Hot drawing processing technology of pure titanium TA4 electronic product part

Through combined cold and hot drawing processing and the use of a special lubricating layer, the problems of poor plasticity and poor bending performance of titanium alloy parts have been solved, an efficient and low-cost production process has been achieved, and pure titanium TA4 electronic product parts have been improved processing performance and production efficiency.

CN118808358APending Publication Date: 2024-10-22ZHONGSHAN (CHANGZHOU) NEW MATERIAL CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411008984.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the existing technology, the processing technology of pure titanium TA4 electronic product parts has the problems of high strength but poor plasticity and poor bending performance, and is not suitable for mass production, resulting in low production efficiency and high cost.

Method used

Using a combined cold and hot drawing processing method combined with a special lubrication layer, the plasticity and bending properties of the titanium alloy are improved through wall reduction cold drawing and hot drawing, reducing the number of processing passes, reducing production costs, and through special lubrication The layer reduces friction loss and scratches and improves the yield rate.

Benefits of technology

It improves the plasticity and bending properties of pure titanium TA4 material, reduces processing passes and production costs, improves production efficiency, reduces the problem of low yield, and achieves efficient industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004963758770000091
    Figure BDA0004963758770000091
Patent Text Reader

Abstract

The invention relates to the field of hot drawing machining of titanium alloy pipes, in particular to a hot drawing machining process of pure titanium TA4 electronic product parts. A hot drawing machining process for pure titanium TA4 electronic product parts comprises the following steps that firstly, a pure titanium TA4 seamless round pipe is sequentially subjected to surface sand blasting treatment, composite lubricating layer preparation and multiple times of wall reduction cold drawing and annealing treatment, the pure titanium TA4 round pipe is drawn into a pure titanium TA4 rectangular pipe after hot drawing treatment, the obtained pure titanium TA4 rectangular pipe is subjected to multiple times of wall reduction hot drawing treatment, and the pure titanium TA4 electronic product parts are obtained. And cleaning the surface to remove the composite lubricating layer to obtain the finished pure titanium TA4 part. The cold drawing and hot drawing combined machining mode is combined with the specially-made lubricating layer, the plasticity and bending performance of the pure titanium TA4 material are improved after heating drawing, and compared with cold drawing, the pass deformation is increased, the machining pass is reduced, the cost is saved, the production efficiency is improved, and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of hot drawing processing of titanium alloy pipes, and in particular to a hot drawing processing technology of pure titanium TA4 electronic product parts. Background Art

[0002] At present, in the rapidly developing electronics industry, there is an increasing demand for electronic product parts with light weight, surface hardness, and corrosion resistance, and the material selection must be a lightweight and high-strength alloy material. Pure titanium TA4, as a high-performance titanium alloy material, is lightweight, high-strength, excellent corrosion resistance, and high surface hardness, which meets the requirements of electronic product parts selection. However, it also has defects: the relatively poor plasticity caused by high strength and the overall bending performance is also biased, and the processing characteristics of electronic product parts are mostly special-shaped, which is not suitable for rolling in mass production technology.

[0003] In the existing technology, the production processes based on pure titanium TA4 materials to process target electronic product parts mostly adopt bending, welding or cold drawing processes, but the bending and welding performance are worse than those of seamless pipes; and the production efficiency is relatively low, and the yield rate is not high, resulting in the high production cost of pure titanium TA4 electronic product parts produced by existing technology, which limits its application and development.

[0004] In order to overcome the defects in the prior art, the inventor provides a preparation method of a hot drawing process for pure titanium TA4 electronic product parts. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present application provides a hot drawing processing technology for pure titanium TA4 electronic product parts. The present invention changes the traditional process technology of cold drawing, bending and welding, and adopts a combined processing method of cold and hot drawing combined with a special lubricating layer. After heated drawing, the plasticity and bending performance of the pure titanium TA4 material are improved, and the deformation amount per pass is increased compared with cold drawing, the number of processing passes is reduced, the cost is saved, the production efficiency is improved, and the production cost is reduced. The use of a special lubricating layer can effectively solve the problem of low yield caused by friction loss and scratches, and further reduce production costs.

[0006] The present application provides a hot drawing process for pure titanium TA4 electronic product parts, which is achieved through the following technical solutions:

[0007] A hot drawing process for pure titanium TA4 electronic product parts comprises the following steps:

[0008] Step 1: sandblasting the surface of the pure titanium TA4 seamless round tube;

[0009] Step 2: preparing a composite lubricating layer on the surface of a pure titanium TA4 seamless round tube, wherein the composite lubricating layer comprises a bottom layer and an outer lubricating layer, and the outer lubricating layer is mainly made of molybdenum disulfide, graphene, and graphite;

[0010] Step 3, the pure titanium TA4 seamless round tube obtained in step 2 is subjected to wall reduction cold drawing, the deformation amount of the wall reduction cold drawing is controlled at 2-15%, and annealing is performed after the wall reduction cold drawing is completed;

[0011] Step 4, repeating the wall-reducing cold drawing and annealing treatment in step 3 until the wall thickness of the obtained pure titanium TA4 seamless round tube is reduced to 0.1-0.5 times the thickness of the pure titanium TA4 seamless round tube in step 1;

[0012] Step 5, hot drawing the pure titanium TA4 seamless round tube obtained in step 4, wherein the pure titanium TA4 seamless round tube undergoes at least three deformation steps: round tube→elliptical tube→elliptical square tube→rectangular tube, and the circumference compression of each step is controlled at 2-8%;

[0013] Step 6, performing wall-reducing hot drawing treatment on the pure titanium TA4 seamless rectangular tube obtained in step 5, wherein the wall-reducing hot drawing deformation is controlled at 5-15%;

[0014] Step seven, repeat the wall reduction hot drawing treatment in step six until the wall thickness of the obtained pure titanium TA4 seamless rectangular tube is reduced to 0.2-0.7 times the thickness of the pure titanium TA4 seamless rectangular tube in step five, and clean the surface to obtain a finished pure titanium TA4 part.

