Method for preparing high-toughness hard alloy based on coating structure powder

The coating structure powder is prepared through the principle of electrostatic self-assembly, which solves the problem of synergistic improvement of hardness, toughness and strength in cemented carbide, realizes the comprehensive performance improvement of cemented carbide, and solves the problem of synergistic improvement of performance that is difficult to achieve by conventional methods, and the process It is simple, easy to implement and easy to be industrialized.

CN118808636APending Publication Date: 2024-10-22BEIJING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410822586.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

It is difficult to synergistically improve hardness, toughness and strength in cemented carbide with existing technology, and it is difficult to achieve uniform improvement of these three performance indicators using conventional methods.

Method used

The principle of electrostatic self-assembly is used to prepare coated structural powder in a rotating drum. By granulating powders with different characteristics in stages and adjusting the proportion of powder, a composite powder with a core and surface layer composed of powders with different characteristics is formed to achieve the hardness of cemented carbide. , the synergistic improvement of toughness and strength.

Benefits of technology

It achieves excellent comprehensive performance of cemented carbide, solves the bottleneck problem of performance synergy improvement that is difficult to achieve with conventional methods, and the process is simple and easy to implement and easy to industrialize.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004909499160000061
    Figure BDA0004909499160000061
  • Figure HDA0004909499300000011
    Figure HDA0004909499300000011
  • Figure HDA0004909499300000012
    Figure HDA0004909499300000012
Patent Text Reader

Abstract

The invention discloses a method for preparing high-toughness hard alloy based on coating structure powder, and belongs to the technical field of powder metallurgy. The preparation method comprises the following steps: preparing spherical powder from 12wt.% of WC-Co-0. 25wt.% of (Cr, V) 2 (C, N) composite powder with the average particle size of 100-250nm, adding 12wt.% of WC-Co-0. 86wt.% of Cr3C2 and 0.25 wt.% of VC powder with the average particle size of 100-250nm into the spherical powder, carrying out rotary granulation through a roller to prepare coated structure powder, and carrying out cold press forming and low-pressure sintering to obtain the high-toughness hard alloy. According to the method, the alloy hardness, toughness and strength of the hard alloy are synergistically improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder metallurgy, and in particular relates to a method for preparing high-strength and tough cemented carbide based on coated structure powder. Background Art

[0002] Cemented carbide represented by WC-Co is a metal-ceramic composite material prepared by powder metallurgy. It is widely used in the processing and manufacturing of cutting tools, mining tools, wear-resistant parts and other products due to its excellent comprehensive mechanical properties such as high hardness, high wear resistance, good toughness and high strength. With the increasingly complex and harsh application conditions, further improving the basic properties of cemented carbide materials such as hardness, toughness and strength is an important prerequisite for the corresponding products to obtain a long service life.

[0003] However, a large number of research results have confirmed that there is an exclusive relationship between hardness, toughness and strength. For example, improving toughness and strength often leads to a significant decrease in hardness, while improving hardness and strength leads to a decrease in toughness. It is difficult to achieve a synergistic improvement in the three performance indicators using conventional methods. Existing research and engineering practice results have shown that through the comprehensive regulation of raw material powder properties (metal phase content, carbon content, oxygen content, particle size distribution, etc.) and forming and sintering processes (forming agent type and content, compact density, sintering temperature and atmosphere pressure, etc.), some performance indicators can be significantly improved, but the cemented carbide with "uniform structure" obtained often still has shortcomings in a certain performance indicator.

[0004] In view of the above problems, in order to obtain cemented carbide materials with better comprehensive performance, the present invention proposes the design concept of "coated structured powder", that is, in the granulation stage of the raw material powder, two or more powders with different characteristics (the cemented carbides prepared thereby have outstanding mechanical properties in some aspects) are granulated in stages to achieve the coating of one by another, and by adjusting the proportion of each powder in the obtained coated powder, the synergistic improvement of the hardness, toughness and strength of the prepared cemented carbide is achieved. Summary of the invention

