Superfine fiber porous material continuous production system based on electrostatic air jet spinning and preparation method of superfine fiber porous material
Through the multi-system collaborative design of electrostatic spray spinning technology, the problems of low solid content and gelation of spinning liquid are solved, and the high-speed, controllable preparation and morphological structure control of microfiber porous materials are achieved, which improves the application range of materials and performance.
Patent Information
- Application Number
- CN202411182158.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing electrostatic spraying technology has low efficiency and poor stability in spinning liquid-solid content, high viscosity and gelation problems, making it difficult to achieve rapid and efficient macro manufacturing and precise morphological structure control of microfiber materials, and lacks Post-treatment equipment for porous materials.
A continuous production system for microfiber porous materials based on electrostatic spray spinning has been developed, including solution preparation device, gelation suppression device, pressure-regulating gas supply device, electrostatic spray spinning module, non-solvent control device, The integrated fiber receiving/solvent recovery device, the thermogenic welding device, the spraying bonding device, the integrated drying and shaping/packing device and the variable atmosphere heat treatment device. Through the combined use of these devices, the fiber diameter refinement and high-speed material Can be controlled.
The spinning production rate and fiber diameter refinement are improved, and the continuous macro preparation of microfiber porous materials is realized, the application range of materials is broadened, and the diversity and performance of materials are improved by precisely regulating the material morphology and structure.
Smart Images

Figure CN119020920A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ultrafine fiber preparation, and specifically relates to an ultrafine fiber porous material continuous production system based on electrostatic air jet spinning and a method for preparing the ultrafine fiber porous material. Background Art
[0002] Compared with traditional fibers, ultrafine fibers have the advantages of smaller diameter, larger specific surface area, and stronger surface adsorption. They can be widely used in thermal insulation, air filtration, sound absorption and noise reduction, waterproof and breathable fields. At present, the main preparation methods of ultrafine fibers are electrospinning, melt blowing, island method, etc., but the fiber diameter obtained by melt blowing is relatively coarse, and the fiber continuity obtained by island method is poor. The fibers prepared by solution electrospinning have a thin diameter and high quality, but the spinning rate is low. Therefore, how to improve the production rate of high-quality ultrafine fibers, further refine the fiber diameter, and realize the continuous large-scale preparation of ultrafine fiber porous materials is a major problem that needs to be solved urgently.
[0003] At present, relevant technicians have done some research in this field. Patent ZL201610067092.4 discloses a gap-adjustable electrospinning nozzle and an array spinning system. The array arrangement of the nozzle increases the density of the spinning jet, thereby increasing the fiber yield. However, this method easily leads to serious electric field interference between the spinning jets, affecting the quality of the ultrafine fiber material. Patent ZL201310606374.3 discloses a high-pressure airflow-assisted nozzle self-rotating electrospinning device. Airflow-assisted spinning is introduced on the basis of electrospinning, which improves the single-needle spinning efficiency and reduces the electric field interference between the spinning jets. However, the nozzle used in the device will produce self-rotation, making it difficult to accurately control the spinning jet morphology. Patent ZL201410667969.4 discloses a method and device for producing polymer nanofibers using high-speed airflow and high-voltage electrostatics. The polymer solution is stretched at high speed using double-layer high-speed airflow and high-voltage electrostatics to increase the spinning rate. However, there is airflow interference between the double-layer high-speed airflows, resulting in poor morphology of the fiber material. Patent ZL201811315128.1 discloses an arc-shaped array electrospinning nozzle with sheath gas constraint. It designs a stepped conductive plate and an arc-shaped needle arrangement to reduce the electric field interference between multi-jet nozzles, improve the nanofiber deposition efficiency and refine the fiber diameter. However, the device can only be used to prepare fiber membranes, and cannot prepare fiber body materials, and cannot yet achieve continuous production of ultrafine fiber porous materials. Summary of the invention
[0004] The purpose of the present invention is to overcome at least one of the defects of the above-mentioned prior art and to provide a continuous production system of ultrafine fiber porous materials based on electrostatic air spinning and a method for preparing ultrafine fiber porous materials. While refining the fiber diameter, the production system meets the controllable and high-speed preparation requirements of ultrafine fiber materials of various materials and structures, thereby realizing the large-scale stable production of ultrafine fiber porous materials.
[0005] Specifically, the technical problem to be solved by the present invention is: the existing electrostatic air jet technology often uses a low-solid content spinning solution for spinning, resulting in low spinning efficiency, so it is necessary to further increase the solid content of the spinning solution, but there are problems such as high viscosity and slow mass transfer in the spinning solution configuration process, which makes it difficult for the spinning solution to be uniform and stable; the spinning solution is prone to gelation during storage, so the spinning solution is usually directly transported to the spinning nozzle for spinning, which makes it difficult to supply the spinning solution stably; in order to ensure the spinning stability, a low-density spinning nozzle is usually used during spinning, which makes it difficult to increase the spinning rate; the existing electrostatic air jet spinning equipment is still in the laboratory test stage, which cannot meet the rapid, efficient and large-scale manufacturing of ultrafine fiber materials, and it is difficult to accurately control the thickness, porosity and other morphological structures of the ultrafine fiber materials, resulting in the prepared materials being relatively single; at the same time, there is currently a lack of post-processing equipment for electrostatic air jet-spun ultrafine fiber porous materials. In view of the above-mentioned problems, the present invention has developed a solution preparation device, a gelation inhibition device, a pressure-stabilizing gas supply device, an electrostatic air jet spinning module, a non-solvent control device, a fiber receiving / solvent recovery integrated device, a thermal welding device, a spray bonding device, a drying and shaping / packaging integrated device, and a variable atmosphere heat treatment device, which are suitable for the preparation of high-viscosity solutions. Through the coordinated use of the above devices, the production rate of ultrafine fibers and the continuous large-scale preparation of ultrafine fiber porous materials can be achieved, which further promotes the capacity upgrade of ultrafine fiber preparation technology and broadens the application scope of ultrafine fiber porous materials and their products.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] One of the purposes of the present invention is to provide a continuous production system of ultrafine fiber porous materials based on electrostatic air-spinning, comprising:
[0008] A solution stabilization configuration subsystem, which includes a gelation inhibition device and a solution preparation device disposed above the gelation inhibition device;
[0009] An electrostatic air-jet spinning subsystem, comprising an electrostatic air-jet spinning module, a non-solvent control device and a fiber receiving / solvent recovery integrated device connected in sequence from top to bottom, and a pressure-stabilizing air supply device connected to the electrostatic air-jet spinning module;
[0010] A fine post-processing subsystem, which includes a first post-processing device and a second post-processing device connected to each other, wherein the ultrafine fiber porous material spun by the electrostatic air jet spinning module is transported to the first post-processing device for post-processing, and then transported to the second post-processing device for processing;
[0011] Wherein, the first post-processing device includes a thermal welding device and / or a spray adhesive bonding device; the second post-processing device includes a drying, shaping / packaging integrated device and / or a variable atmosphere heat treatment device.