[0015] The present invention changes the traditional process technology of cold drawing, bending and welding, and adopts a combined processing method of cold drawing and hot drawing combined with a special lubricating layer. After heated drawing, the plasticity and bending performance of pure titanium TA4 material are improved. Compared with cold drawing, the deformation amount per pass is increased, the processing passes are reduced, the cost is saved, the production efficiency is improved, and the production cost is reduced. The use of a special lubricating layer can effectively solve the problem of low yield rate caused by friction loss and scratches, and further reduce production costs.

[0016] Preferably, in the step one, the pure titanium TA4 seamless round tube is first sandblasted with 60-100 mesh corundum, then sandblasted with 300-400 mesh corundum, and finally sandblasted with 1500-2000 mesh corundum, so that the surface roughness of the titanium alloy tube after sandblasting is Ra1.0-Ra2.5. The pure titanium TA4 seamless round tube after sandblasting is cleaned at least three times with deionized water, and then input into an oven to dry at 80°C for 1-3h for standby use.

[0017] By adopting the above technical solution, pollutants and oxide impurities on the surface can be effectively removed, making it easier to combine with composite lubrication.

[0018] Preferably, in the step two, the preparation of the composite lubricating layer on the surface of the pure titanium TA4 seamless round tube is specifically as follows: first, the surface of the pure titanium TA4 seamless round tube is coated and dried once with an organic titanium compound, and then the surface of the pure titanium TA4 seamless round tube is coated and dried twice with a coupling agent, and finally a lubricant mixed slurry is prepared, and the prepared lubricant mixed slurry is evenly coated on the release paper and dried to form a semi-solidified lubricating film, and the obtained semi-solidified lubricating film is coated on the outer wall of the pure titanium TA4 seamless round tube, and then a composite lubricating layer is formed on the surface of the pure titanium TA4 seamless round tube after hot pressing and drying.

[0019] Preferably, the lubricant mixed slurry in step 2 comprises graphene grafted modified molybdenum disulfide sheets, flake graphite, hydrolyzable latex particles, and deionized water, and the solid content of the lubricant mixed slurry is controlled to be 20-40wt%.

[0020] Preferably, the graphene-grafted modified molybdenum disulfide sheets and flake graphite in the semi-cured lubricating film are bonded and fixed by hydrolyzable latex particles to form a semi-cured lubricating film; the hydrolyzable latex particles are hydrolyzed at 50-70°C and pH 8-9.

[0021] Preferably, the preparation method of the graphene grafted modified molybdenum disulfide sheet is as follows: first, metal nanoclusters are formed on the surface of the molybdenum disulfide sheet by a chemical vapor deposition process or a sol-gel process, and then the graphene aqueous dispersion and the molybdenum disulfide sheet with the surface grafted metal nanoclusters are placed in a planetary ball mill for wet ball milling, first at a rotation speed of 600-800 rpm, and during the ball milling process, heating and vacuuming for 5-10 minutes, after removing part of the water vapor, adjusting the rotation speed to 2000-3000 rpm, vacuuming to remove all the water vapor, and continuing to ball mill at a speed of 2000-3000 rpm for 5-15 minutes to obtain the surface graphene grafted modified molybdenum disulfide sheet.

[0022] Preferably, the organic titanium compound is DORF KETAL organic titanium Tyzor 726; and the coupling agent is a titanate coupling agent.

[0023] By adopting the above technical solution, the use of the above composite lubricating layer can reduce surface scratches during the hot drawing process of the product; and make the surface treatment of the product after drawing convenient, simplify the subsequent surface cleaning process, and save overall production costs.

[0024] Preferably, the heating method of the hot drawing process in step five is electromagnetic induction heating, and the electromagnetic heating induction coil is installed at the front end of the drawing die, and the temperature of the pure titanium TA4 seamless round tube input into the drawing die is 400-600°C.

[0025] Preferably, in step three, the pure titanium TA4 seamless round tube obtained in step two is subjected to wall-reducing cold drawing, the deformation of the wall-reducing cold drawing is controlled at 12-15%, and after the wall-reducing cold drawing is completed, annealing treatment is performed at 700-800° C. for 0.5-2.0 h;

[0026] Preferably, in the step four, the wall-reducing cold drawing and annealing treatment in step three is repeated 2-4 times, and the wall-reducing cold drawing deformation is 12-15%; the wall-reducing cold drawing and annealing treatment in step three is repeated 2-4 times, and the wall-reducing cold drawing deformation is 8-12%; the wall-reducing cold drawing and annealing treatment in step three is repeated 2-8 times, and the wall-reducing cold drawing deformation is 6-8%; the wall-reducing cold drawing and annealing treatment in step three is repeated 2-20 times, and the wall-reducing cold drawing deformation is 2-6%, until the wall thickness of the obtained pure titanium TA4 seamless round tube is reduced to 0.1-0.5 times the thickness of the pure titanium TA4 seamless round tube in the step one.

[0027] Preferably, in step six, the pure titanium TA4 seamless rectangular tube obtained in step five is subjected to wall reduction hot drawing treatment, and the wall reduction hot drawing deformation is controlled at 6-8%;

[0028] Preferably, in the step seven, the wall reducing hot drawing treatment in step six is ​​repeated 2-4 times, and the wall reducing hot drawing deformation is controlled at 6-8%; the wall reducing hot drawing treatment in step six is ​​repeated 2-4 times, and the wall reducing hot drawing deformation is controlled at 4-6%; the wall reducing hot drawing treatment in step six is ​​repeated 2-20 times, and the wall reducing hot drawing deformation is controlled at 2-4%; until the wall thickness of the obtained pure titanium TA4 seamless rectangular tube is reduced to 0.2-0.7 times the thickness of the pure titanium TA4 seamless rectangular tube in the step five, and the finished pure titanium TA4 parts are obtained by ultrasonic surface cleaning and drying in an environment of 50-70°C and pH 8-9.

[0029] By adopting the above technical solution, the probability of R-angle cracks occurring during the drawing process can be effectively reduced, and the yield rate of pure titanium TA4 electronic product parts can be greatly improved, thereby reducing production costs and expanding the application and development of pure titanium TA4 electronic parts.

[0030] In summary, this application has the following advantages:

[0031] 1. The present invention changes the traditional process technology of cold drawing, bending and welding, and adopts a combined cold and hot drawing processing method combined with a special lubricating layer. After heating and drawing, the plasticity and bending performance of pure titanium TA4 material are improved. Compared with cold drawing, the deformation amount per pass is increased, the processing passes are reduced, the cost is saved, the production efficiency is improved, and the production cost is reduced. In addition, the use of a special lubricating layer can effectively solve the problem of low yield rate caused by friction loss and scratches, and further reduce production costs.

