Preparation method of composite ceramic nanofiber sponge plate, composite ceramic nanofiber sponge plate and application of composite ceramic nanofiber sponge plate

Through the preparation method of composite ceramic nanofiber sponge board, the problem of complex process and large volume and weight of ceramic sponge board is solved, and a lightweight and high-temperature resistant nanofiber sponge board is prepared, which is used for fire protection and heat insulation of lithium battery packs, realizing lithium The safety, stability and cruising range of the battery pack are improved.

CN118812271APending Publication Date: 2024-10-22ZHEJIANG ROUHE NEW ENERGY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410888118.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing ceramic sponge board preparation process is complex and has a large volume and weight, making it difficult to be widely used in fireproof and heat insulation materials for lithium battery packs, and cannot effectively prevent thermal runaway and safety hazards of lithium batteries.

Method used

The preparation method of the composite ceramic nanofiber sponge board is adopted, including the preparation of precursor solution, electrospinning and hot pressing molding, to prepare a lightweight, soft, porous sponge board-shaped silicon oxide/alumina composite ceramic nanofiber sponge board, which is small and compact. Lightweight, high temperature resistant and corrosion resistant.

Benefits of technology

It achieves efficient heat isolation in lithium battery packs, ensures safe and stable operation, reduces the risk of battery short-circuit accidents, extends the service mileage of power batteries, and improves the safety and reliability of new energy vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812271A_ABST
    Figure CN118812271A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite ceramic nanofiber sponge plate, the composite ceramic nanofiber sponge plate and application of the composite ceramic nanofiber sponge plate, and belongs to the field of composite ceramic, the preparation method comprises the following steps: S1, preparing a precursor solution: dissolving a silicon source and an aluminum source in a solvent, and stirring until the silicon source and the aluminum source are dissolved to prepare an inorganic precursor; s2, controlling hydrolysis and polycondensation of the inorganic precursor to prepare linear inorganic spinning sol; s3, electrostatic spinning: spinning the linear inorganic spinning sol by using an electrostatic spinning machine to obtain composite ceramic nanofiber sponge; and S4, hot press molding: performing hot press on the composite ceramic nanofiber sponge by adopting a hot press molding machine to obtain the composite ceramic nanofiber sponge plate with the volume density of 0.5 g / cm < 3 >-10 g / cm < 3 >. According to the preparation method of the composite ceramic nanofiber sponge plate, the composite ceramic nanofiber sponge plate and the application of the composite ceramic nanofiber sponge plate, the prepared composite ceramic nanofiber sponge plate is in a light and soft porous sponge plate form, has certain elasticity and strength, and has the characteristics of being small, light, high-temperature-resistant and corrosion-resistant; therefore, the material has wide application prospects in the field of lithium battery pack fire prevention and heat insulation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of composite ceramics, and in particular to a preparation method of a composite ceramic nanofiber sponge board, a composite ceramic nanofiber sponge board and applications thereof. Background Art

[0002] With the improvement of global environmental awareness and strict restrictions on exhaust emissions of traditional fuel vehicles, the rise of new energy vehicles has become an irreversible development trend. In this context, lithium-ion batteries have gradually emerged in the field of new energy vehicles due to their high energy density, long cycle life, and environmental friendliness, and have been increasingly widely used. Whether it is a pure electric vehicle, a hybrid vehicle, or a plug-in hybrid vehicle, lithium-ion batteries play a vital role, providing efficient and stable energy solutions for these models.

[0003] However, in recent years, the thermal runaway problem of lithium battery packs for new energy vehicles has gradually surfaced. For example, thermal runaway caused by overcharging or short circuit will pose a serious safety hazard. Once this hazard turns into an extreme situation of battery combustion or even explosion, it will not only cause significant property losses, but is also likely to directly threaten people's lives. In order to effectively prevent this potential risk, the most critical and effective measure is to install high-temperature fireproof and heat-insulating materials with low thermal conductivity between the batteries of the lithium battery pack.

