Welding rod for welding thermal strength steel and preparation method of welding rod
By using a specific combination of coating and welding core in the welding rod, combined with the slag-making and gas-making functions at arc temperature, the problems of temper embrittlement and low-temperature toughness reduction in the welding of hot-strength steel are solved, and the welding seam is improved. High strength and toughness, suitable for manufacturing high temperature and high pressure equipment.
Patent Information
- Application Number
- CN202411056451.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-02
AI Technical Summary
Under high temperature and high pressure conditions, welds of hot-strength steel are prone to temper embrittlement and reduced low-temperature toughness.
Using a method including marble, calcium fluoride, graphite, silica powder, rutile, 45 ferrosilicon, low carbon ferromanganese, microcarbon ferrochromium, molybdenum powder, ferrovanadium, reduced iron powder, potassium chloride, synthetic mica and rare earth silicon Iron The electrode with coating and low-sulfur and low-phosphorus H08 steel core welding core improves the strength and toughness of the weld through the slagging and gas-generating functions at arc temperature, combined with the addition of chromium, molybdenum, carbon, rare earth ferrosilicon and vanadium elements. .
It improves the porosity resistance, strength and toughness of the weld, ensuring high toughness of the weld metal, and is suitable for the manufacture of high temperature and high pressure equipment such as hydrogenation reactors.
Smart Images

Figure CN118808985A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of welding materials, and in particular to a welding rod for heat-resistant steel welding and a preparation method thereof. Background Art
[0002] With the research of science and technology, my country's chemical industry has been vigorously developed, and hydrogenation reactors have been used more and more widely. Hydrogenation reactors are the core equipment of the hydrocracking process of petroleum refining equipment and are major key equipment in modern oil refining. Usually, the working temperature of hydrogenation reactors is generally above 400°C and the working pressure is about 20Mpa. Because heat-resistant steel has excellent high-temperature strength, oxidation resistance, corrosion resistance, good organizational stability and weldability, it has become an ideal material for manufacturing high-temperature and high-pressure equipment such as hydrogenation reactors, such as 2.25Cr-1Mo-0.25V steel. However, the supporting welding materials required for the manufacturing process of hydrogenation reactors have long relied on imports, which has become a link restricting the complete localization of hydrogenation reactor manufacturing. Under high temperature and high pressure conditions, the welds welded by heat-resistant steel are prone to failure in the form of temper embrittlement and reduced low-temperature toughness. Summary of the invention
[0003] In view of the above shortcomings of the prior art, the present invention provides a welding rod for heat-resistant steel welding and a preparation method thereof, so as to improve the problem that the weld layer is prone to temper embrittlement and low-temperature toughness reduction.
[0004] To achieve the above-mentioned object and other related objects, the present invention provides a welding rod for heat-resistant steel welding, comprising a welding core and a coating, wherein the coating comprises the following components and the weight proportions of each component are respectively: 10-13 parts of marble, 3-5 parts of calcium fluoride, 0.2-0.5 parts of graphite, 1-2 parts of silicon micropowder, 1-2 parts of rutile, 1-2 parts of 45 ferrosilicon, 0.5-1.5 parts of low-carbon ferromanganese, 9-12 parts of micro-carbon ferrochrome, 1-2 parts of molybdenum powder, 0.2-0.5 parts of ferrovanadium, 35-50 parts of reduced iron powder, 0.3-0.6 parts of potassium chloride, 0.3-0.6 parts of synthetic mica, and 0.5-1.5 parts of rare earth ferrosilicon.
[0005] In one example of the present invention, the calcium carbonate content in the marble is ≥96wt%; the silicon dioxide content in the silicon micropowder is ≥98wt%; the manganese content in the low-carbon ferromanganese is ≥80wt%; the chromium content in the micro-carbon ferrochrome is ≥70wt%, and the carbon content is ≤0.06wt%; the molybdenum content in the molybdenum powder is ≥99wt%; the vanadium content in the ferrovanadium is 50-55wt%; the iron content in the reduced iron powder is ≥98wt%;
[0006] In an example of the present invention, the particle sizes of the graphite, the silicon powder and the rare earth ferrosilicon are 80-120 meshes, and the particle sizes of the remaining components are 40-80 meshes.