[0032] 2. The preparation method of the present application is relatively simple and has low operating difficulty, which facilitates industrial production and manufacturing, reduces the production cost of pure titanium TA4 electronic parts, expands their application and development, and promotes the development of the domestic electronics industry. DETAILED DESCRIPTION

[0033] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples.

[0034] Example

[0035] A hot drawing process for pure titanium TA4 electronic product parts comprises the following steps:

[0036] Step 1, the surface of the pure titanium TA4 seamless round tube is sandblasted: first, 60-100 mesh corundum is used for the first sandblasting, then 300-400 mesh corundum is used for the second sandblasting, and then 1500-2000 mesh corundum is used for the third sandblasting, so that the surface roughness of the titanium alloy tube after sandblasting is Ra1.0-Ra2.5, and the pure titanium TA4 seamless round tube after sandblasting is washed at least three times with deionized water, and then put into an oven for drying at 80°C for 1-3h for standby use;

[0037] Step 2, preparation of a composite lubricating layer on the surface of a pure titanium TA4 seamless round tube: The preparation of a composite lubricating layer on the surface of a pure titanium TA4 seamless round tube is specifically as follows: first, an organic titanium compound is used to coat and dry the surface of the pure titanium TA4 seamless round tube once, and then a coupling agent is used to coat and dry the surface of the pure titanium TA4 seamless round tube for a second time, and finally a lubricant mixed slurry is prepared, and the prepared lubricant mixed slurry is evenly coated on the release paper and dried to form a semi-solidified lubricating film. The graphene grafted modified molybdenum disulfide sheet and flake graphite in the semi-solidified lubricating film are bonded and fixed by hydrolyzable latex particles to form a semi-solidified lubricating film; the hydrolyzable latex particles are hydrolyzed at 50-70°C and pH 8-9, and the obtained semi-solidified lubricating film is coated on the outer wall of the pure titanium TA4 seamless round tube, and then hot pressed and dried to form a composite lubricating layer on the surface of the pure titanium TA4 seamless round tube;

[0038] The preparation method of the graphene grafted modified molybdenum disulfide sheet is as follows: firstly, a metal nanocluster is formed on the surface of the molybdenum disulfide sheet by a chemical vapor deposition process or a sol-gel process, and then the graphene water dispersion and the molybdenum disulfide sheet with the surface grafted metal nanocluster are placed in a planetary ball mill for wet ball milling treatment, firstly the ball milling treatment is carried out at a rotation speed of 600-800 rpm, and during the ball milling process, heating and vacuuming are performed for 5-10 minutes, and after part of the water vapor is removed, the rotation speed is adjusted to 2000-3000 rpm, and after vacuuming and removing all the water vapor, the ball milling is continued at a rotation speed of 2000-3000 rpm for 5-15 minutes to obtain the surface graphene grafted modified molybdenum disulfide sheet;

[0039] The composite lubricating layer includes a bottom layer and an outer lubricating layer, and the outer lubricating layer is mainly made of molybdenum disulfide, graphene, and graphite;

[0040] Preferably, the lubricant mixed slurry comprises graphene grafted modified molybdenum disulfide sheets, flake graphite, hydrolyzable latex particles, and deionized water, and the solid content of the lubricant mixed slurry is controlled to be 20-40wt%; the organic titanium compound is DORF KETAL organic titanium Tyzor 726; the coupling agent is a titanate coupling agent;

[0041] Step 3, the pure titanium TA4 seamless round tube obtained in step 2 is subjected to wall reduction cold drawing, the deformation of the wall reduction cold drawing is controlled at 2-15%, and annealing is performed after the wall reduction cold drawing is completed, and the temperature is kept at 700-800° C. for 0.5-2.0 h;

[0042] Step 4, repeating the wall-reducing cold drawing and annealing treatment in step 3 until the wall thickness of the obtained pure titanium TA4 seamless round tube is reduced to 0.1-0.3 times the thickness of the pure titanium TA4 seamless round tube in step 1;

[0043] Preferably, in step three, the pure titanium TA4 seamless round tube obtained in step two is subjected to wall-reducing cold drawing, and the deformation of the wall-reducing cold drawing is controlled at 12-15%, and annealing is performed after the wall-reducing cold drawing is completed; in step four, the wall-reducing cold drawing and annealing treatment in step three are repeated 2-4 times, and the wall-reducing cold drawing deformation is 12-15%; the wall-reducing cold drawing and annealing treatment in step three are repeated 2-4 times, and the wall-reducing cold drawing deformation is 8-12%; the wall-reducing cold drawing and annealing treatment in step three are repeated 2-8 times, and the wall-reducing cold drawing deformation is 6-8%; the wall-reducing cold drawing and annealing treatment in step three are repeated 2-20 times, and the wall-reducing cold drawing deformation is 2-6%, until the wall thickness of the obtained pure titanium TA4 seamless round tube is reduced to 0.1-0.5 times the thickness of the original pure titanium TA4 seamless round tube;

[0044] Step 5, hot drawing the pure titanium TA4 seamless round tube obtained in step 4, the heating method is electromagnetic induction heating, the electromagnetic heating induction coil is installed at the front end of the drawing die, the temperature of the pure titanium TA4 seamless round tube input into the drawing die is 400-600°C by the electromagnetic heating induction coil, and the pure titanium TA4 seamless round tube is deformed through at least three passes: round tube → elliptical tube → elliptical square tube → rectangular tube, and the circumference compression of each pass is controlled at 2-8%;

[0045] Step 6, the pure titanium TA4 seamless rectangular tube obtained in step 5 is subjected to wall reduction hot drawing treatment, the heating method is electromagnetic induction heating, the electromagnetic heating induction coil is installed at the front end of the drawing die, the temperature of the pure titanium TA4 seamless round tube input into the drawing die is 400-600°C by the electromagnetic heating induction coil, and the wall reduction hot drawing deformation is controlled at 2-8%;

[0046] Step seven, repeat the wall reduction hot drawing treatment in step six until the wall thickness of the obtained pure titanium TA4 seamless rectangular tube is reduced to 0.1-0.3 times the thickness of the pure titanium TA4 seamless rectangular tube in step five, and clean the surface to obtain a finished pure titanium TA4 part.

