Diamond bead string and preparation method thereof

By using epoxy resin, polyurethane and phenolic resin as adhesives in diamond beads, combined with antimony and molybdenum, and undergoing high temperature and high pressure treatment, the problem of uneven distribution of diamond beads and adhesive shedding is solved, and the stability of the beads is improved. durability and service life, achieving a stronger lamination structure.

CN118808634APending Publication Date: 2024-10-22QUANZHOU KEEN DIAMOND TOOL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410841756.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the existing diamond bead preparation method, the diamond distribution is uneven, the powder fluidity is poor, and the density deviation is large, resulting in eccentric wear during cutting and abnormal large and small beads, which reduces the service life. In addition, the adhesive easily falls off during the cold pressing process, and the internal structure is unstable. firm.

Method used

Epoxy resin, polyurethane and phenolic resin are used as adhesives. By mixing natural diamond powder, artificial diamond powder, antimony and molybdenum, and undergoing high temperature and high pressure treatment, the adhesive dissolves and liquefies at high temperatures, fills the gaps, and improves the interparticle quality. The contact area and bonding strength reduce gaps.

Benefits of technology

It achieves uniform distribution of diamond beads and improves internal density, enhances the stability and service life of the beads, avoids the problem of adhesive falling off, and forms a stronger lamination structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808634A_ABST
    Figure CN118808634A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of diamond beads, and discloses a diamond bead and a preparation method thereof, and the diamond bead comprises the following components by weight: 28-43% of natural diamond powder; 48%-63% of artificial diamond powder; 1%-2% of antimony; 1%-2% of molybdenum; 4%-6% of an adhesive; the adhesive is prepared by mixing one or two of epoxy resin, polyurethane and phenolic resin. According to the method, the blank is placed in the high-temperature and high-pressure environment, antimony and molybdenum are added to improve the physical property of diamond and play an important role in the heating process, antimony is firstly liquefied at the stage of 600-800 DEG C, diamond powder can be lubricated in the blank, the diamond powder can be more tightly combined, and therefore the diamond powder can be better lubricated. And subsequent liquefaction of molybdenum further lubricates the diamond particles, and gaps are effectively filled, so that the compactness and the bonding strength of the diamond string beads are improved, and the beneficial effects that the pressed diamond string beads do not depend on an adhesive, and bonding is firmer are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of diamond beads, in particular to a diamond bead and a preparation method thereof. Background Art

[0002] The preparation method of diamond beads is to press the mixed diamond powder into a green body by cold pressing, and then perform hot pressing, sintering, strengthening and welding. This preparation method has problems such as uneven distribution of diamonds in the beads, poor powder fluidity, and large density deviation, which leads to abnormalities such as eccentric wear and large and small beads during cutting of the diamond beads, reducing the service life of the diamond beads.

[0003] In order to solve the above technical problems, a diamond bead and its preparation method with publication number CN 116197397 A were found through searching. A layer of adhesive was sprayed on the surface of diamond to obtain a first treated material; the first treated material was fully mixed with the matrix powder to obtain a mixed powder; the mixed powder was dried and screened to obtain a second treated material; the second treated material was cold pressed to obtain a bead blank; the bead blank was sintered to obtain a diamond bead. The present application sprays an adhesive on the surface of diamond so that when the diamond is mixed with the matrix powder, the matrix powder can be evenly wrapped on the surface of the diamond, and the mixed powder after being fully mixed is dried and screened to ensure that the particle size of the screened mixed powder meets the requirements, and the mixed powder is cold pressed and sintered to obtain diamond beads, so that the diamond can be evenly distributed in the prepared diamond beads, the overall stability of the diamond beads is enhanced, and the service life of the diamond beads is improved.