[0012] Furthermore, the solution preparation device includes: a polymer dissolution chamber; an automatic feeding mechanism arranged obliquely above the polymer dissolution chamber and connected thereto; a solution propulsion piston arranged above the polymer dissolution chamber, and a power mechanism connected to the solution propulsion piston; a high-frequency ultrasonic mechanism, a sub-high-frequency ultrasonic mechanism and a turbine-type stirring roller arranged in the polymer dissolution chamber from top to bottom, wherein the high-frequency ultrasonic mechanism is controlled by an external control system; the sub-high-frequency ultrasonic mechanism is controlled by an external control system; and the turbine-type stirring roller is controlled by a stirring control system.
[0013] Furthermore, the solution preparation device also includes a solution propulsion piston disposed above the automatic feeding mechanism, and a power mechanism connected to the solution propulsion piston.
[0014] Furthermore, the gelation inhibition device includes: a liquid storage tank body; a stirring roller transmission mechanism, a variable frequency heating layer and a heat insulation and protection layer arranged on the outer wall of the liquid storage tank body from the inside to the outside; a plurality of screw stirring rollers arranged in the liquid storage tank body, and both ends of the stirring rollers penetrate the liquid storage tank body radially along the liquid storage tank body and are connected to the stirring roller transmission mechanism.
[0015] Furthermore, the pressure-stabilizing air supply device includes: an air compressor; an air storage tank, a first pipeline for connecting the air compressor and the air storage tank is arranged between the two, and an air filter is arranged in the first pipeline; a temperature and humidity control chamber, a second pipeline for connecting the air compressor and the air storage tank is arranged between the two, and an electric control valve for controlling the ventilation volume is arranged on the second pipeline; an air supply pipeline for connecting the temperature and humidity control chamber and the electrostatic air jet spinning module is arranged between the two.
[0016] Furthermore, the electrostatic air jet spinning module includes: a spinning plate; a high-voltage power supply connected to the spinning plate; an air supply pipeline arranged in the spinning plate, one end of the air supply pipeline is connected to the pressure-stabilizing air supply device, and the other end branches out into a plurality of air supply branches; a liquid supply pipeline arranged in the spinning plate, one end of the liquid supply pipeline is connected to the gelation inhibition device, and the other end branches out into a plurality of liquid supply branches; a plurality of spinning nozzles arranged at intervals on the lower end surface of the spinning plate, each of the spinning nozzles is provided with gas pipelines and liquid pipelines that are independent of each other and arranged in an array, the gas pipeline is connected to the air supply branch, and the liquid pipeline is connected to the liquid supply branch.
[0017] Furthermore, the non-solvent control device includes a moisture control mechanism located between the electrostatic air-jet spinning module and the fiber receiving / solvent recovery integrated device.
[0018] Furthermore, the fiber receiving / solvent recovery integrated device includes: a fiber receiving conveying curtain, used to convey the ultrafine fiber porous material spun by the electrostatic air jet spinning module to the first post-processing device for post-processing; a negative pressure suction pipe arranged under the fiber receiving conveying curtain; a gas-liquid filtration and separation mechanism connected to the negative pressure suction pipe; and a negative pressure suction pump connected to the gas-liquid filtration and separation mechanism.
[0019] Furthermore, the thermal welding device includes: a box body; a pneumatic pressure transmission rod that passes through the upper end surface of the box body, a pneumatic pressure control mechanism is provided at one end of the rod that is located outside the box body, and a pressurizing component is provided at one end of the rod that is located inside the box body; a micro-array welding composite mechanism is arranged in the box body and below the pressurizing component; an ultrasonic control system connected to the micro-array welding composite mechanism to control the ultrasonic vibration of the micro-array welding composite mechanism to achieve material welding.
[0020] Furthermore, the glue spraying and bonding device includes a conveyor belt, and also includes the following arranged in sequence along the conveying direction of the conveyor belt: a glue spraying box arranged above the conveyor belt, whose lower end face is provided with an atomizing nozzle, and there is a gap between the atomizing nozzle and the upper end face of the conveyor belt; a limiting roller with a gap between the upper end face of the conveyor belt; a grabbing mechanism, used for stacking fiber materials sprayed with glue; and a cutting mechanism, used for cutting the stacked fiber materials from the unstacked fiber materials.
[0021] Furthermore, the integrated drying, shaping / packaging device comprises: a fiber material driving roller; a hot air drying unit connected to the fiber material driving roller; a fiber material receiving platform arranged above the fiber material driving roller, and a cold air shaping unit and a cold air shaping gun are arranged above the fiber material receiving platform; specifically, the cold air shaping unit is located above the fiber material receiving platform, and the cold air shaping gun is located at the outlet, and the cold air output is controlled from multiple directions to shape the fiber material.
[0022] Furthermore, the variable atmosphere heat treatment device includes: a conveying roller, a lower heating roller and a winding roller arranged along the transportation direction of the fiber material; an upper heating roller arranged above the lower heating roller; a microwave generator arranged above the lower heating roller; and a multi-component gas conveying device arranged below the lower heating roller.