[0047] Preferably, in step six, the pure titanium TA4 seamless rectangular tube obtained in step five is subjected to wall reduction hot drawing treatment, and the wall reduction hot drawing deformation is controlled at 6-8%; in step seven, the wall reduction hot drawing treatment in step six is ​​repeated 2-4 times, and the wall reduction hot drawing deformation is controlled at 6-8%; the wall reduction hot drawing treatment in step six is ​​repeated 2-4 times, and the wall reduction hot drawing deformation is controlled at 4-6%; the wall reduction hot drawing treatment in step six is ​​repeated 2-20 times, and the wall reduction hot drawing deformation is controlled at 2-4%; until the wall thickness of the obtained pure titanium TA4 seamless rectangular tube is reduced to 0.2-0.7 times the thickness of the pure titanium TA4 seamless rectangular tube in step five, and the finished pure titanium TA4 parts are obtained by ultrasonic surface cleaning and drying in an environment of 50-70°C and pH 8-9.

[0048] Embodiment 1: A hot drawing process for pure titanium TA4 electronic product parts, comprising the following steps:

[0049] Step 1, the surface of the pure titanium TA4 seamless round tube (Dongguan Ruiteng Metal Materials Co., Ltd., wall thickness of 1.0mm) is sandblasted: first use 80 mesh corundum for the first sandblasting, then use 325 mesh corundum for the second sandblasting, and then use 2000 mesh corundum for the third sandblasting, so that the surface roughness of the titanium alloy tube after sandblasting is Ra1.0-Ra2.5, the pure titanium TA4 seamless round tube after sandblasting is washed three times with deionized water, and then put into an oven for drying at 80°C for 2h for standby;

[0050] At the same time, graphene grafted modified molybdenum disulfide sheets were prepared. The specific preparation method was as follows: first, metal nanoclusters were formed on the surface of the molybdenum disulfide sheets by chemical vapor deposition process: 6.45g of silver nitrate was dissolved in 250ml of ethanol aqueous solution (50ml of ethanol + 200ml of deionized water) at room temperature and under nitrogen protection, and mixed evenly to obtain a metal precursor mixed solution; at the same time, 0.82g of NaBH4 was dissolved in 500ml of deionized water at room temperature and under nitrogen protection, and 5g of molybdenum disulfide sheets (flaky molybdenum disulfide powder customized by Beijing Beike New Materials Technology Co., Ltd., with a sheet diameter of 3-5μm and a thickness of 50-10 0nm), ultrasonic dispersion treatment at an ultrasonic frequency of 40kHz / 600W for 15min, and a mixed solution of molybdenum disulfide flakes was uniformly dispersed; at room temperature and nitrogen protection conditions, the metal precursor mixed solution was added dropwise to the mixed solution of molybdenum disulfide flakes at a speed of 100 drops / min, and the reaction was continued for 30min after the addition was completed. After standing for 6h, the supernatant was poured out, and 500mL of deionized water was added and stood for 6h, and then the supernatant was poured out, and the above operation was repeated three times to obtain a precipitate, and the obtained precipitate was vacuum heated and dried at a temperature of 98°C and a vacuum drying time of 24h under a vacuum setting value of 0.1Pa, and the obtained solid was placed in a planetary ball mill for wet ball milling treatment, The surface-grafted nano-Ag@MoS2 material with a particle size of D50 = 200 nm can be obtained by ball milling at a speed of 200 rpm for 0.5 h; then 20 g of graphene aqueous dispersion (TimesGraph-graphene dispersion of Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, purity: >98wt%, thickness: 0.55-3.74nm, diameter: 0.5-3μm, number of layers: <10 layers, customized solid content 2.5wt%) and 10 g of surface-grafted nano-Ag@MoS2 material are placed in a planetary ball mill for wet ball milling treatment, first at a speed of 600 rpm, and heated and vacuumed for 5 min during the ball milling process to remove After removing part of the water vapor, adjusting the speed to 2250rpm, vacuuming to remove all the water vapor and continuing to ball mill at 2250rpm for 8min, the surface graphene grafted modified molybdenum disulfide sheet can be obtained; 50wt% high solid content soft resin FS-151650 is diluted with deionized water to become an aqueous polyurethane emulsion with a solid content of 0.5wt%, 5g of the surface graphene grafted modified molybdenum disulfide sheet is placed in 100g of the aqueous polyurethane emulsion with a solid content of 0.5wt% for ultrasonic dispersion treatment for 10min, the ultrasonic frequency is 40kHz / 60W, draining, taking out, and drying at 80°C to obtain the finished surface graphene grafted modified molybdenum disulfide sheet;

[0051] Step 2: Preparation of composite lubricating layer on the surface of pure titanium TA4 seamless round tube: First, use organic titanium compound - DORFKETAL organic titanium Tyzor 726 to coat the surface of pure titanium TA4 seamless round tube with 5g / m 2After drying, the surface of the pure titanium TA4 seamless round tube was coated with 20g / m2 of titanate KR138S hydrolyzate (5mL of titanate KR138S hydrolyzate + 15mL of ethanol + 80mL of deionized water) for the second time. 2 Drying treatment; prepare lubricant mixed slurry: 17g of finished surface graphene grafted modified molybdenum disulfide sheet, 10g of flake graphite (2000 mesh ultrafine graphite powder from Henglin Minerals), 60g of deionized water, 2g of emulsifier OP, 1g of TX-4 alkylphenol polyoxyethylene ether, 6g of polyurethane acrylate, 1.5g of epoxy modified acrylate, 1g of 1,6-hexanediol diacrylate, 0.5g of tripropylene glycol diacrylate, 0.6g of poly Ethylene glycol PEG600 and 0.4g of 2-hydroxy-2-methyl-1-phenyl-1-propanone are prepared into a lubricant mixed slurry with a solid content of 30wt%, and the obtained lubricant mixed slurry is evenly coated on a release paper and dried at 60°C to form a semi-cured film with a thickness of 50-55μm, and the contact surface of the obtained semi-cured lubricating film and the release paper is coated on the outer wall of a pure titanium TA4 seamless round tube, and then hot-pressed and dried to form a composite lubricating layer on the surface of the pure titanium TA4 seamless round tube;

