the aluminum foil has high corrosion resistance, high thermal conductivity and hydrophilicity, so as to solve the problems that the aluminum foil itself is easily oxidized to form an oxide film during use, which reduces its corrosion resistance and thermal conductivity, and condenses water during use of the air-conditioning aluminum foil.

[0006] In order to achieve the above technical purpose, the technical solution adopted by the present invention is as follows:

[0007] The present invention first provides a high-performance aluminum foil modified with white graphene (BN), wherein the aluminum foil has high corrosion resistance, high thermal conductivity and hydrophilicity, and the aluminum foil is coated with an anti-corrosion thermal conductive layer, and the anti-corrosion thermal conductive layer is coated with a hydrophilic layer.

[0008] The present invention also provides a method for preparing the white graphene (BN) modified high-performance aluminum foil, which includes preparing an aluminum foil anti-corrosion heat-conducting layer and a hydrophilic layer:

[0009] Preparation of anti-corrosion thermal conductive layer: First, wipe the clean surface of the aluminum foil with water and ethanol, use the white graphene-doped water-based epoxy resin solution as the anti-corrosion thermal conductive layer coating, and adjust its performance by controlling the different doping amounts of white graphene. Use roller coating to apply on the aluminum foil, place it on a heating table for heating and curing, remove it and cool it to room temperature for use, and obtain the anti-corrosion thermal conductive layer.

[0010] Wherein, the mass fraction of white graphene in the white graphene-doped aqueous epoxy resin solution is 0.5%-5%.

[0011] The aqueous epoxy resin solution used in the present invention comprises epoxy-modified acrylic resin, curing agent, water and ethylene glycol butyl ether, wherein the mass fraction of the epoxy acrylic resin is 10-50%, the curing agent is isocyanate, the content of which is 3-15% (mass fraction wt%), the content of water is 20-95%, and the content of ethylene glycol butyl ether is 1%-20%.

[0012] Furthermore, the content of epoxy-modified acrylic resin and curing agent in the aqueous epoxy resin solution is 24-28%, the content of water is 66-72%, and the content of ethylene glycol butyl ether is 4-6%.

[0013] Wherein, the curing temperature is 100-300° C., and the curing time is 1-30 min.

[0014] Preparation of the hydrophilic layer: Use acrylic resin solution as the hydrophilic layer coating, use a roller to apply the aluminum foil, apply the hydrophilic layer coating on the anti-corrosion thermal conductive layer in step (1), place it on a heating table to heat and cure, and remove it to cool to room temperature.

[0015] The acrylic resin solution used contains 5%-40% acrylic resin, 1%-20% ethylene glycol butyl ether and 70%-90% water in mass fraction.

[0016] Furthermore, the acrylic resin solution contains 10%-15% by mass of acrylic resin, 3%-4% by mass of ethylene glycol butyl ether, and 80%-85% by mass of water.

[0017] Wherein, the curing temperature is 100-300° C., and the curing time is 1-30 min.

[0018] Further preferably, the solid content of the waterborne epoxy resin solution of the present invention is 24 wt %, and the solid content of the acrylic resin solution is 11 wt %.

[0019] Beneficial effects of the present invention:

[0020] Compared with the common anti-corrosion layer treatment, the present invention utilizes the high thermal conductivity of white graphene and combines the characteristics of the water-based epoxy resin solution to form a unique anti-corrosion and thermal conductive layer. Due to the addition of boron nitride (white graphene), the anti-corrosion, thermal conductivity and antioxidant capacity of the aluminum foil, as well as the service life, can be improved. The acrylic resin solution is used as the hydrophilic layer coating, and the hydrophilic layer can reduce the condensation of condensed water, increase the heat exchange area, accelerate the refrigeration rate, etc., which helps to reduce energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The SEM images of the monomer white graphene used in the embodiments of the present invention and the aqueous epoxy resin solution doped with white graphene in Embodiment 1 and Embodiment 2 are shown in FIG.

[0022] Figure 2 The hydrophilic performance diagram of the aluminum foil samples prepared in Examples 1-3 of the present invention and commercial aluminum foil.

[0023] Figure 3 These are corrosion test diagrams of the aluminum foil samples prepared in Examples 2-3 of the present invention and commercial aluminum foil. DETAILED DESCRIPTION

[0024] To help those skilled in the art better understand the technical solution of the present invention, preferred embodiments are described in detail below, but the following embodiments are not limited to the protection scope of the present invention.

