Waterproof and heat-resistant asphalt concrete and preparation process
Through the cross-linking reaction of phenolic resin-modified polyacrylonitrile fibers with epoxy resin and asphalt, the problems of low strength and poor water resistance and water resistance of asphalt concrete are solved, and the effect of improving the mechanical properties and water resistance of asphalt concrete is achieved.
Patent Information
- Application Number
- CN202411314065.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-20
AI Technical Summary
Traditional asphalt concrete has low strength and poor water resistance.
The polyacrylonitrile fibers are modified with phenolic resin, and the cross-linking reaction with epoxy resin and asphalt is formed to form stable chemical bonds, improving the mechanical properties and water resistance of asphalt concrete.
The splitting strength, compressive strength and water resistance of asphalt concrete are significantly improved, the water absorption rate is reduced, and the good mechanical properties are maintained within the temperature range of -20℃ to 60℃.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, in particular to a waterproof and heat-resistant asphalt concrete and a preparation process. Background Art
[0002] Asphalt concrete mainly includes raw materials such as ore aggregate, mineral powder, asphalt, etc., and is widely used in roads, bridges, etc. Among them, epoxy asphalt concrete material, as a special asphalt concrete, can combine the advantages of epoxy resin and asphalt concrete, and has the characteristics of good viscosity, good curing performance, high bonding strength, excellent mechanical properties, etc., and is widely used. Adding polymer fibers such as polyester fibers, polyacrylonitrile fibers, polyethylene fibers, etc. to asphalt concrete can improve the mechanical strength, temperature resistance, waterproof and other properties of concrete materials. The invention patent of the announcement patent CN114835439B discloses an ultra-thin wear layer of epoxy asphalt steel slag concrete and a preparation method thereof. The epoxy asphalt steel slag concrete prepared by using epoxy asphalt, polyester fibers, aggregates including modified waterproof steel slag, etc. as raw materials has good high temperature stability, freeze-thaw resistance and other properties. Compared with polyester fibers, polyacrylonitrile fibers have the advantages of being cheap and easy to obtain, high mechanical strength, and large modulus, and have a better improvement effect on the mechanical properties of concrete. However, the traditional polyacrylonitrile fiber has a poor effect on improving the water resistance and waterproofing of asphalt concrete. Summary of the invention
[0003] The technical problem solved by the invention is to solve the problem of low strength and poor water resistance and waterproof performance of asphalt concrete.
[0004] The technical solution provided by the present invention is: a waterproof and heat-resistant asphalt concrete, including 280-350 parts by weight of coarse aggregate, 500-620 parts by weight of fine aggregate, 100-150 parts by weight of mineral powder, 40-52 parts by weight of base asphalt, 8-10 parts by weight of epoxy resin, 5.5-6.2 parts by weight of curing agent, and 1.5-3 parts by weight of phenolic resin modified polyacrylonitrile fiber.
[0005] The preparation process of phenolic resin modified polyacrylonitrile fiber is as follows:
[0006] (1) Add hydrolyzed polyacrylonitrile fiber to dimethyl sulfoxide, stir, add epoxy phenolic resin, catalyst N,N-dimethylbenzylamine or triethylenediamine, heat to 110-130°C, stir and react for 12-18 hours, add distilled water to dilute, filter, wash the product with distilled water and acetone, and dry to obtain a modified polyacrylonitrile fiber precursor.
[0007] (2) Add the modified polyacrylonitrile fiber precursor to dimethyl sulfoxide, stir, add isocyanoethyl methacrylate and dibutyltin dilaurate, heat to 50-70°C, stir and react for 6-12 hours, add distilled water to dilute, filter, wash the product with distilled water and acetone, and dry to obtain phenolic resin modified polyacrylonitrile fiber.
[0008] Furthermore, the weight ratio of hydrolyzed polyacrylonitrile fiber, epoxy phenolic resin and catalyst is 100:(10-30):(0.04-0.15).
[0009] Furthermore, the weight ratio of modified polyacrylonitrile fiber precursor, isocyanoethyl methacrylate, and dibutyltin dilaurate is 100:(4-12):(0.03-0.1).