[0023] The second object of the present invention is to provide a method for preparing ultrafine fiber porous material, which is prepared by using the continuous production system as described above, and the preparation method comprises the following steps:
[0024] Step 1: Turn on the turbine stirring roller, and put the raw materials from the automatic feeding mechanism into the solution preparation device in sequence; dissolve the raw materials under the joint action of the turbine stirring roller, the high-frequency ultrasonic mechanism, and the sub-high-frequency ultrasonic mechanism; then turn on the power mechanism to drive the solution propulsion piston to move downward, so that the raw material solution flows into the liquid storage tank body of the gelation inhibition device; turn on the variable frequency heating layer heating, and set a plurality of screw stirring rollers in the liquid storage tank body, so that the raw material solution can be stably stored in the liquid storage tank body for at least 200 hours without gelation;
[0025] Step 2: Turn on the humidity control mechanism to adjust the relative humidity of the spinning area, and then pass the raw material solution into the infusion pipe. Under the action of pressure, the solution flows from the infusion pipe to the liquid supply pipe in the electrostatic air jet spinning module, and is extruded into filaments through the spinning nozzle. The raw material solution is polarized and stretched under the action of voltage and airflow to obtain an ultrafine fiber porous material intermediate. Specifically, the raw material solution is introduced into the liquid infusion pipeline, and under the action of pressure, the solution flows from the liquid infusion pipeline to the liquid supply pipeline in the electrostatic air jet spinning module; the raw material solution is polarized and stretched under the action of voltage and airflow, and due to humidity induction, it quickly separates into curly fibers, which are accumulated to form a fluffy structure of ultrafine fiber porous material intermediates, or slowly separates into straight fibers, which are accumulated to form fiber membranes, that is, another ultrafine fiber porous material intermediate; multiple negative pressure suction pipes are installed under the fiber receiving and conveying curtain to suck the solvent vapor in the spinning area, and the gas-liquid filtration separation mechanism is equipped with an adsorption device. The solvent vapor is separated from the solvent by the gas-liquid filtration separation mechanism and dried, and finally discharged to the outdoor environment by a negative pressure suction pump;
[0026] Step 3: Select one of the following:
[0027] ① The ultrafine fiber porous material is continuously transported on the fiber receiving conveying curtain to the thermal fusion device for fine post-processing. The air pressure control mechanism is connected to the pneumatic pressure transmission rod to push the pressurizing component to pressurize the ultrafine fiber porous material. The ultrafine fibers between the pressurizing component and the micro-lattice fusion composite mechanism are melt-bonded under the action of ultrasound and pressure to obtain an ultrafine fiber porous material intermediate that has been post-processed by thermal fusion.
[0028] ② The ultrafine fiber porous material is further transported on the fiber receiving conveying curtain to the glue spraying and bonding device for fine post-processing. The glue in the glue spraying box is evenly sprayed on the inside and outside of the ultrafine fiber porous material through the atomizing nozzle. Then the ultrafine fiber porous material is clamped between the conveyor belt and the limiting roller. The fiber material is cut by the cutting mechanism to obtain the ultrafine fiber porous material intermediate after glue spraying and bonding post-processing;
[0029] Step 4: Choose one of the following:
[0030] ① The ultrafine fiber porous material intermediate that has been post-processed by thermal fusion or the ultrafine fiber porous material intermediate that has been post-processed by spraying glue is transported to the drying, shaping / packaging integrated device for drying, shaping and packaging; the air after drying and impurity removal enters the hot air drying unit, and the air is heated and transported to the ultrafine fiber porous material intermediate on the fiber material transmission roller to dry the ultrafine porous fiber intermediate and soften the glue and low melting point fiber; then the ultrafine fiber porous material intermediate enters the cold air cooling and shaping area, so that the softened ultrafine fiber porous material intermediate is quickly annealed, cooled and shaped, and the cooled fiber material intermediate is transported to the fiber material receiving station for packaging to obtain the ultrafine fiber porous material;
[0031] ② The ultrafine fiber porous material intermediate that has been post-processed by thermal fusion or the ultrafine fiber porous material intermediate that has been post-processed by spray bonding is transported to a variable atmosphere heat treatment device for high-temperature calcination. The organic components in the fiber are pre-broken under the action of microwaves. The multi-component gas conveying equipment supplies one or more of air, oxygen or nitrogen. The organic components are thermally decomposed or carbonized under high temperature conditions. If there are inorganic components in the fiber, the inorganic components undergo grain growth under high temperature conditions to obtain an ultrafine fiber porous material, which is finally wound up and stored by a winding roller.
[0032] In the present invention, the output frequency range of the high-frequency ultrasonic mechanism is 80 to 130 kHz;
[0033] In the present invention, the output frequency range of the sub-high frequency ultrasonic mechanism is 20 to 80 kHz;
[0034] In the present invention, the turbine stirring roller is controlled by a stirring control system, and the turbine stirring roller is located inside the solution preparation device, with a rotation speed of 100 to 6000 rpm, which is suitable for stirring high-viscosity solutions with a viscosity range of 20 to 40000 mPa·s;
[0035] In the present invention, the gelation inhibition device achieves the purpose of inhibiting the gelation of the spinning solution by stable heating and continuous stirring of the screw, and the spinning solution can remain in an ungelled state for 200 to 400 hours;
[0036] In the present invention, the rotation speed of the screw stirring roller is 200 to 700 rpm, the number is 2 to 10, and the arrangement is selected from one or more of a rectangular array, a triangular array, a trapezoidal array, a diamond array, a fractal array or a honeycomb array;
[0037] In the present invention, the temperature and humidity control chamber in the pressure-stabilizing air supply device comprises an insulating layer, and a freeze-drying component and a heating component arranged in the insulating layer. The freeze-drying component is located below the heating component. The temperature range of the air flow blown out by the pressure-stabilizing air supply device is -10 to 80°C.
[0038] Specifically, in the present invention, the temperature and humidity control chamber in the pressure-stabilizing air supply device is mainly composed of an insulation layer, a freeze-drying component and a heating component, and the temperature range of the blown air flow is -10 to 80°C; the thickness of the insulation layer is 2 to 10 cm, and the heating method of the heating component can be circulating hot oil heating, circulating hot water or electric heating; the material of the insulation layer protective layer is alumina, aluminum foil composite glass fiber cloth, silicon carbide fiber, aluminum silicate, glass wool, rock wool, expanded perlite and its composite materials.