[0004] Although the above technical solution uses cold pressing to solve the stability of diamond beads, the gaps between powders in the cold pressing process all rely on the pressure of the pressure equipment and the adhesive to bond, and the adhesive is wrapped around the outer surface of the diamond powder. When under pressure, the adhesive is easy to fall off from its surface. Even if it does not fall off from the surface of the diamond beads, the gaps between the powders inside the diamond beads are also tightly linked by pressure and cannot be penetrated by the adhesive. As a result, the cold-pressed diamond beads only have a bonded surface, and the internal structure is just a solid powder that is pressed together. Once the surface is broken, the interior will automatically disintegrate. Summary of the invention

[0005] 1. Technical issues to be solved

[0006] In view of the deficiencies in the prior art, the present invention provides a diamond bead and a preparation method thereof, which has the advantages that the pressed diamond beads do not rely on adhesives and the bonding is more firm, and there are no gaps between diamond powders to hinder pressing, thereby solving the problems of the above-mentioned technologies.

[0007] (II) Technical solution

[0008] To achieve the above object, the present invention provides the following technical solution: a diamond bead, comprising the following weight ratio formula:

[0009]

[0010] The adhesive is prepared by mixing one or two of epoxy resin, polyurethane and phenolic resin.

[0011] Preferably, the diamond beads include the following formula in weight ratio: 28% natural diamond powder, 63% artificial diamond powder, 2% antimony, 1% molybdenum and 6% adhesive, and other ingredients are inevitable impurities.

[0012] Preferably, natural diamond powder 43%, artificial diamond powder 48%, antimony 2%, molybdenum 2% and binder 5%, and other ingredients are inevitable impurities.

[0013] Preferably, natural diamond powder 38%, artificial diamond powder 54%, antimony 1.5%, molybdenum 1.5% and binder 5%, and other ingredients are inevitable impurities.

[0014] A method for preparing diamond beads, the method is used to prepare the fine steel stone beads according to claim 1, the method comprising the following steps:

[0015] Step 1: Mix natural diamond powder and artificial diamond powder in proportion to obtain diamond raw material powder;

[0016] Step 2: The prepared diamond powder is stirred again with antimony and molybdenum weighed in proportion until the antimony and molybdenum are thoroughly and evenly dispersed in the diamond powder;

[0017] Step 3, adding the binder to the diamond powder obtained in step 2 and stirring until the mixture is uniform to obtain a blank;

[0018] Step 4: Place the blank into the diamond bead mold and fully apply anti-stick coating on the mold to prevent adhesion;

[0019] Step 5: Stage heating to eliminate pores: Place the mold filled with the blank into the curing equipment for heating. In the first stage, the temperature is raised to 100℃-200℃ for 30S, in the second stage, the temperature is raised to 600℃-800℃ for 3-5min, and in the third stage, the temperature is raised to 3400℃.

[0020] Step 6: Apply 5GPa-10GPa pressure to the mold, hold the pressure for 1s-2s to press the blank into finished diamond beads, and take out the mold after the finished diamond beads cool down.

[0021] Preferably, the step 1 further comprises the following detailed steps:

[0022] S1.1. Place the weighed diamond powder into a mixing device, which is a rotary mixer, a V-type mixer or a double cone mixer;

[0023] S1.2, mix the natural diamond powder and the artificial diamond powder evenly at a speed of 30 rpm to 60 rpm and for 5 min to 8 min.

[0024] Preferably, the step 2 further comprises the following detailed steps:

[0025] S2.1, start the mixing equipment to mix the diamond raw material powder, antimony and molybdenum;

[0026] S2.1. After mixing, observe whether the color of the mixture is uniform, without obvious color blocks or color differences. If it meets the standard, it is confirmed to be evenly dispersed.

[0027] Preferably, the step three includes the following detailed steps:

[0028] S3.1. Prepare the diamond powder, antimony and molybdenum mixture in step 2, prepare a binder, and prepare a dry, clean container and stirring equipment;

[0029] S3.2, add the adhesive to the diamond powder mixture in step 2 according to the proportion, start the stirring device, and mix the diamond powder and the adhesive evenly.