[0004] At the same time, oxide ceramics composed of one or more oxides not only have extremely high melting temperatures, but also show excellent stability in oxidizing atmospheres. Oxide ceramic materials include silicon oxide, aluminum oxide, zirconium oxide, and aluminum silicate, which have excellent mechanical strength, electrical insulation properties, and chemical stability and are widely used in daily life. In addition, whether in the development of photovoltaic energy, catalytic degradation, or in the application of adsorption and separation technology, oxide ceramic materials play a vital and irreplaceable role.

[0005] The ceramic sponge board, which is made of ceramic fibers through molding, drying and sintering, is a porous plate-shaped refractory material with a certain thickness, which can effectively reduce the probability of thermal runaway of the battery. However, the existing ceramic sponge board preparation process is complicated, and the volume and weight are large, making it difficult to be widely used as a fireproof and heat-insulating material inside lithium battery packs. Summary of the invention

[0006] To solve the above problems, the present invention provides a method for preparing a composite ceramic nanofiber sponge board, a composite ceramic nanofiber sponge board and applications thereof. The prepared composite ceramic nanofiber sponge board is in the form of a lightweight and soft porous sponge board, and at the same time has certain elasticity and strength, and is small and light, high temperature resistant, and corrosion resistant. Therefore, it has broad application prospects in the field of fire prevention and heat insulation of lithium battery packs.

[0007] To achieve the above object, the present invention provides a method for preparing a composite ceramic nanofiber sponge board, comprising the following steps:

[0008] S1. Preparing a precursor solution: dissolving a silicon source and an aluminum source in a solvent and stirring until dissolved to prepare an inorganic precursor;

[0009] S2, controlling the hydrolysis and polycondensation of the inorganic precursor to prepare a linear inorganic spinning sol;

[0010] S3, electrospinning: using an electrospinning machine to spin the linear inorganic spinning sol to obtain a composite ceramic nanofiber sponge;

[0011] S4. Hot pressing: The composite ceramic nanofiber sponge is hot pressed by a hot pressing machine to obtain a volume density of 0.5 g / cm 3 -10g / cm 3 Composite ceramic nanofiber sponge board.

[0012] Preferably, the silicon source in step S1 is methyl orthosilicate, ethyl orthosilicate or alkoxysilane;

[0013] The aluminum source is one of aluminum chloride hexahydrate, aluminum nitrate nonahydrate, aluminum sulfate, aluminum isopropoxide, aluminum acetate, aluminum trimethoxide, aluminum triethoxide, aluminum tri-n-propoxide, aluminum n-butoxide, aluminum sec-butoxide, aluminum tert-butoxide, and any combination thereof;

[0014] The solvent is one of methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, n-pentanol, ethylene glycol, butanediol, hexanediol or glycerol, and any combination thereof;

[0015] The stirring conditions are as follows: stirring time is 8h-48, stirring rate is 30rpm-600rpm, and stirring temperature is 25℃-80℃.

[0016] Preferably, the hydrolysis and polycondensation conditions of the inorganic precursor in step S2 are as follows: negative pressure of 0.02MPa-0.2MPa, temperature of 25°C-85°C, and time of 1h-12h;

[0017] The viscosity of the obtained linear inorganic spinning sol is 20 mPa·s-3200 mPa·s.

[0018] Preferably, in step S2, the polycondensation reaction efficiency, hydrolysis and polycondensation degree are characterized by a rotational viscometer.

[0019] Preferably, the spinning process parameters described in step S3 are as follows: positive pressure is 15kV-100kV, negative pressure is 0kV-100kV, receiving distance is 15cm-100cm, perfusion rate is 20mL / h-4000mL / h, spinning temperature is 25℃-40℃, and relative humidity is 20%-35%.

[0020] Preferably, in step S4, the hot pressing parameters are as follows: temperature is 60°C-300°C, time is 1 min-10 min, and pressure is 1 kPa-1000 kPa.

[0021] A composite ceramic nanofiber sponge board is obtained by the preparation method of the composite ceramic nanofiber sponge board.

[0022] The composite ceramic nanofiber sponge board is used in the fire protection and heat insulation of lithium battery packs.