[0010] Furthermore, the basalt aggregate has a particle size of 3-10 mm; the fine aggregate is the basalt aggregate with a particle size of ≤3 mm; and the mineral powder is limestone mineral powder.
[0011] Furthermore, the curing agent is a polyamide curing agent.
[0012] Furthermore, the preparation process of waterproof and heat-resistant asphalt concrete is as follows: the base asphalt is placed in a reactor, stirred and melted at 150-155°C, and then epoxy resin and phenolic resin modified polyacrylonitrile fiber are added and stirred and mixed; then coarse aggregate, fine aggregate and mineral powder are added, the temperature is raised to 170-175°C, stirring and mixing is continued, and then poured into a mold, cooled to 150-160°C, a curing agent is added, and after stirring, it is allowed to stand and cure for 5-8 hours, and cured to obtain waterproof and heat-resistant asphalt concrete.
[0013] The technical effect of the present invention is as follows: the present invention uses N, N-dimethylbenzylamine or triethylenediamine as a catalyst to make the carboxyl groups of hydrolyzed polyacrylonitrile fiber and part of the epoxy groups of epoxy phenolic resin undergo a ring-opening reaction to obtain a modified polyacrylonitrile fiber precursor; after the carboxyl groups of hydrolyzed polyacrylonitrile fiber and the epoxy groups of epoxy phenolic resin undergo a ring-opening reaction, hydroxyl groups can be generated, and dibutyltin dilaurate is used as a catalyst to make the generated hydroxyl groups undergo an addition reaction with the isocyanate groups of isocyanoethyl methacrylate to obtain phenolic resin modified polyacrylonitrile fiber, thereby introducing the epoxy phenolic resin molecular chain containing the acrylate group into the side chain of the polyacrylonitrile fiber.
[0014] The present invention uses basalt aggregate, limestone ore powder, matrix asphalt, and epoxy resin as the base materials of epoxy asphalt concrete, and phenolic resin modified polyacrylonitrile fiber as an additive, and obtains waterproof and heat-resistant asphalt concrete through blending and thermal curing; the side chain of polyacrylonitrile fiber introduces the epoxy phenolic resin molecular chain containing acrylate group, and the acrylate group can cross-link with the double bond in asphalt during high temperature curing to generate stable chemical bonds, further improving the interface bonding performance between polyacrylonitrile fiber and asphalt. At the same time, the epoxy group of epoxy phenolic resin, under the action of polyamide curing agent, undergoes curing cross-linking reaction with the epoxy group of epoxy resin, so that the phenolic resin modified polyacrylonitrile fiber plays the effect of increasing the volume of epoxy resin and asphalt, so that epoxy resin and asphalt form a highly compatible curing system, which is conducive to improving the mechanical properties of epoxy asphalt concrete such as splitting strength and compressive strength. In addition, the polyacrylonitrile fiber itself has the advantages of high strength, high modulus, good fracture performance, etc., and is chemically bonded to the curing network of epoxy resin and asphalt, which can further improve the mechanical properties of asphalt concrete.
[0015] The epoxy asphalt concrete of the present invention can still maintain a stable chemically bonded cross-linked network of epoxy resin, asphalt and phenolic resin modified polyacrylonitrile fiber at a low temperature of -20°C and a high temperature of 60°C, and the decrease range of the splitting strength and compressive strength of the asphalt concrete is very low, and still maintains good mechanical strength. At the same time, the epoxy phenolic resin contains an aromatic ring structure and has strong hydrophobicity. A hydrophobic solidified network is formed in the epoxy resin and asphalt, which can inhibit moisture from entering the interior of the asphalt concrete, thereby reducing the water absorption rate and improving the water resistance and waterproof performance of the concrete. DETAILED DESCRIPTION
[0016] For ease of understanding of the present invention, preferred embodiments of the present invention are provided below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive. Unless otherwise defined, all technical and scientific terms used herein are the same as the meanings generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0017] The coarse aggregate of the present invention is basalt aggregate with a particle size of 3-10 mm; the fine aggregate is basalt aggregate with a particle size of ≤3 mm. The epoxy resin model is epoxy resin E51. The phenolic resin brand is R7522E. The polyacrylonitrile fiber model is DQ-PAN12, and the length is 6 mm.