[0039] In the present invention, the spinning nozzle in the electrostatic air jet spinning module is selected from one or more of a coaxial nozzle, a differential nozzle, a conical cluster nozzle or a vortex nozzle; the spacing between two adjacent spinning nozzles is 20 to 50 mm; the number of the spinning nozzles is 30 to 120; the diameter of the jet nozzle of the spinning nozzle is 0.5 to 10 mm, and the diameter of the spinneret hole is 0.1 to 5 mm; the air flow velocity of the jet nozzle is 0 to 25 m / s; the liquid output of each spinneret hole is 5 to 80 ml / h; the spinning voltage range is 0 to 150 kV;
[0040] In the present invention, the humidity control mechanism in the non-solvent control device controls the solvent volatilization rate of the spinning jet and the phase separation rate in the jet according to the requirements of the ultrafine fiber porous material morphology, and can adjust the relative humidity of the environment in the spinning area to 10-99%;
[0041] In the present invention, the air pressure control mechanism generates sufficient air pressure to push the pressurizing assembly connected by the pneumatic pressure transmission rod, and the pressure generated ranges from 2 to 8 MPa.
[0042] In the present invention, the suction pressure range of the negative pressure suction pump is 0 to 5 MPa, and the negative pressure suction pipeline is composed of a main pipe connected to 3 to 12 branch pipes, and the branch pipes are distributed under the fiber receiving and conveying curtain to suck the solvent vapor in the spinning area; the gas-liquid filtration and separation mechanism is equipped with an activated carbon adsorption device, and the solvent vapor is separated from the solvent vapor by the gas-liquid filtration and separation mechanism and dried, and finally discharged to the outdoor environment by the negative pressure suction pump.
[0043] In the present invention, the fiber receiving conveying curtain in the fiber receiving / solvent recovery integrated device is grounded, and the material is selected from one or more of metal, plastic, rubber or fiber reinforced composite materials, and the moving speed of the fiber receiving conveying curtain is 0.1 to 10 m / min;
[0044] In the present invention, the frequency of the sound waves output by the ultrasonic control system in the thermal welding device can be adjusted in the range of 5 to 30 kHz, and the lattice of the micro-lattice welding composite mechanism is selected from one or more of a honeycomb shape, a grid shape, a triangle shape or a diamond shape;
[0045] In the present invention, the glue spraying amount of a single atomizing nozzle in the glue spray bonding device ranges from 0 to 50 mL / min, the diameter of the atomized glue is 1 to 10 μm, and the gap between the conveyor belt and the limiting roller ranges from 0.1 to 20 cm; the material of the conveyor belt is rubber, silicone, polyvinyl chloride, polyurethane, polytetrafluoroethylene or polyethylene;
[0046] In the present invention, the temperature of the air flow blown out by the hot air drying unit in the drying, shaping / packaging integrated device is below the melting point of the ultrafine fiber porous material, and the controllable temperature range is 40-200°C; the temperature range of the air flow blown out by the cold air shaping unit is 5-20°C;
[0047] In the present invention, the hot air drying unit adopts electric heating or hot oil to heat the air. The air needs to go through a drying and impurity removal process before entering the hot air drying unit. The temperature of the air flow blown out by the hot air drying unit is below the melting point of the ultrafine fiber porous material, and the controllable temperature range is 40-200°C. After the air is heated, it is transported to the ultrafine fiber porous material on the fiber material driving roller to dry the ultrafine fiber material and soften the glue and low-melting-point fiber; the cold air drying unit adopts a condenser to cool the air. The air needs to go through a drying and impurity removal process before entering the cold air drying unit. The temperature range of the air flow blown out by the cold air setting unit is 5-20°C. After the air is cooled, it is transported to the ultrafine fiber porous material on the fiber material driving roller to anneal and heat-set the ultrafine fiber porous material; the fiber material receiving table carries the ultrafine fiber porous material that has been dried and set from the fiber material driving roller;
[0048] In the present invention, the multi-component gas delivery device can supply one or more of air, oxygen, and nitrogen, and the organic components in the ceramic precursor fiber and the carbon fiber precursor are thermally decomposed in a high-temperature gas environment to obtain a ceramic fiber material with soft / elastic properties and a carbon fiber material with few pore defects;
[0049] In the present invention, the heating temperature of the lower heating roller and the upper heating roller in the variable atmosphere heat treatment device is 60-800°C;
[0050] In the present invention, the microwave-assisted calcination technology can accelerate the decomposition of organic components, and the frequency of the microwave generator is 300-300000 MHz.
[0051] Furthermore, the ultrafine fiber porous material is selected from one or more of polymer fiber membranes, polymer fiber body materials, ceramic fiber membranes, ceramic fiber body materials, carbon fiber membranes or carbon fiber body materials.
[0052] Furthermore, the diameter of the ultrafine fiber porous material is 50 to 10000 nm.
[0053] Compared with the prior art, the present invention has the following advantages:
[0054] (1) In the solution preparation device, the raw materials are accurately weighed and automatically fed through an automatic feeding mechanism; the viscosity torque of the spinning solution is automatically sensed by a variable speed motor to automatically adjust the stirring speed of the turbine stirring roller; the high-frequency ultrasonic mechanism and the sub-high-frequency ultrasonic mechanism work together to promote the uniformity and stabilization of the spinning solution.
[0055] (2) In the gelation inhibition device, the spinning solution is heated by a variable frequency heating layer. The design of the heat insulation and thermal insulation protective layer reduces the temperature loss of the solution. At the same time, multiple screw stirring rollers are used to dynamically stir the spinning solution, ultimately achieving long-term and stable storage of the spinning solution.
[0056] (3) In the electrostatic air jet spinning module, the spinning solution forms a Taylor cone under the action of the high-voltage electrostatic field, and the high-speed airflow produces a bunching effect at the nozzle, which together with the electrostatic effect promotes the whipping and stretching of the spinning jet, significantly improving the spinning rate.
[0057] (4) The present invention is a continuous production system for ultrafine fiber porous materials based on electrostatic air spinning. When producing ultrafine fiber porous material products, it controls the properties of the spinning solution, the spinning voltage, the spinning airflow blowing speed, the ambient temperature and humidity of the spinning area, etc., to achieve switchable and controllable preparation of dense ultrafine fiber porous materials or fluffy stacked ultrafine fiber porous materials.
[0058] (5) The present invention provides a continuous production system for ultrafine fiber porous materials based on electrostatic air spinning, which transports the dense ultrafine fiber porous material intermediate to a thermal induced welding device, clamps the fiber material between a micro-matrix welding composite mechanism and a pressurizing component, and uses an ultrasonic control system to control the vibration frequency of the micro-matrix welding composite mechanism to achieve lattice welding composite of the fiber material; the fluffy stacked ultrafine fiber porous material is transported to a spray adhesive device, sprays atomized glue on the fiber material to cause adhesion between the fibers, and then clamps the fiber material between a conveyor belt and a limiting roller to control the thickness, and fiber materials of equal thickness are cut by a pneumatic cutter and stacked into fiber blocks with greater thickness.