[0023] The present invention has the following beneficial effects:

[0024] 1. Silica / alumina composite ceramic nanofiber sponge board, due to the excellent high temperature insulation properties of silica and alumina, can still maintain stable mechanical properties in harsh environments of 500°C to 1200°C, ensuring that the composite ceramic nanofiber sponge board can effectively isolate the heat between batteries in the lithium-ion battery pack of new energy vehicles, ensuring the safe and stable operation of the battery pack;

[0025] 2. The preparation can be completed through only three steps: precursor solution preparation, electrospinning and hot pressing, which is a simple and efficient process;

[0026] 3. The silicon oxide / aluminum oxide composite ceramic nanofiber sponge board will not produce toxic gases under high temperature conditions, ensuring the safety and environmental protection of the use process;

[0027] 4. Composite ceramic nanofiber sponge board made of silicon oxide and aluminum oxide ceramic nanofibers, with a density of 0.5g / cm 3 -10g / cm 3 , realizing the lightweight design of lithium-ion batteries, thereby improving the cruising range of new energy vehicles. At the same time, the excellent insulation and heat insulation performance can not only effectively isolate the heat between batteries, but also prevent the occurrence of battery short circuit accidents, thereby improving the safety and reliability of new energy vehicles, and significantly extending the service life of power batteries, thereby further reducing energy consumption.

[0028] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is an electronic scanning diagram of a method for preparing a composite ceramic nanofiber sponge board of the present invention. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages disclosed in the embodiments of the present invention clearer, the embodiments of the present invention are further described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the embodiments of the present invention and are not intended to limit the embodiments of the present invention. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application. Examples of the embodiments are shown in the accompanying drawings, where the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions.

[0031] It should be noted that the terms "include", "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or server comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products or devices.

[0032] Like reference numerals and letters denote similar items in the following drawings, and thus, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0033] like Figure 1 As shown, a method for preparing a composite ceramic nanofiber sponge board comprises the following steps:

[0034] S1. Preparing a precursor solution: dissolving a silicon source and an aluminum source in a solvent and stirring until dissolved to prepare an inorganic precursor;

[0035] The silicon source described in step S1 is methyl orthosilicate (TMOS), ethyl orthosilicate (TEOS) or alkoxysilane; the aluminum source is one of aluminum chloride hexahydrate, aluminum nitrate nonahydrate, aluminum sulfate, aluminum isopropoxide, aluminum acetate, trimethoxyaluminum, triethanol aluminum, tri-n-propoxyaluminum, aluminum n-butoxide, aluminum sec-butoxide, and aluminum tert-butoxide, and any combination thereof; the solvent is one of methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, n-pentanol, ethylene glycol, butanediol, hexanediol, or glycerol, and any combination thereof; the stirring conditions are as follows: the stirring time is 8h-48, the stirring rate is 30rpm-600rpm, and the stirring temperature is 25°C-80°C. In this embodiment, the stirring time can be appropriately reduced according to the increase in the stirring temperature to shorten the preparation process time.

[0036] S2, controlling the hydrolysis and polycondensation of the inorganic precursor to prepare a linear inorganic spinning sol;

[0037] The hydrolysis and polycondensation conditions of the inorganic precursor in step S2 are as follows: negative pressure of 0.02MPa-0.2MPa, temperature of 25°C-85°C, and time of 1h-12h;

[0038] The viscosity of the obtained linear inorganic spinning sol is 20 mPa·s-3200 mPa·s.

[0039] In step S2, the polycondensation reaction efficiency, hydrolysis and polycondensation degree are characterized by a rotational viscometer.

[0040] S3, electrospinning: using an electrospinning machine to spin the linear inorganic spinning sol to obtain a composite ceramic nanofiber sponge;

[0041] The spinning process parameters described in step S3 are as follows: positive pressure is 15kV-100kV, negative pressure is 0kV-100kV, receiving distance is 15cm-100cm, perfusion rate is 20mL / h-4000mL / h, spinning temperature is 25℃-40℃, and relative humidity is 20%-35%.

[0042] S4. Hot pressing: The composite ceramic nanofiber sponge is hot pressed by a hot pressing machine to obtain a volume density of 0.5 g / cm 3 -10g / cm 3 Composite ceramic nanofiber sponge board.