[0007] In an example of the present invention, the welding core is made of a low-sulfur and low-phosphorus H08 steel core, and the P content of the welding core is ≤0.015wt%, and the S content is ≤0.010wt%.
[0008] In an example of the present invention, the diameter of the welding core is 3.2-5.0 mm.
[0009] The present invention also provides a method for preparing a welding rod for heat-resistant steel welding, comprising the following steps: weighing various components of the coating according to a ratio and mixing them evenly to obtain a coating powder; adding a binder to the coating powder and stirring evenly to form a coating mixture; pressing the coating mixture onto the surface of the welding core and drying it to obtain the welding rod for heat-resistant steel welding.
[0010] In one example of the present invention, the binder is a water glass binder, and the mass of the binder is 23-25% of the total mass of the coating powder.
[0011] In one example of the present invention, the weight of the coating mixture in the heat-resistant steel welding electrode after drying is 40-45% of the total weight of the heat-resistant steel welding electrode.
[0012] In an example of the present invention, the pressure during the pressure coating is 9-15 MPa.
[0013] In an example of the present invention, the drying temperature is 280-350° C., and the drying time is 1-2 hours.
[0014] The welding rod for heat-resistant steel welding of the present invention adopts an alkaline slag system to ensure that the weld has a low oxygen content and ensures high toughness of the weld metal; marble is added to the coating to play a slag-making and gas-making function at the arc temperature, which can improve the anti-porosity performance of the welding rod; low-carbon ferromanganese, micro-carbon ferrochrome, 45 ferrosilicon, ferrovanadium, molybdenum powder, and graphite are added to the weld to infiltrate alloys, wherein chromium, molybdenum, and carbon elements can improve the strength of the weld, and rare earth ferrosilicon, molybdenum, and vanadium elements can refine the structure of the deposited metal and improve the toughness of the weld. The welding rod for heat-resistant steel welding prepared by the present invention has a smooth surface, good pressure coating, high deposition rate, and strong strength, toughness, and crack resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0016] Figure 1 The present invention is a flow chart of the preparation of the welding rod for heat-resistant steel welding. DETAILED DESCRIPTION
[0017] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.
[0018] It should be noted that "%" and "wt%" in this specification represent mass percentage, and "part" represents part by weight.
[0019] The welding rod for heat-resistant steel welding of the present invention comprises a welding core and a coating, wherein the coating comprises the following components and the weight proportions of the components are respectively: 10-13 parts of marble, 3-5 parts of calcium fluoride, 0.2-0.5 parts of graphite, 1-2 parts of silicon micropowder, 1-2 parts of rutile, 1-2 parts of 45 ferrosilicon, 0.5-1.5 parts of low-carbon ferromanganese, 9-12 parts of micro-carbon ferrochrome, 1-2 parts of molybdenum powder, 0.2-0.5 parts of ferrovanadium, 35-50 parts of reduced iron powder, 0.3-0.6 parts of potassium chloride, 0.3-0.6 parts of synthetic mica and 0.5-1.5 parts of rare earth ferrosilicon.
[0020] The functions of each component in the drug skin are as follows:
[0021] Marble: It mainly plays the role of gasification and providing alkaline slag. The calcium carbonate content in marble is ≥96wt%. During the welding process, calcium carbonate decomposes into calcium oxide and carbon dioxide gas. The generated carbon dioxide can keep the molten pool in inert gas protection. The weight proportion of marble in the coating of the present invention is 10 to 13 parts. For example, the weight proportion of marble can be any value within the range of 10 to 13 parts, such as 10 parts, 11 parts, 12 parts or 13 parts.
[0022] Calcium fluoride: mainly plays a role in slag formation. During the welding process, calcium can play a role in deoxidation and desulfurization, and fluorine can play a role in dehydrogenation and purification of the deposited metal. The weight proportion of calcium fluoride in the coating of the present invention is 3 to 5 parts, for example, the weight proportion of calcium fluoride can be any value within the range of 3 to 5 parts, such as 3 parts, 3.5 parts, 4 parts or 5 parts.