[0059] (6) The present invention provides a continuous production system for ultrafine fiber porous materials based on electrostatic air spinning, which transports polymer fiber materials to an integrated drying, shaping / packaging device, and achieves precise control of the morphology and structure of ultrafine fiber porous materials through the alternating use of hot air and cold air; ceramic precursor fibers and carbon fiber precursors are transported to a variable atmosphere heat treatment device, and the fibers are calcined at high temperatures under different gas environments to remove organic components or carbonize them, thereby obtaining ceramic fiber materials and carbon fiber materials; microwave-assisted calcination technology can accelerate the decomposition of organic components, reduce pore defects in ceramic fiber materials, and improve the mechanical properties of materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 A schematic diagram of a continuous production system of ultrafine fiber porous materials based on electrostatic air spinning provided by the present invention;
[0061] Figure 2 for Figure 1 A partial magnified view of the solution stabilization configuration subsystem;
[0062] Figure 3 for Figure 1 A partial enlarged view of the electrostatic air jet spinning subsystem;
[0063] Figure 4 for Figure 1 A partial magnified view of the medium-fine post-processing subsystem;
[0064] The numbers in the figure are as follows: 1-solution preparation device, 11-power mechanism, 12-solution propulsion piston, 13-automatic feeding mechanism, 14-high-frequency ultrasonic mechanism, 15-sub-high-frequency ultrasonic mechanism, 16-turbine stirring roller, 17-stirring control system, 2-gelation inhibition device, 21-liquid storage tank, 22-thermal insulation and heat preservation protective layer, 23-frequency conversion heating layer, 24-stirring roller transmission mechanism, 25-screw stirring roller, 26-infusion pipeline, 3- Pressure-stabilizing air supply device, 31-air compressor, 32-air filter, 33-air storage bin, 34-temperature and humidity control chamber, 341-insulation layer, 342-freeze drying component, 343-heating component, 35-air supply pipeline, 36-electrically controlled valve, 4-electrostatic air jet spinning module, 41-liquid supply pipeline, 42-air supply pipeline, 43-spinning plate, 44-spinning nozzle, 45-high voltage power supply, 5-non-solvent control device, 51-humidity control mechanism, 6-fiber Fiber receiving / solvent recovery integrated device, 61-fiber receiving conveying curtain, 62-negative pressure suction pipeline, 63-gas-liquid filtration separation mechanism, 64-negative pressure suction pump, 7-thermal welding device, 71-air pressure control mechanism, 72-pneumatic pressure transmission rod, 73-pressurization component, 74-ultrasonic control system, 75-micro-dot matrix welding composite mechanism, 8-spray glue bonding device, 81-conveyor belt, 82-spray glue box, 83-atomizing nozzle, 84-limiting roller , 85-grabbing mechanism, 86-cutting mechanism, 9-drying and setting / packaging integrated device, 91-hot air drying unit, 92-fiber material transmission roller, 93-cold air setting unit, 94-cold air setting gun, 95-fiber material receiving platform, 10-variable atmosphere heat treatment device, 101-transmission roller, 102-multi-component gas transmission equipment, 103-lower heating roller, 104-upper heating roller, 105-microwave generator, 106-winding roller. DETAILED DESCRIPTION
[0065] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0066] Features such as component models, material names, connection structures, control methods, etc. that are not clearly stated in this technical solution shall be deemed as common technical features disclosed in the prior art.
[0067] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", "vertical", "horizontal", "top", "bottom" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0068] In the description of the present invention, "multiple" means two or more than two, unless otherwise specifically defined. In addition, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integrated connection; it can be a bolt connection or a welding connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0069] The existing electrostatic air jet technology often uses a low-solid content spinning solution for spinning, resulting in low spinning efficiency. Therefore, it is necessary to further increase the solid content of the spinning solution. However, there are problems such as high viscosity and slow mass transfer in the spinning solution preparation process, which makes it difficult for the spinning solution to be uniform and stable. The spinning solution is prone to gelation during storage, so the spinning solution is usually directly transported to the spinning nozzle for spinning, which makes it difficult to stably supply the spinning solution. In order to ensure the spinning stability during spinning, a low-density spinning nozzle is usually used, which makes it difficult to increase the spinning rate. The existing electrostatic air jet spinning equipment is still in the laboratory test stage and cannot meet the rapid and efficient large-scale manufacturing of ultrafine fiber materials. It is also difficult to accurately control the thickness, porosity and other morphological structures of the ultrafine fiber materials, resulting in the prepared materials being relatively single. At the same time, there is currently a lack of post-processing equipment for electrostatic air jet-spun ultrafine fiber porous materials. The present invention provides a continuous production system for ultrafine fiber porous materials based on electrostatic air jet spinning, and its structure can refer to Figure 1-4 ,include:
[0070] A solution stabilization configuration subsystem, comprising a gelation inhibition device 2, and a solution preparation device 1 disposed above the gelation inhibition device 2;
[0071] The electrostatic air-jet spinning subsystem comprises an electrostatic air-jet spinning module 4, a non-solvent control device 5 and a fiber receiving / solvent recovery integrated device 6 which are sequentially connected from top to bottom, and a pressure-stabilizing air supply device 3 which is connected to the electrostatic air-jet spinning module 4;
[0072] A fine post-processing subsystem, which includes a first post-processing device and a second post-processing device connected to each other, wherein the ultrafine fiber porous material spun by the electrostatic air jet spinning module 4 is transported to the first post-processing device for post-processing, and then transported to the second post-processing device for processing;
[0073] Among them, the first post-processing device includes a thermal welding device 7 and / or a spray adhesive bonding device 8; the second post-processing device includes a drying, shaping / packaging integrated device 9 and / or a variable atmosphere heat treatment device 10.
[0074] In some embodiments of the present invention, the solution preparation device 1 includes: a polymer dissolution chamber; an automatic feeding mechanism 13 arranged obliquely above the polymer dissolution chamber and connected thereto; a solution propulsion piston 12 arranged above the polymer dissolution chamber, and a power mechanism 11 connected to the solution propulsion piston 12; a high-frequency ultrasonic mechanism 14, a sub-high-frequency ultrasonic mechanism 15 and a turbine-type stirring roller 16 arranged in the polymer dissolution chamber from top to bottom, wherein the high-frequency ultrasonic mechanism is controlled by an external control system; the sub-high-frequency ultrasonic mechanism is controlled by an external control system; and the turbine-type stirring roller is controlled by a stirring control system.