[0052] Step 3, the pure titanium TA4 seamless round tube obtained in step 2 is subjected to wall reduction cold drawing, the deformation of the wall reduction cold drawing is controlled at 14%, and after the wall reduction cold drawing is completed, annealing treatment is performed, the temperature is raised to 760° C. and kept for 0.5 h, and then cooled to room temperature by self-cooling;

[0053] Step 4: Repeat the wall-reducing cold drawing and annealing treatment in step 3 twice, and the wall-reducing cold drawing deformation is 13 / 12% respectively; repeat the wall-reducing cold drawing and annealing treatment in step 3 4 times, and the wall-reducing cold drawing deformation is 11 / 10 / 9 / 8%; repeat the wall-reducing cold drawing and annealing treatment in step 3 4 times, and the wall-reducing cold drawing deformation is 7 / 7 / 6 / 6%; repeat the wall-reducing cold drawing and annealing treatment in step 3 2 times, and the wall-reducing cold drawing deformation is 4 / 2%, and the wall thickness of the pure titanium TA4 seamless round tube is 0.317 mm, which is reduced to 0.317 times the thickness of the pure titanium TA4 seamless round tube before drawing;

[0054] Step 5, the pure titanium TA4 seamless round tube obtained in step 4 is subjected to hot drawing treatment, and the heating method is electromagnetic induction heating. The electromagnetic heating induction coil is installed at the front end of the drawing die, and the temperature of the pure titanium TA4 seamless round tube input into the drawing die is 580°C through the electromagnetic heating induction coil. The pure titanium TA4 seamless round tube undergoes three deformations: round tube → elliptical tube → elliptical square tube → rectangular tube, and the circumference compression of each pass is controlled at 4%;

[0055] Step 6, the pure titanium TA4 seamless rectangular tube obtained in step 5 is subjected to wall reduction hot drawing treatment, the heating method is electromagnetic induction heating, the electromagnetic heating induction coil is installed at the front end of the drawing die, the temperature of the pure titanium TA4 seamless round tube input into the drawing die is 580°C by the electromagnetic heating induction coil, and the wall reduction hot drawing deformation is controlled at 8%;

[0056] Step seven, repeat the wall reduction hot drawing treatment in step six twice, and the wall reduction hot drawing deformation is controlled at 7 / 6%; repeat the wall reduction hot drawing treatment in step six twice, and the wall reduction hot drawing deformation is controlled at 5 / 4%; repeat the wall reduction hot drawing treatment in step six 4 times, and the wall reduction hot drawing deformation is controlled at 3 / 3 / 2 / 2%. The obtained pure titanium TA4 seamless rectangular tube has a thick wall of 0.194mm, which is reduced to 0.61 times the thickness of the pure titanium TA4 seamless rectangular tube in step five. The obtained pure titanium TA4 seamless rectangular tube is subjected to ultrasonic surface cleaning for 300s in an environment of 70°C, pH 8 sodium bicarbonate aqueous solution, with an ultrasonic frequency of 44kHz and an ultrasonic power of 600W. After the ultrasonic cleaning is completed, it is washed twice with deionized water and dried to obtain a finished pure titanium TA4 part.

[0057] The difference between Example 2 and Example 1 is that: Step 2, preparation of composite lubricating layer on the surface of pure titanium TA4 seamless round tube: firstly, the surface of pure titanium TA4 seamless round tube is coated with 5g / m2 organic titanium compound-DORF KETAL organic titanium Tyzor 726. 2 After drying, the surface of the pure titanium TA4 seamless round tube was coated with 20g / m2 of titanate KR138S hydrolyzate (5mL of titanate KR138S hydrolyzate + 15mL of ethanol + 80mL of deionized water) for the second time. 2 Drying treatment; preparing lubricant mixed slurry: firstly, 0.5g of graphene and 16.5g of molybdenum disulfide sheet were placed in a planetary ball mill and ball-milled at 200rpm for 15min to obtain 17g of mixed material, and 17g of mixed material was mixed with 10g of flake graphite, 60g of deionized water, 2g of emulsifier OP, 1g of TX-4 alkylphenol polyoxyethylene ether, 6g of polyurethane acrylate, 1.5g of epoxy modified acrylate, 1g of 1,6-hexanediol diacrylate, 0.5g of tripropylene glycol. Diacrylate, 0.6g polyethylene glycol PEG600, and 0.4g 2-hydroxy-2-methyl-1-phenyl-1-propanone are prepared into a lubricant mixed slurry with a solid content of 30wt%. The obtained lubricant mixed slurry is evenly coated on the release paper and dried at 60°C to form a semi-cured film with a thickness of 50-55μm. The contact surface of the obtained semi-cured lubricating film and the release paper is coated on the outer wall of the pure titanium TA4 seamless round tube, and then hot pressed and dried to form a composite lubricating layer on the surface of the pure titanium TA4 seamless round tube.

[0058] The difference between Example 3 and Example 1 is that: in step three, the pure titanium TA4 seamless round tube obtained in step two is subjected to wall-reducing cold drawing, and the deformation of the wall-reducing cold drawing is controlled at 14%. After the wall-reducing cold drawing is completed, annealing is performed, the temperature is raised to 680°C and kept for 0.5h, and then cooled to room temperature by self-cooling; in step four, the wall-reducing cold drawing and annealing treatments in step three are repeated 6 times, and the wall-reducing cold drawing deformations are 14% respectively; the wall-reducing cold drawing and annealing treatments in step three are repeated, and the wall-reducing cold drawing deformation is 9%, and the wall thickness of the pure titanium TA4 seamless round tube is 0.317mm.

[0059] The difference between Example 4 and Example 1 is that: in step seven, the wall reduction hot drawing treatment in step six is ​​repeated three times, and the wall reduction hot drawing deformation is 8%; the wall reduction hot drawing treatment in step six is ​​repeated once, and the wall reduction hot drawing deformation is 4%. The obtained pure titanium TA4 seamless rectangular tube has a thick wall of 0.193 mm, which is reduced to 0.61 times the thickness of the pure titanium TA4 seamless rectangular tube in step five. The obtained pure titanium TA4 seamless rectangular tube is subjected to ultrasonic surface cleaning for 300 s in an environment of 70°C, pH 8, and sodium bicarbonate aqueous solution. The ultrasonic frequency is 44 kHz, and the ultrasonic power is 600 W. After the ultrasonic cleaning is completed, it is washed twice with deionized water and dried to obtain the finished pure titanium TA4 parts.