[0023] Graphite: Its main function is to transfer carbon elements to the deposited metal, thereby increasing the hardness of the deposited metal. It can also deoxidize and improve the pressure-coating properties, but too much graphite will increase spatter. The weight percentage of graphite in the coating of the present invention is 0.2 to 0.5 parts, for example, the weight percentage of graphite can be any value within the range of 0.2 to 0.5 parts, such as 0.2 parts, 0.25 parts, 0.4 parts or 0.5 parts.
[0024] Silicon powder: The silicon dioxide content in the silicon powder is ≥98wt%, which is mainly used for slag making and can adjust the melting point and tension of the welding slag. The weight proportion of silicon powder in the coating of the present invention is 1 to 2 parts, for example, the weight proportion of silicon powder can be any value within the range of 1 to 2 parts, such as 1 part, 1.5 parts or 2 parts.
[0025] Rutile: The main component of rutile is titanium dioxide, which can stabilize the arc, reduce spatter, and improve slag removal when used with other slag-forming agents. The weight percentage of rutile in the coating of the present invention is 1 to 2 parts. For example, the weight percentage of rutile can be any value within the range of 1 to 2 parts, such as 1 part, 1.5 parts, 1.8 parts or 2 parts.
[0026] 45 ferrosilicon: mainly used as a deoxidizer and alloying agent. Too much ferrosilicon will increase spatter and reduce toughness. The weight percentage of 45 ferrosilicon in the coating of the present invention is 1 to 2 parts. For example, the weight percentage of 45 ferrosilicon can be any value within the range of 1 to 2 parts, such as 1 part, 1.5 parts or 2 parts.
[0027] Low carbon ferromanganese: mainly used as a deoxidizer, alloying agent and desulfurizer, and excessive content thereof will increase splashing. The weight proportion of low carbon ferromanganese in the coating of the present invention is 0.5 to 1.5 parts, for example, the weight proportion of low carbon ferromanganese can be any value within the range of 0.5 to 1.5 parts, such as 0.5 parts, 0.8 parts, 1 part or 1.5 parts.
[0028] Micro-carbon ferrochrome: The chromium content of micro-carbon ferrochrome is ≥70wt%, and the carbon content is ≤0.06wt%. It is mainly used for alloying. Properly adding a certain amount of micro-carbon ferrochrome can improve the strength and hardness of the weld. The weight proportion of micro-carbon ferrochrome in the coating of the present invention is 9 to 12 parts, for example, the weight proportion of micro-carbon ferrochrome can be any value within the range of 9 to 12 parts, such as 9 parts, 10 parts or 12 parts.
[0029] Molybdenum powder: mainly used for alloying, molybdenum can be dissolved into carbides, so that the hardness and strength of (Fe, Cr)7C3 are improved, and the wear resistance of the material is correspondingly improved. The weight proportion of molybdenum iron in the coating of the present invention is 1 to 2 parts, for example, the weight proportion of molybdenum iron can be any value within the range of 1 to 2 parts, such as 1 part, 1.5 parts or 2 parts.
[0030] Ferrovanadium: The vanadium content of ferrovanadium is 50-55wt%, which is mainly used for alloying. Vanadium can improve the wear resistance of the weld, refine the grains, and improve the impact toughness of the steel. However, excessive vanadium will reduce the wear resistance of the welding wire. The weight percentage of ferrovanadium in the coating of the present invention is 0.2-0.5 parts, for example, the weight percentage of ferrovanadium can be any value within the range of 0.2-0.5 parts, such as 0.2 parts, 0.3 parts, 0.4 parts or 0.5 parts.
[0031] Reduced iron powder: mainly used as a deoxidizer and alloying agent to ensure the alloying element composition in the weld and ensure the weld strength. The weight percentage of reduced iron powder in the coating of the present invention is 35 to 50 parts, for example, the weight percentage of reduced iron powder can be any value within the range of 35 to 50 parts, such as 35 parts, 36 parts, 40 parts or 50 parts.