[0075] In some embodiments of the present invention, the gelation inhibition device 2 includes: a liquid storage tank body 21; a stirring roller transmission mechanism 24, a variable frequency heating layer 23 and a heat insulation and thermal protection layer 22 arranged on the outer wall of the liquid storage tank body 21 from the inside to the outside; a plurality of screw stirring rollers 25 arranged in the liquid storage tank body 21, and both ends of the stirring rollers 25 radially penetrate the liquid storage tank body 21 and are connected to the stirring roller transmission mechanism 24.
[0076] In some embodiments of the present invention, the pressure-stabilizing air supply device 3 includes: an air compressor 31; an air storage bin 33, a first pipeline for connecting the air compressor 31 is arranged between the air storage bin 33 and the air filter 32 is arranged in the first pipeline; a temperature and humidity control chamber 34, a second pipeline for connecting the air compressor 31 is arranged between the temperature and humidity control chamber 34 and the air storage bin 33, an electric control valve 36 for controlling the ventilation volume is arranged on the second pipeline; an air supply pipeline 35 for connecting the temperature and humidity control chamber 34 and the electrostatic air jet spinning module 4 is arranged between the temperature and humidity control chamber 34 and the electrostatic air jet spinning module 4.
[0077] In some embodiments of the present invention, the electrostatic air jet spinning module 4 includes: a spinning plate 43; a high-voltage power supply 45 connected to the spinning plate 43, used to uniformly charge the spinning liquid; an air supply pipeline 42 arranged in the spinning plate 43, one end of the air supply pipeline 42 is connected to the pressure-stabilizing air supply device 3, and the other end branches out into a plurality of air supply branches; a liquid supply pipeline 41 arranged in the spinning plate 43, one end of the liquid supply pipeline 41 is connected to the gelation inhibition device 2, and the other end branches out into a plurality of liquid supply branches; a plurality of spinning nozzles 44 are arranged at intervals on the lower end surface of the spinning plate 43, each of the spinning nozzles 44 is provided with gas pipelines and liquid pipelines that are independent of each other and arranged, the gas pipeline is connected to the gas supply branch, and the liquid pipeline is connected to the liquid supply branch.
[0078] In some embodiments of the present invention, the non-solvent control device 5 includes a humidity control mechanism 51 located between the electrostatic air-jet spinning module 4 and the fiber receiving / solvent recovery integrated device 6 .
[0079] In some embodiments of the present invention, the fiber receiving / solvent recovery integrated device 6 includes: a fiber receiving conveying curtain 61, which is used to convey the ultrafine fiber porous material spun by the electrostatic air jet spinning module 4 to the first post-processing device for post-processing; a negative pressure suction pipe 62 arranged below the fiber receiving conveying curtain 61; a gas-liquid filtration and separation mechanism 63 connected to the negative pressure suction pipe 62; and a negative pressure suction pump 64 connected to the gas-liquid filtration and separation mechanism 63.
[0080] In some embodiments of the present invention, the thermal welding device 7 includes: a box body; a pneumatic pressure transmission rod 72 that passes through the upper end surface of the box body, and a pneumatic pressure control mechanism 71 is provided at one end of the rod that is located outside the box body, and a pressurizing component 73 is provided at one end of the rod that is located inside the box body; a micro-array welding composite mechanism 75 is arranged in the box body and below the pressurizing component 73; an ultrasonic control system 74 connected to the micro-array welding composite mechanism 75 to control the ultrasonic vibration of the micro-array welding composite mechanism to achieve material welding.
[0081] In some embodiments of the present invention, the glue spraying bonding device 8 includes a conveyor belt 81, and also includes the following arranged in sequence along the conveying direction of the conveyor belt 81: a glue spraying box 82 arranged above the conveyor belt 81, whose lower end face is provided with an atomizing nozzle 83, and there is a gap between the atomizing nozzle 83 and the upper end face of the conveyor belt 81; a limiting roller 84 with a gap between the upper end face of the conveyor belt 81; a grabbing mechanism 85, used for stacking fiber materials sprayed with glue; a cutting mechanism 86, used for cutting the stacked fiber materials from the unstacked fiber materials.
[0082] In some embodiments of the present invention, the integrated drying, shaping / packaging device 9 includes: a fiber material transmission roller 92; a hot air drying unit 91 connected to the fiber material transmission roller 92; a fiber material receiving platform 95 arranged above the fiber material transmission roller 92, and a cold air shaping unit 93 and a cold air shaping gun 94 are arranged above the fiber material receiving platform 95; specifically, the cold air shaping unit 93 is located above the fiber material receiving platform, and the cold air shaping gun 94 is located at the exit, and the cold air output is controlled from multiple directions to shape the fiber material.
[0083] In some embodiments of the present invention, the variable atmosphere heat treatment device 10 includes: a conveying roller 101, a lower heating roller 103 and a winding roller 106 arranged along the transportation direction of the fiber material; an upper heating roller 104 arranged above the lower heating roller 103; a microwave generator 105 arranged above the lower heating roller 103; and a multi-component gas conveying device 102 arranged below the lower heating roller 103.
[0084] The above embodiments can be implemented individually or in any combination of two or more. The above embodiments are described in more detail below with reference to specific examples.
[0085] Example 1
[0086] like Figure 1-4 As shown, this embodiment provides a continuous production system of ultrafine fiber porous materials based on electrostatic air spinning, including a solution stabilization configuration subsystem, an electrostatic air spinning subsystem and a fine post-processing subsystem.