[0025] The contents not described in detail in the examples are usually completed according to conventional experimental methods, and the processes involved can also be understood and simply implemented by technicians in the field according to product specifications or basic knowledge. Obviously, the examples only represent some applications of the present invention, not all.

[0026] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative work shall fall within the scope of protection of the present invention.

[0027] The aqueous epoxy resin solution used in the present invention comprises epoxy-modified acrylic resin, curing agent, water and ethylene glycol butyl ether, wherein the mass fraction of the epoxy acrylic resin is 10-50%, the curing agent is isocyanate, the content of which is 3-15% (mass fraction wt%), the content of water is 20-95%, and the content of ethylene glycol butyl ether is 1%-20%.

[0028] Furthermore, the aqueous epoxy resin solution contains 24-28% of epoxy-modified acrylic resin and curing agent, 66-72% of water, and 4-6% of ethylene glycol butyl ether.

[0029] The acrylic resin solution used contains 5%-40% acrylic resin, 1%-20% ethylene glycol butyl ether and 70%-90% water in mass fraction.

[0030] Furthermore, the acrylic resin solution contains 10%-15% by mass of acrylic resin, 3%-4% by mass of ethylene glycol butyl ether, and 80%-85% by mass of water.

[0031] The above two materials can be purchased from conventional markets.

[0032] In the embodiment of the present invention, an aqueous epoxy resin solution with a solid content of 24 wt % and an acrylic resin solution with a solid content of 11 wt % are selected as examples.

[0033] Embodiment 1:

[0034] Firstly, a white graphene-doped aqueous epoxy resin solution is prepared, wherein the mass fraction of the white graphene is 0.5%.

[0035] Then, a 0.5% white graphene-doped aqueous epoxy resin solution was used as an anti-corrosion thermal conductive layer coating. First, the surface of the aluminum foil was cleaned with water and ethanol, and the primer coating was applied to the surface of the aluminum foil using an 8μm roller. The aluminum foil with the primer was placed on a 200°C heating table for curing for 3 minutes, then removed and cooled to room temperature for use.

[0036] Use an 8μm roller to coat the aluminum foil, apply the acrylic resin solution hydrophilic layer coating on the above-mentioned anti-corrosion thermal conductive layer material, place it on a heating table and heat and cure it at 200°C for 3 minutes, then remove it and cool it to room temperature to obtain white graphene (BN) modified high-performance aluminum foil.

[0037] Embodiment 2:

[0038] Firstly, a white graphene-doped aqueous epoxy resin solution is prepared, wherein the mass fraction of the white graphene is 1%.

[0039] A 1% white graphene-doped aqueous epoxy resin solution was used as the anti-corrosion thermal conductive layer coating. First, the surface of the aluminum foil was cleaned with water and ethanol, and the primer coating was applied to the surface of the aluminum foil using an 8μm roller. The aluminum foil with the primer was placed on a 200°C heating table for curing for 3 minutes, then removed and cooled to room temperature for use.

[0040] Use an 8μm roller to coat the aluminum foil, apply the acrylic resin solution hydrophilic layer coating on the anti-corrosion thermal conductive layer material obtained above, place it on a heating table and heat and cure it at 200°C for 3 minutes, then remove it and cool it to room temperature to obtain white graphene (BN) modified high-performance aluminum foil.

[0041] Embodiment 3:

[0042] Firstly, a white graphene-doped aqueous epoxy resin solution is prepared, wherein the mass fraction of the white graphene is 2%.

[0043] A 2% white graphene-doped aqueous epoxy resin solution was used as the anti-corrosion thermal conductive layer coating. First, the surface of the aluminum foil was cleaned with water and ethanol, and the primer coating was applied to the surface of the aluminum foil using an 8μm roller. The aluminum foil with the primer was placed on a 200°C heating table for curing for 3 minutes, then removed and cooled to room temperature for use.

[0044] Use an 8μm roller to coat the aluminum foil, apply the acrylic resin solution hydrophilic layer coating on the anti-corrosion thermal conductive layer material obtained above, place it on a heating table and heat and cure it at 200°C for 3 minutes, then remove it and cool it to room temperature to obtain a high-performance aluminum foil modified with white graphene (BN).