[0018] 10 g of polyacrylonitrile fiber was added into 400 mL of 5% sodium hydroxide solution, heated to 70°C, stirred for 6 min, diluted hydrochloric acid was added to adjust the pH of the solution to 5, filtered, washed with distilled water, and dried to obtain hydrolyzed polyacrylonitrile fiber.
[0019] To 40g of epichlorohydrin, add 5g of phenolic resin and 12g of tetrabutylammonium bromide, heat to 60°C in a nitrogen atmosphere, stir and react for 5h, then add 8mL of 20% sodium hydroxide solution by mass, heat to 85°C, react for 3h, add 10mL of ethyl acetate after cooling, mix well and filter to remove impurities, add 200mL of saturated sodium chloride solution to the filtrate, let stand to separate, collect the organic layer, dry and remove the solvent to obtain epoxy phenolic resin.
[0020] Example 1
[0021] (1) Add 20 g of hydrolyzed polyacrylonitrile fiber to 600 mL of dimethyl sulfoxide and stir for 4 h. Then add 2 g of epoxy phenolic resin and 8 mg of catalyst N,N-dimethylbenzylamine (CAS No. 103-83-3). Heat to 110 °C and stir for 18 h. Add distilled water to dilute. After filtering, wash the product with distilled water and acetone and dry it to obtain a modified polyacrylonitrile fiber precursor.
[0022] (2) Add 20 g of modified polyacrylonitrile fiber precursor to 400 mL of dimethyl sulfoxide and stir for 4 h. Then add 0.8 g of isocyanoethyl methacrylate (CAS No. 30674-80-7) and 6 mg of dibutyltin dilaurate (CAS No. 77-58-7). Heat to 50 °C and stir for 8 h. Add distilled water to dilute. After filtering, wash the product with distilled water and acetone and dry it to obtain phenolic resin modified polyacrylonitrile fiber.
[0023] (3) Place 400 g of base asphalt in a reactor, stir and melt at 155°C, then add 80 g of epoxy resin and 15 g of phenolic resin modified polyacrylonitrile fiber, and stir and mix for 3 min; then add 2800 g of basalt coarse aggregate, 6200 g of basalt fine aggregate, and 1000 g of limestone powder, raise the temperature to 175°C, continue to stir and mix for 20 min, then pour into a mold, cool to 160°C, add 55 g of curing agent polyamide 651, stir and let stand for 8 h to cure, and cure at room temperature for 14 days to obtain waterproof and heat-resistant asphalt concrete.
[0024] Example 2
[0025] (1) Add 20 g of hydrolyzed polyacrylonitrile fiber to 800 mL of dimethyl sulfoxide and stir for 4 h. Then add 4 g of epoxy phenolic resin and 16 mg of catalyst triethylenediamine (CAS No. 280-57-9). Heat to 120 °C and stir for 18 h. Add distilled water to dilute. After filtering, wash the product with distilled water and acetone and dry it to obtain a modified polyacrylonitrile fiber precursor.
[0026] (2) Add 20 g of modified polyacrylonitrile fiber precursor to 500 mL of dimethyl sulfoxide and stir for 4 h. Then add 1.6 g of isocyanoethyl methacrylate and 14 mg of dibutyltin dilaurate. Heat to 50 °C and stir for 12 h. Add distilled water to dilute. After filtering, wash the product with distilled water and acetone and dry it to obtain phenolic resin modified polyacrylonitrile fiber.