[0030] Preferably, in the first stage of step five, the binder is dissolved at 100°C-200°C, the antimony is melted at 600°C-800°C in the second stage, and the liquefied antimony flows out of the blank to lubricate the natural diamond powder and artificial diamond powder in the blank, and the blank is further compacted by applying pressure with the mold. The molybdenum is melted at 3400°C in the third stage. At this time, the temperature is close to the melting point of the diamond powder, and the liquefied molybdenum plays a secondary lubrication role to lubricate the natural diamond powder and artificial diamond powder again to completely eliminate their gaps.

[0031] Preferably, the diamond cooling time in step six is ​​10 minutes.

[0032] Compared with the prior art, the present invention provides a diamond bead and a preparation method thereof, which has the following beneficial effects:

[0033] 1. The present invention places the blank under high temperature and high pressure environment, especially at the high temperature of 3400°C reached in the third stage, the surface of the diamond powder will liquefy, and this liquefaction helps the surface mutual diffusion between the diamond powders, thereby increasing the contact area between the particles at a microscopic level, improving the mechanical connection between the diamond particles, and no longer relying on adhesives. The addition of antimony and molybdenum is not only used to improve the physical properties of diamond, but also plays an important role in the heating process. Antimony first liquefies at the stage of 600°C-800°C, which helps to lubricate the diamond powder in the blank and make it more tightly combined. The subsequent liquefaction of molybdenum further lubricates the diamond particles and effectively fills the gaps, thereby improving the density and bonding strength of the diamond beads, achieving the beneficial effect that the pressed diamond beads do not rely on adhesives and are more firmly bonded.

[0034] 2. In the present invention, during the staged heating process in step 5, the diamond powder is affected by high temperature, so that the adhesive is dissolved in the first stage (100°C-200°C), the antimony is melted in the second stage (600°C-800°C), and the molybdenum is melted in the third stage (3400°C). The liquefaction under these high temperature conditions helps the microscopic surface diffusion between the diamond powders and fills the possible gaps, thereby improving the density of the diamond beads. The added antimony and molybdenum are liquefied successively at high temperatures, which not only physically lubricates the diamond powder particles, making it easier to combine tightly during the pressing process, but also fills any tiny gaps. The presence of these elements effectively reduces the gaps between the diamond powders, ensures a good pressing effect under high pressure treatment, and achieves the beneficial effect that there are no gaps between the diamond powders to hinder pressing. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic diagram of the process of the present invention; DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] See also Figure 1 , a diamond bead comprising the following formula in weight ratio:

[0038]

[0039] The adhesive is prepared by mixing one or two of epoxy resin, polyurethane and phenolic resin.

[0040] Embodiment 1

[0041] The diamond beads include the following formula in weight ratio: 28% natural diamond powder, 63% artificial diamond powder, 2% antimony, 1% molybdenum and 6% adhesive, and other ingredients are inevitable impurities.

[0042] 28% natural diamond powder and 63% artificial diamond powder are mixed evenly in proportion to ensure the uniformity of the diamond powder in the raw materials, laying the foundation for subsequent processing steps. Next, 2% antimony and 1% molybdenum are added to the diamond powder and evenly dispersed by stirring. The addition of antimony and molybdenum helps to improve the physical properties of diamond, especially during high-temperature lubrication. The liquefaction of antimony and molybdenum helps to fill potential tiny gaps and improve the bonding strength and density between diamond particles. The adhesive accounts for 6%. The selected adhesives include a mixture of epoxy resin, polyurethane or phenolic resin. The role of the adhesive is to solidify and stabilize the bonding of the diamond powder before heating and high-pressure treatment, and then it will melt and be removed at high temperature.

[0043] Embodiment 2

[0044] Natural diamond powder 43%, artificial diamond powder 48%, antimony 2%, molybdenum 2% and adhesive 5%, other ingredients are inevitable impurities.

[0045] Natural diamond powder accounts for 43%, artificial diamond powder accounts for 48%, antimony accounts for 2%, molybdenum accounts for 2%, and binder accounts for 5%. Compared with the previous formula, the ratio of natural diamond powder and artificial diamond powder is adjusted, and the content of antimony and molybdenum is slightly adjusted. At the same time, the amount of binder used is reduced. The blank undergoes a high temperature and high pressure treatment process, including the liquefaction of the binder and metal elements, to ensure that there are no gaps between the diamond powders, thus forming a solid, high-quality diamond bead product.