[0045] Embodiment 4:

[0046] Firstly, a white graphene-doped aqueous epoxy resin solution is prepared, wherein the mass fraction of the white graphene is 1%.

[0047] A 1% white graphene-doped aqueous epoxy resin solution was used as the anti-corrosion thermal conductive layer coating. First, the surface of the aluminum foil was cleaned with water and ethanol, and the primer coating was applied to the surface of the aluminum foil using an 8μm roller. The aluminum foil with the primer was placed on a 100°C heating table for curing for 30 minutes, then removed and cooled to room temperature for use.

[0048] Use an 8μm roller to coat the aluminum foil, apply the acrylic resin solution hydrophilic layer coating on the anti-corrosion thermal conductive layer material obtained above, place it on a heating table and heat and cure it at 100°C for 30 minutes, remove it and cool it to room temperature to obtain a high-performance aluminum foil modified with white graphene (BN).

[0049] Embodiment 5:

[0050] Firstly, a white graphene-doped aqueous epoxy resin solution is prepared, wherein the mass fraction of the white graphene is 1%.

[0051] A 1% white graphene-doped aqueous epoxy resin solution was used as the anti-corrosion thermal conductive layer coating. First, the surface of the aluminum foil was cleaned with water and ethanol, and the primer coating was applied to the surface of the aluminum foil using an 8μm roller. The aluminum foil with the primer was placed on a 300°C heating table for curing for 1 minute, then removed and cooled to room temperature for use.

[0052] Use an 8μm roller to coat the aluminum foil, apply the acrylic resin solution hydrophilic layer coating on the anti-corrosion thermal conductive layer material obtained above, place it on a heating table and heat and cure it at 300°C for 1 minute, remove it and cool it to room temperature to obtain a high-performance aluminum foil modified with white graphene (BN).

[0053] Embodiment 6:

[0054] Firstly, a white graphene-doped aqueous epoxy resin solution is prepared, wherein the mass fraction of the white graphene is 5%.

[0055] Then, a 5% white graphene-doped aqueous epoxy resin solution was used as an anti-corrosion thermal conductive layer coating. First, the surface of the aluminum foil was cleaned with water and ethanol, and the primer coating was applied to the surface of the aluminum foil using an 8μm roller. The aluminum foil with the primer was placed on a 200°C heating table for curing for 3 minutes, then removed and cooled to room temperature for use.

[0056] Use an 8μm roller to coat the aluminum foil, apply the acrylic resin solution hydrophilic layer coating on the above-mentioned anti-corrosion thermal conductive layer material, place it on a heating table and heat and cure it at 200°C for 3 minutes, then remove it and cool it to room temperature to obtain white graphene (BN) modified high-performance aluminum foil.

[0057] Comparative Example 1:

[0058] A water-based epoxy resin solution without white graphene doping was used as the anti-corrosion thermal conductive layer coating. First, the surface of the aluminum foil was cleaned with water and ethanol, and the primer coating was applied to the surface of the aluminum foil using an 8μm roller. The aluminum foil with the primer was placed on a 200°C heating table for curing for 3 minutes, then removed and cooled to room temperature for use.

[0059] Use an 8μm roller to coat the aluminum foil, apply the acrylic resin solution hydrophilic layer coating on the anti-corrosion thermal conductive layer material obtained above, place it on a heating table and heat and cure it at 200°C for 3 minutes, then remove it and cool it to room temperature to obtain a comparison aluminum foil that has not been modified with white graphene (BN).

[0060] In the present invention, a contact angle tester, a self-prepared corrosion solution (a mixture of 70 mL H2O+20 gCuSO4+10 mL concentrated HCl), a laser thermal conductivity meter, and a differential scanner are used to conduct a comparative experiment on the hydrophilicity, corrosion resistance, and thermal conductivity of the prepared high-performance (corrosion-resistant, thermally conductive, and hydrophilic) aluminum foil and commercial aluminum foil (conventionally commercially available).

[0061] Figure 1 The SEM images of the white graphene monomer used in the embodiments of the present invention, the aqueous epoxy resin solution doped with 0.5% white graphene in Example 1, and the aqueous epoxy resin solution doped with 1% white graphene in Example 2, Figure 1 It can be clearly seen that the white graphene monomer is a regular nanosheet structure. The SEM images of the materials in Examples 1 and 2 do not show the white graphene structure clearly, indicating that the white graphene is uniformly doped in the aqueous epoxy resin solution.