[0027] (3) Place 450 g of base asphalt in a reactor, stir and melt at 150°C, then add 90 g of epoxy resin and 22 g of phenolic resin modified polyacrylonitrile fiber, and stir and mix for 3 min; then add 3500 g of basalt coarse aggregate, 5000 g of basalt fine aggregate, and 1500 g of limestone powder, raise the temperature to 170°C, continue to stir and mix for 20 min, then pour into a mold, cool to 150°C, add 58 g of curing agent polyamide 651, stir and let stand for 8 h to cure, and cure at room temperature for 14 days to obtain waterproof and heat-resistant asphalt concrete.
[0028] Example 3
[0029] (1) Add 20 g of hydrolyzed polyacrylonitrile fiber to 800 mL of dimethyl sulfoxide and stir for 4 h. Then add 6 g of epoxy phenolic resin and 30 mg of catalyst triethylenediamine. Heat to 130 °C and stir for 12 h. Add distilled water to dilute. After filtering, wash the product with distilled water and acetone and dry it to obtain a modified polyacrylonitrile fiber precursor.
[0030] (2) Add 20 g of modified polyacrylonitrile fiber precursor to 600 mL of dimethyl sulfoxide and stir for 4 h. Then add 2.4 g of isocyanoethyl methacrylate and 20 mg of dibutyltin dilaurate. Heat to 70 °C and stir for 6 h. Add distilled water to dilute. After filtering, wash the product with distilled water and acetone and dry it to obtain phenolic resin modified polyacrylonitrile fiber.
[0031] (3) Place 520 g of base asphalt in a reactor, stir and melt at 150°C, then add 100 g of epoxy resin and 30 g of phenolic resin modified polyacrylonitrile fiber, and stir and mix for 3 min; then add 3000 g of basalt coarse aggregate, 5700 g of basalt fine aggregate, and 1300 g of limestone powder, raise the temperature to 175°C, continue to stir and mix for 20 min, then pour into a mold, cool to 150°C, add 62 g of curing agent polyamide 651, stir and let stand for 8 h to cure, and cure at room temperature for 14 days to obtain waterproof and heat-resistant asphalt concrete.
[0032] Comparative Example 1
[0033] (1) Place 400 g of base asphalt in a reactor, stir and melt at 155°C, then add 80 g of epoxy resin and stir and mix for 3 min; then add 2800 g of basalt coarse aggregate, 6200 g of basalt fine aggregate and 1000 g of limestone powder, raise the temperature to 175°C, continue to stir and mix for 20 min, then pour into a mold, cool to 160°C, add 55 g of curing agent polyamide 651, stir and let stand for 8 h to cure, and cure at room temperature for 14 days to obtain waterproof and heat-resistant asphalt concrete.
[0034] Comparative Example 2
[0035] (1) Place 400 g of base asphalt in a reactor, stir and melt at 155°C, then add 80 g of epoxy resin and 15 g of hydrolyzed polyacrylonitrile fiber, and stir and mix for 3 min; then add 2800 g of basalt coarse aggregate, 6200 g of basalt fine aggregate, and 1000 g of limestone powder, raise the temperature to 175°C, continue to stir and mix for 20 min, then pour into a mold, cool to 160°C, add 55 g of curing agent polyamide 651, stir and let stand for 8 h to cure, and cure at room temperature for 14 days to obtain waterproof and heat-resistant asphalt concrete.
[0036] Comparative Example 3
[0037] (1) Place 400 g of base asphalt in a reactor, stir and melt at 155°C, then add 80 g of epoxy resin and 15 g of epoxy phenolic resin, and stir and mix for 3 min; then add 2800 g of basalt coarse aggregate, 6200 g of basalt fine aggregate, and 1000 g of limestone powder, raise the temperature to 175°C, continue to stir and mix for 20 min, then pour into a mold, cool to 160°C, add 55 g of curing agent polyamide 651, stir and let stand for 8 h to cure, and cure at room temperature for 14 days to obtain waterproof and heat-resistant asphalt concrete.