[0032] Potassium chloride: mainly improves slag viscosity, stabilizes arc, optimizes weld formation, and improves weld slag removal performance. The weight percentage of potassium chloride in the coating of the present invention is 0.3 to 0.6 parts, for example, the weight percentage of potassium chloride can be any value within the range of 0.3 to 0.6 parts, such as 0.3 parts, 0.35 parts, 0.4 parts, 0.55 parts or 0.6 parts.
[0033] Synthetic mica: mainly increases the fluidity of the powder, makes the coating easy to be evenly pressed on the surface of the welding core, and improves the crack resistance of the electrode coating. The weight proportion of the synthetic mica in the coating of the present invention is 0.3 to 0.6 parts, for example, the weight proportion of the synthetic mica can be any value within the range of 0.3 to 0.6 parts, such as 0.3 parts, 0.4 parts or 0.6 parts.
[0034] Rare earth ferrosilicon: used to refine grains and improve low temperature impact toughness of weld metal. The weight percentage of rare earth ferrosilicon in the coating of the present invention is 0.5 to 1.5 parts, for example, the weight percentage of rare earth ferrosilicon can be any value within the range of 0.5 to 1.5 parts, such as 0.5 parts, 0.6 parts, 1 parts, 1.4 parts or 1.5 parts.
[0035] In one embodiment, the particle sizes of graphite, silicon powder and rare earth ferrosilicon are 80-120 meshes, and the particle sizes of other components are 40-80 meshes.
[0036] See also Figure 1 The present invention provides a method for preparing a welding rod for heat-resistant steel welding, comprising the following steps:
[0037] S1. Weigh the components of the coating according to the ratio and mix them evenly to obtain coating powder;
[0038] S2, adding a binder to the coating powder and stirring to form a coating mixture;
[0039] S3. Press the coating mixture onto the surface of the welding core and dry it to obtain a welding rod for heat-resistant steel welding.
[0040] In step S1, the coating includes the following components and the weight proportions of each component are: 10-13 parts of marble, 3-5 parts of calcium fluoride, 0.2-0.5 parts of graphite, 1-2 parts of silicon micropowder, 1-2 parts of rutile, 1-2 parts of 45 ferrosilicon, 0.5-1.5 parts of low-carbon ferromanganese, 9-12 parts of low-carbon ferrochrome, 1-2 parts of molybdenum powder, 0.2-0.5 parts of ferrovanadium, 35-50 parts of reduced iron powder, 0.3-0.6 parts of potassium chloride, 0.3-0.6 parts of synthetic mica, and 0.5-1.5 parts of rare earth ferrosilicon.
[0041] In step S2, the binder is a water glass binder, and the mass of the binder is 23-25% of the total mass of the coating powder, for example, 23%, 24% or 25%. Further, the binder is a potassium-sodium water glass binder, the mass ratio of potassium to sodium in the potassium-sodium water glass binder is 1:1, and the modulus of the binder is 2.5-2.8.
[0042] In step S3, the welding core uses H08 steel core, the P content of the welding core is ≤0.015wt%, and the S content is ≤0.010wt%; the diameter of the welding core is 3.2-5.0mm, for example, the welding core diameter can be any value within the range of 3.2-5.0mm, such as 3.2mm, 4mm or 5mm.
[0043] During pressure coating, pressure coating, forming and other operations are performed on conventional oil pressure welding rod production equipment to uniformly pressure coat the coating mixture on the surface of the welding core, wherein the pressure coating pressure is 9 to 15 MPa, for example, any value within the range of 9 to 15 MPa such as 9 MPa, 12 MPa or 15 MPa. After pressure coating, the welding core coated with the coating mixture is dried at a temperature of 280 to 350°C, for example, 280°C, 320°C or 350°C, and a drying time of 1 to 2 hours, for example, 1 hour, 1.5 hours or 2 hours. Furthermore, after the coating mixture is pressure coated on the surface of the welding core, drying also includes low-temperature drying, for example, drying at 80°C for 1 hour, so as to partially remove the moisture in the coating mixture, prepare for high-temperature drying, prevent the prepared welding rod from sticking and bubbling, and improve the drying quality of the welding rod.