[0005] The process flow and principle of the preparation method provided by the present invention are: based on the principle of electrostatic self-assembly, the WC-Co based powder containing the binder is spontaneously agglomerated into spherical particles in a rotating drum; using this granulation process, firstly, the A type powder is subjected to rotational granulation, the size of the agglomerated particles is regulated by controlling the rotation time, and then the B type powder is added, and the rotational granulation is continued to gradually coat the surface of the A type powder, forming a coating structure composite powder in which the "core" and "surface" are respectively composed of powders with different characteristics. For example, when the cemented carbide prepared from the A type powder alone has high hardness and strength, and the cemented carbide prepared from the B type powder alone has high toughness and strength, the cemented carbide with a "uniform heterogeneous structure" prepared by coating the two powders together will obtain simultaneously improved hardness, toughness and strength. This method can design the raw material powder with high freedom according to needs, effectively solving the bottleneck problem that conventional methods are difficult to achieve synergistic improvement of the comprehensive performance of cemented carbide, and the method is simple and easy to implement, and easy to realize industrialization.

[0006] The present invention provides a method for preparing high-strength and tough cemented carbide based on coated structure powder, characterized in that it comprises the following steps:

[0007] (1) a composite powder having an average particle size of 100-250 nm (preferably 190 nm) and a composition of WC-12wt.%Co-0.25wt.%(Cr,V)2(C,N) is mixed with polyethylene glycol and anhydrous ethanol and ball-milled for 3-5 hours, dried and sieved through an 80-mesh sieve, and then rotary granulated in a cylinder, wherein the amount of polyethylene glycol added is 2%-3% of the mass of the composite powder, the cylinder rotation rate is 30-50 r / min, and the rotation time is 30-60 min to obtain a spherical powder;

[0008] (2) a composite powder having an average particle size of 100-250 nm (preferably 190 nm) and a composition of WC-12wt.%Co-0.86wt.%Cr3C2-0.25wt.%VC is mixed with polyethylene glycol and anhydrous ethanol and ball-milled for 3-5 hours, and then dried and sieved through an 80-mesh sieve, wherein the amount of polyethylene glycol added is 2%-3% of the mass of the composite powder;

[0009] (3) adding the sieved powder of step (2) to the spherical powder obtained in step (1) for secondary rotary granulation, the drum rotating speed is 30-50 r / min, the rotating time is 30-60 min, and a spherical powder with an average particle size of 0.30-0.85 mm is obtained, and the powder added in step (3) accounts for 20%-80% of the total mass of the powder (i.e., the total mass of the spherical powder in step 1 and the sieved powder in step 2);

[0010] (4) The coating structure powder prepared in step (3) is cold pressed to form a green body with a density of 7.5-8.0 g / cm 3, and then sintered and densified at a temperature of 1400-1410°C. When the furnace temperature rises to the target temperature, 5-6MPa argon is introduced and kept warm for 80 minutes. Then, it is naturally cooled to 1000°C and rapid cooling is started. When the furnace temperature drops to 80°C, the argon is discharged and cooled to room temperature to obtain a cemented carbide with synergistically improved hardness, toughness and strength. The rapid cooling process described here is that the time from 1000°C to 80°C is 100-150min.

[0011] The technical features and advantages of the method of the present invention are mainly as follows: (1) The innovative design concept of granulation based on the principle of electrostatic self-assembly so that the powder has a "coating structure" can realize the preparation of cemented carbide with uniform heterogeneous structure and excellent comprehensive performance, and can also be expanded to the design and preparation of other high-performance powder metallurgy materials; (2) By optimizing the composition and proportion of raw material powders with different characteristics in the coating structure powder, the synergistic improvement of the hardness, toughness and strength of the prepared cemented carbide is achieved; (3) The bottleneck problem that conventional methods are difficult to achieve synergistic improvement of the comprehensive performance of cemented carbide is solved. The method is simple and easy to implement and easy to realize industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 Schematic diagram of the preparation process principle of the coated structure powder in the present invention;

[0013] Figure 2 The present invention discloses a scanning electron microscope (SEM) morphology and grain size distribution diagram of the WC-Co cemented carbide prepared in accordance with the present invention; wherein, (a) is a SEM morphology and grain size distribution diagram of the WC-Co cemented carbide prepared in Example 1, (b) is a SEM morphology and grain size distribution diagram of the WC-Co cemented carbide prepared in Example 2, (c) is a SEM morphology and grain size distribution diagram of the WC-Co cemented carbide prepared in Comparative Example 1, and (d) is a SEM morphology and grain size distribution diagram of the WC-Co cemented carbide prepared in Comparative Example 2.