[0038] Comparative Example 4
[0039] (1) 400 g of base asphalt was placed in a reactor, stirred and melted at 155°C, and then 80 g of epoxy resin and 15 g of modified polyacrylonitrile fiber precursor prepared in Example 1 were added and stirred for 3 min. Then 2800 g of basalt coarse aggregate, 6200 g of basalt fine aggregate and 1000 g of limestone powder were added, the temperature was raised to 175°C, and the stirring was continued for 20 min. Then the mixture was poured into a mold, cooled to 160°C, 55 g of curing agent polyamide 651 was added, and the mixture was allowed to stand and cure for 8 h after stirring. The mixture was cured at room temperature for 14 days to obtain waterproof and heat-resistant asphalt concrete.
[0040] Weigh the waterproof and heat-resistant asphalt concrete, place it in distilled water, soak it at room temperature for 7 days, take it out, wipe off the surface moisture, weigh it, and calculate the water absorption rate. Water absorption rate = (m-m0) / m0×100%. The results are shown in Table 1.
[0041] Table 1 Asphalt concrete water absorption test
[0042] ;
[0043] Asphalt concrete was made into a test piece with a diameter of 100 mm and a height of 60 mm, placed at a temperature of -20 to 60°C for 7 days, and then the splitting performance and compressive resistance of the asphalt concrete were tested according to the method of JTJ052-2000. The results are shown in Table 2-3.
[0044] Table 2 Splitting strength test of asphalt concrete
[0045] ;
[0046] Table 3 Compressive strength test of asphalt concrete
[0047] ;
[0048] It can be seen from Table 1 that the water absorption rate of the asphalt concrete of Examples 1-3 is only 0.029-0.061%, which is much lower than the water absorption rate of the asphalt concrete of Comparative Examples 1-4. The splitting strength after being placed at 25°C reaches 4.97-6.64MPa; the compressive strength reaches 10.15-13.54MPa. And after being placed at -20°C, the splitting strength remains at 4.63-6.18MPa; the compressive strength remains at 9.40-12.16MPa. After being placed at 60°C, the splitting strength remains at 4.90-6.45MPa; the compressive strength remains at 10.01-13.41MPa. This is because phenolic resin modified polyacrylonitrile fiber is added to the epoxy asphalt concrete, and the side chain of the polyacrylonitrile fiber introduces the epoxy phenolic resin molecular chain containing the acrylate group. During the high-temperature curing process, the acrylate group can undergo a cross-linking reaction with the double bonds in the asphalt to generate a stable chemical bond, further improving the interface bonding performance between the polyacrylonitrile fiber and the asphalt. At the same time, the epoxy groups of epoxy phenolic resin react with the epoxy groups of epoxy resin under the action of polyamide curing agent to undergo curing and crosslinking reaction, so that the phenolic resin modified polyacrylonitrile fiber can increase the capacity of epoxy resin and asphalt, so that epoxy resin and asphalt form a highly compatible curing system, which is beneficial to improving the mechanical properties of epoxy asphalt concrete, such as splitting strength and compressive strength. In addition, polyacrylonitrile fiber itself has the advantages of high strength, high modulus, and good fracture performance. Chemically bonding to the curing network of epoxy resin and asphalt can further improve the mechanical properties of asphalt concrete. At low temperatures of -20°C and high temperatures of 60°C, epoxy resin, asphalt and phenolic resin modified polyacrylonitrile fiber can still maintain a stable chemically bonded crosslinking network, and the decrease in splitting strength and compressive strength of asphalt concrete is very low, and good mechanical strength is still maintained. At the same time, epoxy phenolic resin contains an aromatic ring structure and has strong hydrophobicity. It forms a hydrophobic curing network in epoxy resin and asphalt, which can inhibit moisture from entering the interior of asphalt concrete, thereby reducing water absorption and improving the water resistance and waterproofing of concrete.
[0049] Compared with Example 1, in Comparative Example 1, no phenolic resin-modified polyacrylonitrile fiber was added, and the mechanical properties of the epoxy asphalt concrete were the worst, the water absorption rate was high, and the water resistance and waterproofing performance were poor.
[0050] In Comparative Example 2, only hydrolyzed polyacrylonitrile fiber was added. Polyacrylonitrile does not contain acrylate groups and has poor compatibility with asphalt, and cannot play the role of increasing the volume of asphalt and epoxy resin. The mechanical properties of epoxy asphalt concrete are low, the water absorption rate is high, and the water resistance and waterproofing performance are poor.