[0087] The solution stabilization configuration subsystem is composed of a solution preparation device 1 and a gelation inhibition device 2. The solution preparation device 1 is mainly composed of a power mechanism 11, a solution propulsion piston 12, an automatic feeding mechanism 13, a high-frequency ultrasonic mechanism 14, a sub-high-frequency ultrasonic mechanism 15, a turbine stirring roller 16, and a stirring control system 17; the automatic feeding mechanism 13 realizes the precise weighing and automatic feeding of raw materials; the turbine stirring roller 16 is in the form of a screw type, a paddle type, an anchor type or a propulsion type; the output frequency range of the high-frequency ultrasonic mechanism 14 is 80 to 130 kHz, and the output frequency range of the sub-high-frequency ultrasonic mechanism 15 is 20 to 80 kHz; the speed of the turbine stirring roller 16 is 100 to 6000 rpm, which can adapt to the stirring of high-viscosity solutions with a viscosity range of 20 to 40000 mPa·s; when the solution is completely dissolved, the power mechanism 11 pushes the solution propulsion piston downward to inject the spinning solution into the gelation inhibition device 2; the spinning solution used is a polymer The invention relates to a solution in which a polymer is dissolved in a corresponding good solvent, or an inorganic sol, wherein the polymer is one or a combination of polysulfone, polylactic acid, polystyrene, polypropylene, polyetherimide, polyvinylidene fluoride, polyvinyl alcohol, polyethylene oxide, polypyrrolidone, polymethyl methacrylate, polyacrylonitrile, polyurethane, polyacrylic acid, polyamide, polyethylene, polyvinyl chloride, polycaprolactone, polyaniline, polyacrylamide, polyetheretherketone, polytrimethylene terephthalate, polyethylene terephthalate, polyethylene oxide, polyvinyl acetate, polyvinyl butyral, poly(m-phenylene terephthalamide), polyimide, polyhydroxybutyrate, polycarbonate, polybutylene succinate, polybenzimidazole, polyethylene glycol, polylactic acid-caprolactone, poly(p-phenylene terephthalamide), polyaramid, poly(p-phenylene vinylene) and polybenzoxazine, and the inorganic sol is one or a combination of silicon system, aluminum system, zirconium system, titanium system or a mixed system thereof.
[0088] The gelation inhibition device 2 is mainly composed of a liquid storage tank body 21, a heat insulation and heat preservation protective layer 22, a variable frequency heating layer 23, a stirring roller transmission mechanism 24, a screw stirring roller 25 and a liquid infusion pipeline 26; the thickness of the heat insulation and heat preservation protective layer 22 is 2 to 10 cm, and the heating method of the variable frequency heating layer 23 can be circulating hot oil heating, circulating hot water, circulating hot air heating or electric heating, and the output temperature range is 20 to 150 ° C; the screw stirring roller 25 is arranged in an array in the liquid storage tank body, and is selected from a rectangular array, a triangular array, a The invention relates to a mixing roller comprising a plurality of mixing rollers, and the mixing rollers are selected from the group consisting of a plurality of mixing rollers, and the mixing rollers are selected from the group consisting of a plurality of mixing rollers. The ...
[0089] The electrostatic air jet spinning subsystem includes a pressure-stabilizing air supply device 3 , an electrostatic air jet spinning module 4 , a non-solvent control device 5 and a fiber receiving / solvent recovery integrated device 6 . The pressure-stabilizing air supply device is mainly composed of an air compressor 31, an air storage bin 33, and a temperature and humidity control chamber 34; the air compressor 31 is connected to the air storage bin 33 through a gas pipeline, and an air filter 32 is arranged in the gas pipeline; the temperature and humidity control chamber 34 is connected to the air storage bin 33 through an internal pipeline, and the ventilation volume is controlled by an electric control valve; the temperature and humidity control chamber 34 is connected to the electrostatic air jet spinning module 4 through the air supply pipeline; the temperature and humidity control chamber 34 in the pressure-stabilizing air supply device 3 is mainly composed of an insulation layer 341, a freeze-drying component 342 and a heating component 343, and the temperature range of the blown air flow is -10 to 80°C; the thickness of the insulation layer 341 is 2 to 10 cm, and the heating method of the heating component 343 can be circulating hot oil heating, circulating hot water or electric heating; the material of the protective layer of the insulation layer 341 is alumina, aluminum foil composite glass fiber cloth, silicon carbide fiber, aluminum silicate, glass wool, rock wool, expanded perlite and its composite materials.
[0090] The electrostatic air jet spinning module mainly consists of a liquid supply pipe 41, an air supply pipe 42, a spinning plate 43, a spinning nozzle 44 and a high-voltage power supply 45; the air supply pipe 42 is coated on the outside of the liquid supply pipe 41 and is connected to the spinning plate 43 and the spinning nozzle 44; the spinning plate 43 is connected to the high-voltage power supply 45, and a spinning nozzle 44 is provided at the lower end; the spinning nozzle 44 is selected from a coaxial nozzle, a differential nozzle, a conical cluster nozzle, and a vortex nozzle; the spinning nozzle 44 is arranged in an array The cloth is installed under the spinning plate 43, the nozzle spacing is 20-50mm, the number of nozzles is 30-120, the nozzle diameter of the spinning nozzle 44 is 0.5-10mm, the air flow blown out of the nozzle is the air flow after impurities are filtered, the air flow velocity range is 0-25m / s, the spinneret diameter is 0.1-5mm, the liquid output of a single spinneret is 5-80mL / h, and the spinning voltage range applied to the spinning plate 43 is 0-150kV.
[0091] The non-solvent control device 5 is mainly composed of a humidity control mechanism 51, which controls the solvent volatilization rate of the spinning jet and the phase separation rate in the jet according to the requirements of the ultrafine fiber porous material morphology, and can adjust the relative humidity of the spinning area to 10-99%.
[0092] The fiber receiving / solvent recovery integrated device 6 is mainly composed of a fiber receiving conveying curtain 61, a negative pressure suction pipe 62, a gas-liquid filtration separation mechanism 63, and a negative pressure suction pump 64; the fiber receiving conveying curtain 61 is grounded, the moving speed is 0.1-10 m / min, and the material is selected from metal, plastic, rubber and fiber reinforced composite materials; the suction pressure generated by the negative pressure suction pump 64 is in the range of 0-5 MPa, and the negative pressure suction pipe 62 is composed of a main pipe connected to 3-12 branch pipes, and the branch pipes are distributed under the fiber receiving conveying curtain 61 to suck the solvent vapor in the spinning area; the gas-liquid filtration separation mechanism 63 is equipped with an activated carbon adsorption device, and the solvent vapor is separated from the solvent by the gas-liquid filtration separation mechanism 63 and dried, and finally discharged to the outdoor environment by the negative pressure suction pump 64.