[0014] Table 1 shows the mechanical properties of the WC-Co cemented carbide prepared by the present invention. DETAILED DESCRIPTION

[0015] The following examples further explain the present invention, but the present invention is not limited to the following examples. The following examples are all based on the preparation of WC-12wt.%Co cemented carbide as an example.

[0016] Example 1

[0017] (1) A composite powder with an average particle size of 190 nm and a composition of WC-12wt.%Co-0.25wt.%(Cr,V)2(C,N) was mixed with polyethylene glycol and anhydrous ethanol and ball-milled for 3 h, dried and sieved through an 80-mesh sieve, and then rotary granulated in a cylinder. The amount of polyethylene glycol added was 2% of the powder mass, the cylinder rotation rate was 40 r / min, and the rotation time was 30 min;

[0018] (2) a composite powder having an average particle size of 190 nm and a composition of WC-12wt.%Co-0.86wt.%Cr3C2-0.25wt.%VC was mixed with polyethylene glycol and anhydrous ethanol and ball-milled for 3 h, and then dried and sieved through an 80-mesh sieve. The amount of polyethylene glycol added was 2% of the powder mass;

[0019] (3) adding the sieved powder of step (2) to the spherical powder obtained in step (1) for secondary rotary granulation, the drum rotating speed is 40 r / min, the rotating time is 30 min, and a spherical powder with an average particle size of 0.5 mm is obtained, and the powder added in step (3) accounts for 80% of the total mass of the powder;

[0020] (4) The coating structure powder prepared in step (3) is cold pressed to form a green body with a density of 7.7 g / cm 3 , and then sintered and densified at 1410℃. When the furnace temperature rises to the target temperature, 5MPa of high-purity argon is introduced and kept warm for 80min. Then, when it cools to 1000℃, rapid cooling is started. When the furnace temperature drops to 80℃, argon is discharged. After cooling to room temperature, a cemented carbide with high comprehensive performance is obtained. Its scanning electron microscope morphology is as follows Figure 2 As shown in (a), the properties are shown in Table 1. It can be seen that its hardness, toughness and strength are further improved compared with the single-component cemented carbide prepared in Comparative Example 1.

[0021] Example 2

[0022] (1) A composite powder with an average particle size of 190 nm and a composition of WC-12wt.%Co-0.25wt.%(Cr,V)2(C,N) was mixed with polyethylene glycol and anhydrous ethanol and ball-milled for 3 h, dried and sieved through an 80-mesh sieve, and then rotary granulated in a cylinder. The amount of polyethylene glycol added was 2% of the powder mass, the cylinder rotation rate was 40 r / min, and the rotation time was 30 min;

[0023] (2) a composite powder having an average particle size of 190 nm and a composition of WC-12wt.%Co-0.86wt.%Cr3C2-0.25wt.%VC was mixed with polyethylene glycol and anhydrous ethanol and ball-milled for 3 h, and then dried and sieved through an 80-mesh sieve. The amount of polyethylene glycol added was 2% of the powder mass;

[0024] (3) adding the sieved powder of step (2) to the spherical powder obtained in step (1) for secondary rotary granulation, the drum rotating speed is 40 r / min, the rotating time is 30 min, and a spherical powder with an average particle size of 0.5 mm is obtained, and the powder added in step (3) accounts for 20% of the total mass of the powder;

[0025] (4) The coating structure powder prepared in step (3) is cold pressed to form a green body with a density of 7.7 g / cm 3 , and then sintered and densified at 1410℃. When the furnace temperature rises to the target temperature, 5MPa of high-purity argon is introduced and kept warm for 80min. Then, when it cools to 1000℃, rapid cooling is started. When the furnace temperature drops to 80℃, argon is discharged. After cooling to room temperature, a cemented carbide with high comprehensive performance is obtained. Its scanning electron microscope morphology is as follows Figure 2 As shown in (b), the properties are shown in Table 1. It can be seen that its hardness and strength are further improved compared with the single-component cemented carbide prepared in Comparative Example 2.