[0046] Embodiment 3

[0047] Natural diamond powder 38%; artificial diamond powder 54%, antimony 1.5%, molybdenum 1.5% and adhesive 5%, other ingredients are inevitable impurities.

[0048] 38% natural diamond powder and 54% artificial diamond powder are evenly mixed to ensure the uniformity and stability of the diamond powder in the raw materials. 1.5% antimony and 1.5% molybdenum are added to the diamond powder and properly stirred to ensure its uniform dispersion. These additives fill the tiny gaps that may exist during the high-temperature lubrication process and enhance the bonding force and density between the diamond particles.

[0049] A method for preparing diamond beads, the method is used to prepare the fine steel stone beads according to claim 1, the method comprising the following steps:

[0050] Step 1: Mix natural diamond powder and artificial diamond powder in proportion to obtain diamond raw material powder;

[0051] Step 2: The prepared diamond powder is stirred again with antimony and molybdenum weighed in proportion until the antimony and molybdenum are thoroughly and evenly dispersed in the diamond powder;

[0052] Step 3, adding the binder to the diamond powder obtained in step 2 and stirring until the mixture is uniform to obtain a blank;

[0053] Step 4: Place the blank into the diamond bead mold and fully apply anti-stick coating on the mold to prevent adhesion;

[0054] Step 5: Stage heating to eliminate pores: Place the mold filled with the blank into the curing equipment for heating. In the first stage, the temperature is raised to 100℃-200℃ for 30S, in the second stage, the temperature is raised to 600℃-800℃ for 3-5min, and in the third stage, the temperature is raised to 3400℃.

[0055] Step 6: Apply 5GPa-10GPa pressure to the mold, hold the pressure for 1s-2s to press the blank into finished diamond beads, and take out the mold after the finished diamond beads cool down.

[0056] Natural diamond is one of the hardest substances on earth. Its crystal texture is more perfect and its crystal clarity is higher. Therefore, it may have higher value and beauty in some applications. Compared with natural diamond, artificial diamond is cheaper and suitable for large-scale production and application. The crystal texture of artificial diamond powder is relatively uniform and the quality is stable, which can ensure the consistency of the product. The combination of natural diamond powder and artificial diamond powder ensures the beauty of diamond beads while reducing their production costs, which is conducive to large-scale production.

[0057] Specifically, the step 1 also includes the following detailed steps:

[0058] S1.1. Place the weighed diamond powder into a mixing device, which is a rotary mixer, a V-type mixer or a double cone mixer;

[0059] S1.2, mix the natural diamond powder and the artificial diamond powder evenly at a speed of 30 rpm to 60 rpm and for 5 min to 8 min.

[0060] Specifically, the step 2 also includes the following detailed steps:

[0061] S2.1, start the mixing equipment to mix the diamond raw material powder, antimony and molybdenum;

[0062] S2.1. After mixing, observe whether the color of the mixture is uniform, without obvious color blocks or color differences. If it meets the standard, it is confirmed to be evenly dispersed.

[0063] Specifically, the step three includes the following detailed steps:

[0064] S3.1. Prepare the diamond powder, antimony and molybdenum mixture in step 2, prepare a binder, and prepare a dry, clean container and stirring equipment;

[0065] S3.2, add the adhesive to the diamond powder mixture in step 2 according to the proportion, start the stirring device, and mix the diamond powder and the adhesive evenly.

[0066] Specifically, in the first stage of step five, the adhesive is dissolved at 100°C-200°C, the antimony is melted at 600°C-800°C in the second stage, and the liquefied antimony flows out of the blank to lubricate the natural diamond powder and the artificial diamond powder in the blank, and the blank is further compacted by applying pressure with the mold. In the third stage, molybdenum is melted at 3400°C, and the temperature is close to the melting point of the diamond powder. The liquefied molybdenum plays a secondary lubrication role to lubricate the natural diamond powder and the artificial diamond powder again to completely eliminate their gaps.