[0062] Figure 2 The hydrophilic properties of the aluminum foil samples prepared in Examples 1-3 of the present invention and commercial aluminum foil are shown in FIG. 1 . The results show that the hydrophilicity of the aluminum foil prepared by the present invention is almost the same as that of the commercial aluminum foil.

[0063] Figure 3 The corrosion test diagram of the aluminum foil sample prepared in Example 2-3 of the present invention and the commercial aluminum foil, wherein the interval time is 30 minutes. The results show that the aluminum foil prepared in the present invention has better corrosion resistance than the blank commercial aluminum foil.

[0064] Table 1 shows the thermal conductivity data of the aluminum foil samples prepared in Examples 1-2 of the present invention, the samples prepared in Comparative Example 1, and commercial aluminum foil. It can be clearly seen from the figure that the addition of epoxy resin causes a sharp decrease in thermal conductivity and heat transfer data, which is attributed to the poor thermal conductivity of the epoxy resin itself. After being doped with white graphene, its performance is similar to that of commercial aluminum foil without any treatment, which is attributed to the high thermal conductivity of white graphene.

[0065] Table 1. Thermal conductivity data of the aluminum foil samples prepared by the present invention and commercial aluminum foil

[0066]

[0067] Note: The above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention; therefore, although this specification has described the present invention in detail with reference to the above embodiments, a person skilled in the art should understand that the present invention can still be modified or replaced by equivalents; and all technical solutions and improvements thereof that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a high-performance aluminum foil modified with white graphene, characterized in that: The method comprises the following steps: Preparation of anti-corrosion thermal conductive layer: Wipe the clean aluminum foil surface with water and ethanol, use the white graphene-doped water-based epoxy resin solution as the anti-corrosion thermal conductive layer coating, apply it to the aluminum foil, place it on a heating table for heating and curing, remove it and cool it to room temperature for use. Preparation of the hydrophilic layer: Use acrylic resin solution as the hydrophilic layer coating, apply aluminum foil, apply the hydrophilic layer coating on the anti-corrosion thermal conductive layer, place it on a heating table for heating and curing, and remove it to cool to room temperature.

2. The preparation method according to claim 1, characterized in that: The mass fraction of white graphene in the white graphene-doped aqueous epoxy resin solution is 0.5%-5%.

3. The preparation method according to claim 1, characterized in that: The aqueous epoxy resin solution comprises epoxy acrylic resin, curing agent, water and ethylene glycol butyl ether, wherein the mass fraction of epoxy acrylic resin is 10-50%, the curing agent is isocyanate with a content of 3-15%, the content of water is 20-95%, and the content of ethylene glycol butyl ether is 1%-20%.

4. The preparation method according to claim 1, characterized in that: The content of epoxy-modified acrylic resin and curing agent in the waterborne epoxy resin solution is 24-28%, the content of water is 66-72%, and the content of ethylene glycol butyl ether is 4-6%.

5. The preparation method according to claim 1, characterized in that: The curing temperature is 100-300° C., and the curing time is 1-30 minutes.

6. The preparation method according to claim 1, characterized in that: The acrylic resin solution contains 5%-40% acrylic resin, 1%-20% ethylene glycol butyl ether and 70%-90% water in mass fractions.

7. The preparation method according to claim 1, characterized in that: The acrylic resin solution contains 10%-15% acrylic resin, 3%-4% ethylene glycol butyl ether and 80%-85% water in mass fractions.

8. The preparation method according to claim 1, characterized in that: The curing temperature is 100-300° C., and the curing time is 1-30 minutes.

9. The high-performance aluminum foil modified with white graphene prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The aluminum foil has high corrosion resistance, high thermal conductivity and hydrophilicity. The aluminum foil is coated with an anti-corrosion thermal conductive layer, and the anti-corrosion thermal conductive layer is coated with a hydrophilic layer.

Citation Information

Patent Citations

  • High-corrosion-resistance high-thermal-conductivity composite aluminum foil and production method thereof

    CN109926294A

  • Heat-dissipation coating for lampshade and using method of coating

    CN110003770A