[0060] The difference between Example 5 and Example 1 is that: Step 3, the pure titanium TA4 seamless round tube obtained in Step 2 is subjected to wall reduction cold drawing, and the wall reduction cold drawing deformation is controlled at 14%. After the wall reduction cold drawing is completed, annealing treatment is performed, the temperature is raised to 680°C and kept for 0.5h, and then cooled to room temperature by self-cooling; Step 4, the wall reduction cold drawing and annealing treatment in Step 3 are repeated 6 times, and the wall reduction cold drawing deformation is 14%; Repeat the wall reduction cold drawing and annealing treatment in Step 1, and the wall reduction cold drawing deformation is 9%. The wall thickness of the pure titanium TA4 seamless round tube is 0.317mm and Step 7 is repeated 3 times in Step 6 The wall-reducing hot drawing treatment is performed, and the wall-reducing hot drawing deformation is 8%; the wall-reducing hot drawing treatment in step six is ​​repeated once, and the wall-reducing hot drawing deformation is 4%. The thick wall of the obtained pure titanium TA4 seamless rectangular tube is 0.193 mm, that is, it is reduced to 0.61 times the thickness of the pure titanium TA4 seamless rectangular tube in step five. The obtained pure titanium TA4 seamless rectangular tube is subjected to ultrasonic surface cleaning treatment for 300 s at 70°C and pH 8 in a sodium bicarbonate aqueous solution environment, with an ultrasonic frequency of 44 kHz and an ultrasonic power of 600 W. After the ultrasonic cleaning is completed, it is washed twice with deionized water and dried to obtain a finished pure titanium TA4 part.

[0061] The difference between Comparative Example 1 and Example 1 is as follows: Step 2, preparation of composite lubricating layer on the surface of pure titanium TA4 seamless round tube: firstly, the surface of pure titanium TA4 seamless round tube is coated with 5g / m2 organic titanium compound-DORF KETAL organic titanium Tyzor 726. 2After drying, the surface of the pure titanium TA4 seamless round tube was coated with 20g / m2 of titanate KR138S hydrolyzate (5mL of titanate KR138S hydrolyzate + 15mL of ethanol + 80mL of deionized water) for the second time. 2 Drying treatment; preparing lubricant mixed slurry: 27g flake graphite, 60g deionized water, 2g emulsifier OP, 1g TX-4 alkylphenol polyoxyethylene ether, 6g polyurethane acrylate, 1.5g epoxy modified acrylate, 1g 1,6-hexanediol diacrylate, 0.5g tripropylene glycol diacrylate, 0.6g polyethylene glycol PEG600, 0.4g 2-hydroxy-2-methyl-1-phenyl-1-propanone are prepared into a lubricant mixed slurry with a solid content of 30wt%. The obtained lubricant mixed slurry is evenly coated on release paper and dried at 60°C to form a semi-cured film with a thickness of 50-55μm. The obtained semi-cured lubricating film and the contact surface of the release paper are coated on the outer wall of the pure titanium TA4 seamless round tube, hot pressed and dried to form a composite lubricating layer on the surface of the pure titanium TA4 seamless round tube.

[0062] The difference between Comparative Example 2 and Example 1 is that: Step 2, preparation of composite lubricating layer on the surface of pure titanium TA4 seamless round tube: firstly, a 20 g / m2 coating is performed on the surface of pure titanium TA4 seamless round tube using titanate KR138S hydrolyzate (5 mL of titanate KR138S hydrolyzate + 15 mL of ethanol + 80 mL of deionized water) 2 Drying treatment; preparing lubricant mixed slurry: 27g flake graphite, 60g deionized water, 2g emulsifier OP, 1g TX-4 alkylphenol polyoxyethylene ether, 6g polyurethane acrylate, 1.5g epoxy modified acrylate, 1g 1,6-hexanediol diacrylate, 0.5g tripropylene glycol diacrylate, 0.6g polyethylene glycol PEG600, 0.4g 2-hydroxy-2-methyl-1-phenyl-1-propanone are prepared into a lubricant mixed slurry with a solid content of 30wt%. The obtained lubricant mixed slurry is evenly coated on release paper and dried at 60°C to form a semi-cured film with a thickness of 50-55μm. The obtained semi-cured lubricating film and the contact surface of the release paper are coated on the outer wall of the pure titanium TA4 seamless round tube, hot pressed and dried to form a composite lubricating layer on the surface of the pure titanium TA4 seamless round tube.

[0063] The difference between Comparative Example 3 and Example 1 is: Step 2, preparing a lubricant mixed slurry: 27g of flake graphite, 60g of deionized water, 2g of emulsifier OP, 1g of TX-4 alkylphenol polyoxyethylene ether, 6g of polyurethane acrylate, 1.5g of epoxy modified acrylate, 1g of 1,6-hexanediol diacrylate, 0.5g of tripropylene glycol diacrylate, 0.6g of polyethylene glycol PEG600, and 0.4g of 2-hydroxy-2-methyl-1-phenyl-1-propanone are prepared into a lubricant mixed slurry with a solid content of 30wt%. The obtained lubricant mixed slurry is evenly coated on a release paper and dried at 60°C to form a semi-cured film with a thickness of 50-55μm. The obtained semi-cured lubricating film and the contact surface of the release paper are coated on the outer wall of the pure titanium TA4 seamless round tube, hot pressed, and dried to form a composite lubricating layer on the surface of the pure titanium TA4 seamless round tube.