[0067] Specifically, the diamond cooling time in step six is ​​10 minutes.

[0068] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A diamond bead, It is characterized in that A formulation comprising the following weight ratios: The adhesive is prepared by mixing one or two of epoxy resin, polyurethane and phenolic resin.

2. A diamond bead according to claim 1, Features: The diamond beads include the following formula in weight ratio: 28% natural diamond powder, 63% artificial diamond powder, 2% antimony, 1% molybdenum and 6% adhesive, and other ingredients are inevitable impurities.

3. A diamond bead according to claim 1, Features: Natural diamond powder 43%, artificial diamond powder 48%, antimony 2%, molybdenum 2% and adhesive 5%, other ingredients are inevitable impurities.

4. A diamond bead according to claim 1, Features: Natural diamond powder 38%; artificial diamond powder 54%, antimony 1.5%, molybdenum 1.5% and adhesive 5%, other ingredients are inevitable impurities.

5. A method for preparing diamond beads, Features: The preparation method is used to prepare the fine steel stone beads according to claim 1, and the preparation method comprises the following steps: Step 1: Mix natural diamond powder and artificial diamond powder in proportion to obtain diamond raw material powder; Step 2: The prepared diamond powder is stirred again with antimony and molybdenum weighed in proportion until the antimony and molybdenum are thoroughly and evenly dispersed in the diamond powder; Step 3, adding the binder to the diamond powder obtained in step 2 and stirring until the mixture is uniform to obtain a blank; Step 4: Place the blank into the diamond bead mold and fully apply anti-stick coating on the mold to prevent adhesion; Step 5: Stage heating to eliminate pores: Place the mold filled with the blank into the curing equipment for heating. In the first stage, the temperature is raised to 100℃-200℃ for 30S, in the second stage, the temperature is raised to 600℃-800℃ for 3-5min, and in the third stage, the temperature is raised to 3400℃. Step 6: Apply 5GPa-10GPa pressure to the mold, hold the pressure for 1s-2s to press the blank into finished diamond beads, and take out the mold after the finished diamond beads cool down.

6. A method for preparing diamond beads according to claim 1, Features: The step 1 also includes the following detailed steps: S1.

1. Place the weighed diamond powder into a mixing device, which is a rotary mixer, a V-type mixer or a double cone mixer; S1.2, mix the natural diamond powder and the artificial diamond powder evenly at a speed of 30 rpm to 60 rpm and for 5 min to 8 min.

7. A method for preparing diamond beads according to claim 1, Features: The step 2 also includes the following detailed steps: S2.1, start the mixing equipment to mix the diamond raw material powder, antimony and molybdenum; S2.

1. After mixing, observe whether the color of the mixture is uniform, without obvious color blocks or color differences. If it meets the standard, it is confirmed to be evenly dispersed.

8. A method for preparing diamond beads according to claim 1, Features: The step three includes the following detailed steps: S3.

1. Prepare the diamond powder, antimony and molybdenum mixture in step 2, prepare a binder, and prepare a dry, clean container and stirring equipment; S3.2, add the adhesive to the diamond powder mixture in step 2 according to the proportion, start the stirring device, and mix the diamond powder and the adhesive evenly.

9. A method for preparing diamond beads according to claim 1, Features: In the step 5, the first stage is to dissolve the adhesive at 100°C-200°C, the second stage is to melt antimony at 600°C-800°C, and the liquefied antimony flows out of the blank to lubricate the natural diamond powder and artificial diamond powder in the blank, and the blank is further compacted by applying pressure with the mold. The third stage is to melt molybdenum at 3400°C. At this time, the temperature is close to the melting point of diamond powder. The liquefied molybdenum plays a secondary lubrication role to lubricate the natural diamond powder and artificial diamond powder again to completely eliminate their gaps.

10. A method for preparing diamond beads according to claim 1, Features: The diamond cooling time in step 6 is 10 minutes.