[0044] The technical scheme of the present invention is described in detail below through several specific examples. Unless otherwise specified, the raw materials and reagents used in the following examples are all commercially available products, or can be prepared by conventional methods in the art, and the instruments used in the examples are all commercially available.
[0045] Example 1
[0046] The welding rod for heat-resistant steel welding of this embodiment includes a welding core and a coating, wherein the coating includes the following components and the weight proportions of each component are respectively: 11 parts of marble, 5 parts of calcium fluoride, 0.25 parts of graphite, 1.5 parts of silicon micropowder, 1.5 parts of rutile, 1.5 parts of 45 ferrosilicon, 0.8 parts of low-carbon ferromanganese, 10 parts of micro-carbon ferrochrome, 2 parts of molybdenum powder, 0.4 parts of ferrovanadium, 40 parts of reduced iron powder, 0.4 parts of potassium chloride, 0.4 parts of synthetic mica, and 1 part of rare earth ferrosilicon. The above components are mixed evenly to obtain a coating powder, a water glass binder is added to the coating powder and stirred evenly to form a coating mixture, the coating mixture is pressed on the surface of the welding core at a pressure of 9MPa, and dried at 80°C for 1h and 320°C for 1h in turn to obtain a welding rod for heat-resistant steel welding. In this embodiment, the welding core is a 3.2 mm H08A steel core, the amount of water glass binder added is 23% of the total mass of the coating powder, and the mass of the coating mixture after drying accounts for 43% of the total mass of the welding rod for heat-resistant steel welding.
[0047] Example 2
[0048] The welding rod for heat-resistant steel welding of this embodiment includes a welding core and a coating, wherein the coating includes the following components and the weight proportions of each component are: 12 parts of marble, 4 parts of calcium fluoride, 0.4 parts of graphite, 1 part of silicon micropowder, 2 parts of rutile, 2 parts of 45 ferrosilicon, 1.5 parts of low-carbon ferromanganese, 9 parts of micro-carbon ferrochrome, 1.5 parts of molybdenum powder, 0.5 parts of ferrovanadium, 50 parts of reduced iron powder, 0.55 parts of potassium chloride, 0.6 parts of synthetic mica, and 1.4 parts of rare earth ferrosilicon. The above components are mixed evenly to obtain a coating powder, a water glass binder is added to the coating powder and stirred evenly to form a coating mixture, the coating mixture is pressed on the surface of the welding core at a pressure of 15MPa, and dried at 80°C for 1h and 280°C for 1.5h to obtain a welding rod for heat-resistant steel welding. In this embodiment, the welding core is a 4 mm H08A steel core, the amount of water glass binder added is 24% of the total mass of the coating powder, and the mass of the coating mixture after drying accounts for 40% of the total mass of the welding rod for heat-resistant steel welding.
[0049] Example 3
[0050] The welding rod for heat-resistant steel welding of this embodiment includes a welding core and a coating, wherein the coating includes the following components and the weight proportions of each component are: 13 parts of marble, 3.5 parts of calcium fluoride, 0.5 parts of graphite, 2 parts of silicon micropowder, 1.8 parts of rutile, 1 part of 45 ferrosilicon, 1 part of low-carbon ferromanganese, 12 parts of micro-carbon ferrochrome, 1 part of molybdenum powder, 0.3 parts of ferrovanadium, 36 parts of reduced iron powder, 0.35 parts of potassium chloride, 0.3 parts of synthetic mica, and 0.6 parts of rare earth ferrosilicon. The above components are mixed evenly to obtain a coating powder, a water glass binder is added to the coating powder and stirred evenly to form a coating mixture, the coating mixture is pressed on the surface of the welding core at a pressure of 15MPa, and dried at 80°C for 1h and 350°C for 2h to obtain a welding rod for heat-resistant steel welding. In this embodiment, the welding core is a 5 mm H08A steel core, the amount of water glass binder added is 25% of the total mass of the coating powder, and the mass of the coating mixture after drying accounts for 45% of the total mass of the welding rod for heat-resistant steel welding.