[0051] In Comparative Example 3, only epoxy phenolic resin was added without adding polyacrylonitrile fiber, and the mechanical properties of epoxy asphalt concrete were poor.
[0052] In Comparative Example 4, only modified polyacrylonitrile fiber precursor is added, which contains epoxy phenolic resin molecular chains but does not contain acrylate groups. It cannot undergo cross-linking reaction with the double bonds in asphalt to generate stable chemical bonds, has poor volume expansion effect on epoxy resin and asphalt, and fails to form a stable chemical bonding cross-linking network with epoxy resin and asphalt, resulting in the mechanical strength of the epoxy asphalt concrete being lower than that of Example 1.
Claims
1. A waterproof and heat-resistant asphalt concrete, It is characterized in that The waterproof and heat-resistant asphalt concrete comprises 280-350 parts by weight of coarse aggregate, 500-620 parts by weight of fine aggregate, 100-150 parts by weight of mineral powder, 40-52 parts by weight of base asphalt, 8-10 parts by weight of epoxy resin, 5.5-6.2 parts by weight of curing agent, and 1.5-3 parts by weight of phenolic resin-modified polyacrylonitrile fiber; The preparation process of the phenolic resin modified polyacrylonitrile fiber is as follows: (1) adding hydrolyzed polyacrylonitrile fiber to dimethyl sulfoxide, stirring, adding epoxy phenolic resin and catalyst, stirring and reacting, adding distilled water to dilute, filtering, washing, and drying to obtain a modified polyacrylonitrile fiber precursor; (2) Adding a modified polyacrylonitrile fiber precursor to dimethyl sulfoxide, adding isocyanoethyl methacrylate and dibutyltin dilaurate after stirring, adding distilled water to dilute after stirring, filtering, washing, and drying to obtain phenolic resin modified polyacrylonitrile fiber.
2. The waterproof and heat-resistant asphalt concrete according to claim 1, It is characterized in that The weight ratio of the hydrolyzed polyacrylonitrile fiber, epoxy phenolic resin and catalyst in (1) is 100:(10-30):(0.04-0.15).
3. The waterproof and heat-resistant asphalt concrete according to claim 2, It is characterized in that The catalyst is N,N-dimethylbenzylamine or triethylenediamine.
4. The waterproof and heat-resistant asphalt concrete according to claim 1, It is characterized in that The reaction temperature in (1) is 110-130°C and the reaction time is 12-18h.
5. The waterproof and heat-resistant asphalt concrete according to claim 1, It is characterized in that The weight ratio of modified polyacrylonitrile fiber precursor, isocyanoethyl methacrylate and dibutyltin dilaurate in (2) is 100:(4-12):(0.03-0.1).
6. The waterproof and heat-resistant asphalt concrete according to claim 1, It is characterized in that The reaction temperature in (2) is 50-70°C and the reaction time is 6-12h.
7. The waterproof and heat-resistant asphalt concrete according to claim 1, It is characterized in that The coarse aggregate is basalt aggregate with a particle size of 3-10 mm; the fine aggregate is basalt aggregate with a particle size of less than 3 mm; and the mineral powder is limestone mineral powder.
8. The waterproof and heat-resistant asphalt concrete according to claim 1, It is characterized in that The curing agent is a polyamide curing agent.
9. A process for preparing the waterproof and heat-resistant asphalt concrete according to any one of claims 1 to 8, It is characterized in that The preparation process is as follows: place the base asphalt in a reaction kettle, stir and melt at 150-155°C, then add epoxy resin and phenolic resin modified polyacrylonitrile fiber, stir and mix; then add coarse aggregate, fine aggregate, and mineral powder, heat to 170-175°C, continue to stir and mix, then pour into a mold, cool to 150-160°C, add a curing agent, stir and let stand for curing for 5-8 hours, and cure to obtain waterproof and heat-resistant asphalt concrete.