[0064] The difference between Comparative Example 4 and Example 1 is as follows: Step 2, preparation of composite lubricating layer on the surface of pure titanium TA4 seamless round tube: firstly, the surface of pure titanium TA4 seamless round tube is coated with 5g / m2 organic titanium compound-DORF KETAL organic titanium Tyzor 726. 2 After drying, the surface of the pure titanium TA4 seamless round tube was coated with 20g / m2 of titanate KR138S hydrolyzate (5mL of titanate KR138S hydrolyzate + 15mL of ethanol + 80mL of deionized water) for the second time. 2 Drying treatment; preparing lubricant mixed slurry: 17g of finished surface graphene grafted modified molybdenum disulfide sheet, 10g of flake graphite (2000 mesh ultrafine graphite powder of Henglin Mineral), 55g of deionized water, 2g of emulsifier OP, 1g of TX-4 alkylphenol polyoxyethylene ether, and 20g of 50wt% high solid content soft resin FS-151650 are prepared into a lubricant mixed slurry with a solid content of 30wt%. The obtained lubricant mixed slurry is evenly coated on the release paper and dried at 60°C to form a semi-cured film with a thickness of 50-55μm. The obtained semi-cured lubricating film and the contact surface of the release paper are coated on the outer wall of the pure titanium TA4 seamless round tube, and a composite lubricating layer can be formed on the surface of the pure titanium TA4 seamless round tube after hot pressing and drying.

[0065] Performance test: Appearance test: Observe the adhesion and scratches of the lubricating layer on the surface of the finished pure titanium TA4 parts with the naked eye. Yield evaluation method: 20 raw material pure titanium TA4 seamless round tubes of the same batch are respectively subjected to the hot drawing process of Examples 1-5 and Comparative Examples 1-4, and the surface of the obtained finished pure titanium TA4 parts tube is photographed with a high-definition digital camera to check the R-angle cracks on the surface of the finished pure titanium TA4 parts, and the finished pure titanium TA4 parts tube is subjected to impact strength test. When the impact strength of the finished pure titanium TA4 parts tube is greater than 0.9 times that of the raw material pure titanium TA4 seamless round tube, it is qualified, otherwise it is waste.

[0066] Table 1: Test parameters of finished pure titanium TA4 parts tubes in Examples 1-5 and Comparative Examples 1-4

[0067]

[0068]

[0069] It can be seen from Examples 1-5 and Comparative Examples 1-4 and Table 1 that the formula of the composite lubricating layer and its preparation process have a correlation with the scratches, R-angle cracks and yield rate of the finished pure titanium TA4 parts tube. The finished pure titanium TA4 parts tube prepared by the preparation process provided in the present application has stable surface performance and a high yield rate, which can reduce the overall production cost.

[0070] It can be seen from Examples 1-5 and Comparative Examples 1-4 and Table 1 that the wall-reducing cold drawing deformation of the wall-reducing cold drawing process has a correlation with the scratches, R-angle cracks and yield rate of the finished pure titanium TA4 part tube. The finished pure titanium TA4 part tube prepared by the preparation process provided by the present application has stable surface performance and a high yield rate.

[0071] It can be seen from Examples 1-5 and Comparative Examples 1-4 and Table 1 that the wall-reducing hot drawing deformation of the wall-reducing hot drawing process has a correlation with the scratches, R-angle cracks and yield rate of the finished pure titanium TA4 part tube. The finished pure titanium TA4 part tube prepared by the preparation process provided by the present application has stable surface performance and a high yield rate.

[0072] Combining Examples 1-5 and Comparative Examples 1-4 and Table 1, it can be seen that the hot drawing process method for the pure titanium TA4 electronic product parts of Example 1 has relatively excellent material stability performance. In order to verify the industrial mass production performance of the technical solution of Example 1, the hot drawing process of the pure titanium TA4 electronic product parts of Example 1 was used to carry out pilot production of 500 finished pure titanium TA4 parts tubes. According to the above-mentioned yield evaluation method, 496 of the 500 finished pure titanium TA4 parts tubes produced by the hot drawing process of the pure titanium TA4 electronic product parts of Example 1 were good products, 1 was scrapped because the impact strength of the finished pure titanium TA4 parts tube was 0.9 times lower than the impact strength of the raw material pure titanium TA4 seamless round tube due to too many R-angle cracks, and 3 were scrapped because the appearance inspection failed to meet the standards due to the deep scratches on the local surface, and the yield rate was 99.2%.

[0073] It can be seen from Examples 1-5 and Comparative Examples 1-4 and Table 1-2 that the present invention changes the traditional process technology of cold drawing, bending and welding, and adopts a combined processing method of cold drawing and hot drawing combined with a special lubricating layer. The cold drawing process combined with the special lubricating layer effectively reduces the wall thickness while reducing the probability of cold drawing scratches, thereby improving the overall material stability. The plasticity and bending properties of the pure titanium TA4 material are improved after post-hot drawing. Compared with cold drawing, the deformation amount per pass is increased, the number of processing passes is reduced, costs are saved, production efficiency is improved, and production costs are reduced. The use of a special lubricating layer can effectively solve the problem of low yield caused by friction loss and scratches, and the lubricating layer is easy to clean, further reducing the overall production cost.

[0074] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A hot drawing process for pure titanium TA4 electronic product parts, characterized in that: The following steps are involved: Step 1: sandblasting the surface of the pure titanium TA4 seamless round tube; Step 2: preparing a composite lubricating layer on the surface of a pure titanium TA4 seamless round tube, wherein the composite lubricating layer comprises a bottom layer and an outer lubricating layer, and the outer lubricating layer is mainly made of molybdenum disulfide, graphene, and graphite; Step 3, performing wall-reducing cold drawing on the pure titanium TA4 seamless round tube obtained in step 2, wherein the deformation amount of the wall-reducing cold drawing is controlled at 2-15%, and annealing is performed after the wall-reducing cold drawing is completed; Step 4, repeating the wall-reducing cold drawing and annealing treatment in step 3 until the wall thickness of the obtained pure titanium TA4 seamless round tube is reduced to 0.1-0.5 times the thickness of the pure titanium TA4 seamless round tube in step 1; Step 5, hot drawing the pure titanium TA4 seamless round tube obtained in step 4, wherein the pure titanium TA4 seamless round tube undergoes at least three deformation steps: round tube→elliptical tube→elliptical square tube→rectangular tube, and the circumference compression of each step is controlled at 2-8%; Step 6, performing wall-reducing hot drawing treatment on the pure titanium TA4 seamless rectangular tube obtained in step 5, wherein the wall-reducing hot drawing deformation is controlled at 5-15%; Step seven, repeat the wall reduction hot drawing treatment in step six until the wall thickness of the obtained pure titanium TA4 seamless rectangular tube is reduced to 0.2-0.7 times the thickness of the pure titanium TA4 seamless rectangular tube in step five, and clean the surface to obtain a finished pure titanium TA4 part.