[0051] Example 4
[0052] The welding rod for heat-resistant steel welding of this embodiment includes a welding core and a coating, wherein the coating includes the following components and the weight proportions of each component are: 10 parts of marble, 4.5 parts of calcium fluoride, 0.3 parts of graphite, 1.8 parts of silicon micropowder, 1.2 parts of rutile, 1.3 parts of 45 ferrosilicon, 1.2 parts of low-carbon ferromanganese, 11 parts of micro-carbon ferrochrome, 1.2 parts of molybdenum powder, 0.4 parts of ferrovanadium, 45 parts of reduced iron powder, 0.6 parts of potassium chloride, 0.5 parts of synthetic mica, and 1.5 parts of rare earth ferrosilicon. The above components are mixed evenly to obtain a coating powder, a water glass binder is added to the coating powder and stirred evenly to form a coating mixture, the coating mixture is pressed on the surface of the welding core at a pressure of 13MPa, and dried at 80°C for 1h and 330°C for 2h to obtain a welding rod for heat-resistant steel welding. In this embodiment, the welding core is a 3.5 mm H08A steel core, the amount of water glass binder added is 23% of the total mass of the coating powder, and the mass of the coating mixture after drying accounts for 42% of the total mass of the welding rod for heat-resistant steel welding.
[0053] Example 5
[0054] The welding rod for heat-resistant steel welding of this embodiment includes a welding core and a coating, wherein the coating includes the following components and the weight proportions of each component are: 12 parts of marble, 3 parts of calcium fluoride, 0.2 parts of graphite, 1.3 parts of silicon micropowder, 1 part of rutile, 1.8 parts of 45 ferrosilicon, 0.5 parts of low-carbon ferromanganese, 10 parts of micro-carbon ferrochrome, 1.8 parts of molybdenum powder, 0.2 parts of ferrovanadium, 35 parts of reduced iron powder, 0.3 parts of potassium chloride, 0.4 parts of synthetic mica, and 0.5 parts of rare earth ferrosilicon. The above components are mixed evenly to obtain a coating powder, a water glass binder is added to the coating powder and stirred evenly to form a coating mixture, the coating mixture is pressed on the surface of the welding core at a pressure of 10MPa, and dried at 80°C for 1h and 320°C for 1.8h to obtain a welding rod for heat-resistant steel welding. In this embodiment, the welding core is a 4.5 mm H08A steel core, the amount of water glass binder added is 25% of the total mass of the coating powder, and the mass of the coating mixture after drying accounts for 41% of the total mass of the welding rod for heat-resistant steel welding.
[0055] The contents of the components of the coating in the heat-resistant steel welding electrodes of Examples 1 to 5 are shown in Table 1. According to GB / T25776-2010, the heat-resistant steel welding electrodes provided in Examples 1 to 5 were subjected to the chemical composition detection of the deposited metal and the welding processability test, and the chemical composition of the deposited metal is shown in Table 2; the mechanical properties and high-temperature tensile strength of the deposited metal are shown in Table 3; the crack resistance, deposition rate and welding processability of the deposited metal are shown in Table 4.
[0056] Table 1: Coating composition of heat-resistant steel welding electrodes of Examples 1 to 5
[0057]
[0058] Table 2: Chemical composition of deposited metal of heat-resistant steel welding electrodes of Examples 1 to 5
[0059]
[0060]
[0061] Table 3: Properties of deposited metal of heat-resistant steel welding electrodes of Examples 1 to 5
[0062]
[0063] Table 4: Crack resistance, deposition rate, and welding processability of the deposited metal of the heat-resistant steel welding electrode of Examples 1 to 5
[0064]
[0065] It can be seen from Tables 3 and 4 that the welding rod for heat-resistant steel welding of the present invention has good welding processability, high welding deposition rate, and has strong strength, toughness and crack resistance, is suitable for welding heat-resistant steel, and the strength of the deposited metal is well maintained at high temperature, and can be used in hydrogenation reactors.