[0043] In step S4, the hot pressing parameters are as follows: temperature is 60°C-300°C, time is 1 min-10 min, and pressure is 1 kPa-1000 kPa.

[0044] A composite ceramic nanofiber sponge board is obtained by the preparation method of the composite ceramic nanofiber sponge board.

[0045] The composite ceramic nanofiber sponge board is used in the fire protection and heat insulation of lithium battery packs.

[0046] Therefore, the present invention adopts the preparation method of the above-mentioned composite ceramic nanofiber sponge board, the composite ceramic nanofiber sponge board and its application. The prepared composite ceramic nanofiber sponge board is in the form of a lightweight and soft porous sponge board, and at the same time has certain elasticity and strength, and is small and light, has low mass density, good mechanical strength, high temperature resistance, and corrosion resistance. After the test, there is no mechanical damage, breakage or deformation. Therefore, it has broad application prospects in the field of fire prevention and heat insulation of lithium battery packs, so as to meet the application needs of more efficient fire prevention and heat insulation in lithium battery packs, which is of great significance for promoting the development of new energy vehicle batteries.

[0047] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a composite ceramic nanofiber sponge board, characterized in that: The following steps are involved: S1. Preparing a precursor solution: dissolving a silicon source and an aluminum source in a solvent and stirring until dissolved to prepare an inorganic precursor; S2, controlling the hydrolysis and polycondensation of the inorganic precursor to prepare a linear inorganic spinning sol; S3, electrospinning: using an electrospinning machine to spin the linear inorganic spinning sol to obtain a composite ceramic nanofiber sponge; S4. Hot pressing: The composite ceramic nanofiber sponge is hot pressed by a hot pressing machine to obtain a volume density of 0.5 g / cm 3 -10g / cm 3 Composite ceramic nanofiber sponge board.

2. The method for preparing the composite ceramic nanofiber sponge board according to claim 1, characterized in that: The silicon source in step S1 is methyl orthosilicate, ethyl orthosilicate or alkoxysilane; The aluminum source is one of aluminum chloride hexahydrate, aluminum nitrate nonahydrate, aluminum sulfate, aluminum isopropoxide, aluminum acetate, aluminum trimethoxide, aluminum triethoxide, aluminum tri-n-propoxide, aluminum n-butoxide, aluminum sec-butoxide, aluminum tert-butoxide, and any combination thereof; The solvent is one of methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, n-pentanol, ethylene glycol, butanediol, hexanediol or glycerol, and any combination thereof; The stirring conditions are as follows: stirring time is 8h-48, stirring rate is 30rpm-600rpm, and stirring temperature is 25℃-80℃.

3. The method for preparing the composite ceramic nanofiber sponge board according to claim 1, characterized in that: The hydrolysis and polycondensation conditions of the inorganic precursor in step S2 are as follows: negative pressure of 0.02MPa-0.2MPa, temperature of 25°C-85°C, and time of 1h-12h; The viscosity of the obtained linear inorganic spinning sol is 20 mPa·s-3200 mPa·s.

4. The method for preparing the composite ceramic nanofiber sponge board according to claim 1, characterized in that: In step S2, the polycondensation reaction efficiency, hydrolysis and polycondensation degree are characterized by a rotational viscometer.

5. The method for preparing the composite ceramic nanofiber sponge board according to claim 1, characterized in that: The spinning process parameters described in step S3 are as follows: positive pressure is 15kV-100kV, negative pressure is 0kV-100kV, receiving distance is 15cm-100cm, perfusion rate is 20mL / h-4000mL / h, spinning temperature is 25℃-40℃, and relative humidity is 20%-35%.

6. The method for preparing the composite ceramic nanofiber sponge board according to claim 1, characterized in that: In step S4, the hot pressing parameters are as follows: temperature is 60°C-300°C, time is 1 min-10 min, and pressure is 1 kPa-1000 kPa.

7. A composite ceramic nanofiber sponge board, characterized in that: The composite ceramic nanofiber sponge board is obtained by the preparation method of any one of claims 1 to 6.

8. Application of the composite ceramic nanofiber sponge board as claimed in claim 7 in fire protection and heat insulation of lithium battery packs.