2. The hot drawing process of pure titanium TA4 electronic product parts according to claim 1 is characterized in that: In the step 1, the pure titanium TA4 seamless round tube is first sandblasted with 60-100 mesh corundum, then sandblasted with 300-400 mesh corundum, and finally sandblasted with 1500-2000 mesh corundum, so that the surface roughness of the titanium alloy tube after sandblasting is Ra1.0-Ra2.

5. The pure titanium TA4 seamless round tube after sandblasting is cleaned at least three times with deionized water, and then put into an oven for drying at 80°C for 1-3 hours for standby use.

3. The hot drawing process of pure titanium TA4 electronic product parts according to claim 1, characterized in that: The step two, the preparation of the composite lubricating layer on the surface of the pure titanium TA4 seamless round tube is specifically as follows: first, the surface of the pure titanium TA4 seamless round tube is coated and dried once with an organic titanium compound, and then the surface of the pure titanium TA4 seamless round tube is coated and dried twice with a coupling agent, and finally a lubricant mixed slurry is prepared, and the prepared lubricant mixed slurry is evenly coated on the release paper and dried to form a semi-solidified lubricating film, and the obtained semi-solidified lubricating film is coated on the outer wall of the pure titanium TA4 seamless round tube, and then hot pressed and dried to form a composite lubricating layer on the surface of the pure titanium TA4 seamless round tube.

4. The hot drawing process of pure titanium TA4 electronic product parts according to claim 3 is characterized in that: The lubricant mixed slurry in step 2 comprises graphene grafted modified molybdenum disulfide sheets, flake graphite, hydrolyzable latex particles, and deionized water. The solid content of the lubricant mixed slurry is controlled to be 20-40wt%.

5. The hot drawing process of pure titanium TA4 electronic product parts according to claim 4, characterized in that: The graphene grafted modified molybdenum disulfide sheets and flake graphite in the semi-cured lubricating film are bonded and fixed by hydrolyzable latex particles to form a semi-cured lubricating film; the hydrolyzable latex particles are hydrolyzed at 50-70° C. and pH 8-9.

6. The hot drawing process of pure titanium TA4 electronic product parts according to claim 4, characterized in that: The preparation method of the graphene grafted modified molybdenum disulfide sheet is as follows: firstly, metal nanoclusters are formed on the surface of the molybdenum disulfide sheet by a chemical vapor deposition process or a sol-gel process, and then the graphene water dispersion and the molybdenum disulfide sheet with the surface grafted metal nanoclusters are placed in a planetary ball mill for wet ball milling treatment, firstly ball milling treatment at a rotation speed of 600-800 rpm, heating and vacuuming for 5-10 minutes during the ball milling process, after removing part of the water vapor, adjusting the rotation speed to 2000-3000 rpm, vacuuming and removing all the water vapor, and continuing to ball mill at a rotation speed of 2000-3000 rpm for 5-15 minutes to obtain the surface graphene grafted modified molybdenum disulfide sheet.

7. The hot drawing process of pure titanium TA4 electronic product parts according to claim 3 is characterized in that: The organic titanium compound is DORF KETAL organic titanium Tyzor 726; and the coupling agent is a titanate coupling agent.

8. The hot drawing process of pure titanium TA4 electronic product parts according to claim 1, characterized in that: The heating method of the hot drawing process in step five is electromagnetic induction heating. The electromagnetic heating induction coil is installed at the front end of the drawing die. The temperature of the pure titanium TA4 seamless round tube input into the drawing die is 400-600℃ through the electromagnetic heating induction coil.

9. The hot drawing process of pure titanium TA4 electronic product parts according to claim 1, characterized in that: In the step three, the pure titanium TA4 seamless round tube obtained in the step two is subjected to wall-reducing cold drawing, and the deformation of the wall-reducing cold drawing is controlled at 12-15%. After the wall-reducing cold drawing is completed, annealing is performed and the temperature is kept at 700-800°C for 0.5-2.0h; in the step four, the wall-reducing cold drawing and annealing treatment in step three are repeated 2-4 times, and the wall-reducing cold drawing deformation is 12-15%; the wall-reducing cold drawing and annealing treatment in step three are repeated 2-4 times, and the wall-reducing cold drawing deformation is 8-12%; the wall-reducing cold drawing and annealing treatment in step three are repeated 2-8 times, and the wall-reducing cold drawing deformation is 6-8%; the wall-reducing cold drawing and annealing treatment in step three are repeated 2-20 times, and the wall-reducing cold drawing deformation is 2-6%, until the thick wall of the obtained pure titanium TA4 seamless round tube is reduced to 0.1-0.5 times the thickness of the pure titanium TA4 seamless round tube in the step one.

10. The hot drawing process of pure titanium TA4 electronic product parts according to claim 1, characterized in that: Step six, perform wall reduction hot drawing treatment on the pure titanium TA4 seamless rectangular tube obtained in step five, and the wall reduction hot drawing deformation is controlled at 6-8%; step seven, repeat the wall reduction hot drawing treatment in step six 2-4 times, and the wall reduction hot drawing deformation is controlled at 6-8%; repeat the wall reduction hot drawing treatment in step six 2-4 times, and the wall reduction hot drawing deformation is controlled at 4-6%; repeat the wall reduction hot drawing treatment in step six 2-20 times, and the wall reduction hot drawing deformation is controlled at 2-4%; until the wall thickness of the obtained pure titanium TA4 seamless rectangular tube is reduced to 0.2-0.7 times the thickness of the pure titanium TA4 seamless rectangular tube in step five, perform ultrasonic surface cleaning treatment and drying in an environment of 50-70°C and pH 8-9 to obtain a finished pure titanium TA4 part.

Citation Information

Cited By

  • Temperature drawing preparation method and device for magnesium alloy thin-wall micro pipe

    CN119794103A

  • A method and device for warm drawing magnesium alloy thin-walled micro-tube

    CN119794103B

  • High-strength and high-plasticity TA4G alloy and double-temperature-zone stepped hot drawing preparation method thereof