[0066] The welding rod for heat-resistant steel welding of the present invention adopts an alkaline slag system to ensure that the weld has a low oxygen content and ensures high toughness of the weld metal; marble is added to the coating to play a slag-making and gas-making function at the arc temperature, which can improve the anti-porosity performance of the welding rod; low-carbon ferromanganese, micro-carbon ferrochrome, 45 ferrosilicon, ferrovanadium, ferromolybdenum, and graphite are added to the weld to infiltrate alloys, wherein chromium, molybdenum, and carbon elements can improve the strength of the weld, and rare earth ferrosilicon, molybdenum, and vanadium elements can refine the structure of the deposited metal and improve the toughness of the weld. The welding rod for heat-resistant steel welding prepared by the present invention has a smooth surface, good pressure coating, high welding deposition rate, and strong strength, toughness, and crack resistance. Therefore, the present invention effectively overcomes some practical problems in the prior art and has a high utilization value and use significance.
[0067] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A welding rod for heat-resistant steel welding, characterized in that: The welding rod comprises a welding core and a coating, and the coating comprises the following components and the weight proportions of each component are respectively: 10-13 parts of marble, 3-5 parts of calcium fluoride, 0.2-0.5 parts of graphite, 1-2 parts of silicon micropowder, 1-2 parts of rutile, 1-2 parts of 45 ferrosilicon, 0.5-1.5 parts of low-carbon ferromanganese, 9-12 parts of micro-carbon ferrochrome, 1-2 parts of molybdenum powder, 0.2-0.5 parts of ferrovanadium, 35-50 parts of reduced iron powder, 0.3-0.6 parts of potassium chloride, 0.3-0.6 parts of synthetic mica, and 0.5-1.5 parts of rare earth ferrosilicon.
2. The welding rod for heat-resistant steel welding according to claim 1, characterized in that: The calcium carbonate content in the marble is ≥96wt%; the silicon dioxide content in the silicon micropowder is ≥98wt%; the manganese content in the low-carbon ferromanganese is ≥80wt%; the chromium content in the micro-carbon ferrochrome is ≥70wt%, and the carbon content is ≤0.06wt%; the molybdenum content in the molybdenum powder is ≥99wt%; the vanadium content in the ferrovanadium is 50-55wt%; the iron content in the reduced iron powder is ≥98wt%.
3. The welding rod for heat-resistant steel welding according to claim 1, characterized in that: The particle sizes of the graphite, the silicon powder and the rare earth ferrosilicon are 80-120 meshes, and the particle sizes of the remaining components are 40-80 meshes.
4. The welding rod for heat-resistant steel welding according to claim 1, characterized in that: The welding core adopts H08 steel core, and the P content of the welding core is ≤0.015wt%, and the S content of the welding core is ≤0.010wt%.
5. The welding rod for heat-resistant steel welding according to claim 1, characterized in that: The diameter of the welding core is 3.2-5.0 mm.
6. A method for preparing a heat-resistant steel welding electrode according to any one of claims 1 to 5, characterized in that: The steps include: Weigh the various components of the coating according to the ratio and mix them evenly to obtain coating powder; Adding a binder to the coating powder and stirring evenly to form a coating mixture; The coating mixture is pressed onto the surface of the welding core and dried to obtain the welding rod for heat-resistant steel welding.
7. The preparation method according to claim 6, characterized in that: The binder is a water glass binder, and the mass of the binder is 23-25% of the total mass of the coating powder.
8. The preparation method according to claim 6, characterized in that: The weight of the coating mixture in the welding rod for heat-resistant steel welding after drying is 40-45% of the total weight of the welding rod for heat-resistant steel welding.
9. The preparation method according to claim 6, characterized in that: The pressure during the pressure coating is 9-15 MPa.
10. The preparation method according to claim 6, characterized in that: The drying temperature is 280-350°C and the drying time is 1-2 hours.
Citation Information
Patent Citations
Carbon steel covered electrode for nuclear power carbon steel welding and preparation method
CN103551760A
Electric welding rod with novel slag system for welding 9Ni steel for storage tanks of LNG (liquefied natural gas) ships
CN103753051A
High-temperature wear-resistant welding rod and production method thereof
CN108393605A
Ultralow-hydrogen and moisture-absorption-resistant welding electrode taking seamless flux-cored wire as welding core and preparation method
CN110153586A
Iron powder low hydrogen type coated arc welding electrode
JP2021109200A