[0026] Comparative Example 1

[0027] A composite powder with an average particle size of 190 nm and a composition of WC-12wt.%Co-0.86wt.%Cr3C2-0.25wt.%VC was mixed with polyethylene glycol and anhydrous ethanol and ball-milled for 3 hours. After drying, the powder was passed through an 80-mesh sieve, and the amount of polyethylene glycol added was 2% of the powder mass. The sieved powder was placed in a cylinder for rotary granulation. The cylinder rotation rate was 40r / min and the rotation time was 60min to obtain a spherical powder with an average particle size of 0.5mm. The spherical powder was pressed into a green body with a green body density of 7.72g / cm 3 Then, it was sintered and densified at 1410°C. When the furnace temperature reached the target temperature, 5MPa of argon was introduced and kept warm for 80min. Then, it was cooled to 1000°C and rapid cooling was started. When the furnace temperature dropped to 80°C, the argon was discharged and cooled to room temperature to obtain a cemented carbide with a composition of WC-12wt.%Co-0.86wt.%Cr3C2-0.25wt.%VC. The SEM morphology and grain size distribution are shown in Figure 2 (c), mechanical properties are shown in Table 1.

[0028] Comparative Example 2

[0029] A composite powder with an average particle size of 190 nm and a composition of WC-12wt.%Co-0.25wt.%(Cr,V)2(C,N) was mixed with polyethylene glycol and anhydrous ethanol and ball-milled for 3 hours. After drying, the powder was sieved through an 80-mesh sieve, and the amount of polyethylene glycol added was 2% of the powder mass. The sieved powder was placed in a cylinder for rotary granulation. The cylinder rotation rate was 40r / min and the rotation time was 60min to obtain a spherical powder with an average particle size of 0.5mm. The spherical powder was pressed into a green body with a green body density of 7.72g / cm 3 , and then sintered and densified at 1410℃. When the furnace temperature rises to the target temperature, 5MPa argon is introduced and kept warm for 80min. Then, rapid cooling is started when the furnace temperature is cooled to 1000℃. When the furnace temperature drops to 80℃, argon is discharged. After cooling to room temperature, a cemented carbide with a composition of WC-12wt.%Co-0.25wt.%(Cr,V)2(C,N) is obtained. The SEM morphology and grain size distribution are shown in Figure 2 (d), mechanical properties are shown in Table 1.

[0030] Table 1 Mechanical properties of WC-Co cemented carbides prepared based on different powders in different embodiments

[0031]

Claims

1. A method for preparing high-strength and tough cemented carbide based on coated structure powder, characterized in that: The following steps are involved: (1) a composite powder having an average particle size of 100-250 nm and a composition of WC-12wt.%Co-0.25wt.%(Cr,V)2(C,N) is mixed with polyethylene glycol and anhydrous ethanol and ball-milled for 3-5 hours, dried and sieved through an 80-mesh sieve, and then rotary granulated in a cylinder, wherein the amount of polyethylene glycol added is 2%-3% of the mass of the composite powder, the cylinder rotation rate is 30-50r / min, and the rotation time is 30-60min to obtain a spherical powder; (2) a composite powder having an average particle size of 100-250 nm and a composition of WC-12wt.%Co-0.86wt.%Cr3C2-0.25wt.%VC is mixed with polyethylene glycol and anhydrous ethanol and ball-milled for 3-5 hours, and then dried and sieved through an 80-mesh sieve, wherein the amount of polyethylene glycol added is 2%-3% of the mass of the composite powder; (3) adding the sieved powder of step (2) to the spherical powder obtained in step (1) for secondary rotary granulation, the drum rotating speed is 30-50 r / min, the rotating time is 30-60 min, and a spherical powder with an average particle size of 0.30-0.85 mm is obtained, and the powder added in step (3) accounts for 20%-80% of the total mass of the powder; (4) The coating structure powder prepared in step (3) is cold pressed to form a green body with a density of 7.5-8.0 g / cm 3 , and then sinter and densify at 1400-1410℃. When the furnace temperature rises to the target temperature, 5-6MPa argon is introduced and kept warm for 80 minutes. Then, rapid cooling is started when it is cooled to 1000℃. When the furnace temperature drops to 80℃, the argon is discharged. After cooling to room temperature, a cemented carbide with synergistically improved hardness, toughness and strength is obtained.

2. A method for preparing high-strength and tough cemented carbide based on coated structure powder according to claim 1, characterized in that: The average particle size of the composite powder in step (1) is 190 nm; the average particle size of the composite powder in step (2) is 190 nm.

3. A method for preparing high-strength and tough cemented carbide based on coated structure powder according to claim 1, characterized in that: The rapid cooling process in step (4) is a process of cooling the temperature from 1000°C to 80°C for 100-150 minutes.

4. A high-strength and tough cemented carbide prepared according to the method described in any one of claims 1 to 3.