[0093] The fine post-processing subsystem includes a thermal welding device 7, a spray adhesive bonding device 8, a drying and shaping / packaging integrated device 9 and a variable atmosphere heat treatment device 10. The thermal welding device 7 is mainly composed of an air pressure control mechanism 71, a pneumatic pressure transmission rod 72, a pressurizing component 73, an ultrasonic control system 74 and a micro-lattice welding composite mechanism 75; the air pressure control mechanism 71 generates sufficient air pressure to push the pressurizing component 73 connected by the pneumatic pressure transmission rod 72, and the pressure range generated is 2 to 8 MPa, the frequency of the sound wave output by the ultrasonic control system 74 can be adjusted in the range of 5 to 30 kHz, and the lattice of the micro-lattice welding composite mechanism 75 is selected from honeycomb, grid, triangle and rhombus.
[0094] The glue spraying bonding device 8 is mainly composed of a conveyor belt 81, a glue spraying box 82, an atomizing nozzle 83, a limiting roller 84, a grabbing mechanism 85 and a cutting mechanism 86; the glue spraying amount of a single atomizing nozzle ranges from 0 to 50 mL / min, the diameter of the atomized glue is 1 to 10 μm, the fiber material is sandwiched between the conveyor belt 81 and the limiting roller 84, and the thickness of the ultrafine fiber porous material is controlled by adjusting the distance between the conveyor belt 81 and the limiting roller 84. The gap between the conveyor belt 81 and the limiting roller 84 ranges from 0.1 to 20 cm; the width of the conveyor belt 81 ranges from 0.8 to 3 m, the conveying speed is 0.1 to 50 m / min, and the material of the conveyor belt 81 is rubber, silicone, polyvinyl chloride, polyurethane, polytetrafluoroethylene or polyethylene. In this embodiment, the grabbing mechanism 85 and the cutting mechanism 86 are prior art and are not the improvement of the present invention, so the specific structure and use method are not repeated here.
[0095] The drying and shaping / packaging integrated device 9 is mainly composed of a hot air drying unit 91, a fiber material driving roller 92, a cold air shaping unit 93, a cold air shaping gun 94, and a fiber material receiving platform 95; the hot air drying unit 91 uses electric heating or hot oil to heat the air, and the air needs to go through a drying and impurity removal process before entering the hot air drying unit 91. The air flow temperature blown out by the hot air drying unit 91 is below the melting point of the ultrafine fiber porous material, and the controllable temperature range is 40-200°C. After the air is heated, it is blown to the ultrafine fibers on the fiber material driving roller 92. The porous material is transported to dry the ultrafine fiber material and soften the glue and low-melting-point fiber; the cold air drying unit 93 uses a condenser to cool the air, and the air needs to go through a drying and impurity removal process before entering the cold air drying unit 93. The air flow temperature range of the cold air setting unit 93 is 5 to 20°C. After the air is cooled, it is transported to the ultrafine fiber porous material on the fiber material driving roller 92 to anneal and heat-set the ultrafine fiber porous material; the fiber material receiving platform 95 carries the ultrafine fiber porous material that has been dried and set from the fiber material driving roller 92.
[0096] The atmosphere-changing heat treatment device 10 is mainly composed of a conveying roller 101, a multi-component gas conveying device 102, a lower heating roller 103, an upper heating roller 104, a microwave generator 105 and a winding roller 106; the multi-component gas conveying device 102 can supply one or more of air, oxygen and nitrogen, and the organic components in the ceramic precursor fiber and the carbon fiber precursor are thermally decomposed in a high-temperature gas environment to obtain a ceramic fiber material with soft / elastic properties and a carbon fiber material with fewer pore defects; the heating temperature of the lower heating roller 103 and the upper heating roller 104 in the atmosphere-changing heat treatment device 10 is 60-800°C; the microwave-assisted calcination technology can accelerate the decomposition of organic components, and the frequency of the microwave generator 105 is 300-300000MHz.
[0097] Application Example 1
[0098] The ultrafine fiber membrane was prepared using the continuous production system in Example 1, and the preparation steps were as follows:
[0099] The first step: turn on the turbine stirring roller 16, set the rotation speed of the turbine stirring roller 16 to 6000rpm, and put 6kg of N,N-dimethylformamide and 5kg of polyurethane from the automatic feeding mechanism 13 into the solution preparation device 1 in sequence; at the same time, set the output frequency of the high-frequency ultrasonic mechanism 14 to 130kHz, and the output frequency of the sub-high-frequency ultrasonic mechanism 15 to 80kHz, so that the polymer is dissolved under the joint action of the turbine stirring roller 16, the high-frequency ultrasonic mechanism 14, and the sub-high-frequency ultrasonic mechanism 15; then turn on the power mechanism 11 to drive the solution propulsion piston to move downward, so that the dissolved polyurethane solution flows into the liquid storage tank body 21 of the gelation inhibition device 2; turn on the variable frequency heating layer 23, set the tank body temperature to 150°C, set 10 screw stirring rollers 25 equidistantly arranged in a diamond array in the liquid storage tank body 21, the spacing between the stirring rollers is 10cm, the rotation speed of the screw stirring rollers 25 is 700rpm, and the polyurethane solution can be stably stored in the liquid storage tank body 21 for 400 hours without gelation.
[0100] Step 2: The solution is introduced into the infusion pipe 26. Under a certain pressure, the solution flows from the infusion pipe 26 to the liquid supply pipe 41 in the electrostatic air jet spinning module 4; the spacing between the spinning nozzles 44 is set to 20 mm, and a coaxial nozzle with a jet diameter of 2.1 mm and a spinneret diameter of 0.7 mm is selected. 150 spinning nozzles 44 are distributed on a single spinning plate, 16 spinning plates 43 are used, and the liquid output of a single spinneret is set to 5 ml / h. The air flow rate in a single spinneret is 25 m / s, and the air flow temperature is -10°C. A spinning voltage of 150 kV is applied to each spinning plate 43, and the humidity control mechanism 51 is turned on to adjust the relative ambient humidity of the spinning area to 40%. The polyurethane spinning solution is polarized and stretched under the action of voltage and airflow, and deposited on the fiber receiving and conveying curtain 61 to obtain a dense ultrafine fiber porous material intermediate. The conveying speed of the fiber receiving and conveying curtain 61 is set to 10m / min, the suction pressure generated by the negative pressure suction pump 64 is set to 2MPa, and 12 negative pressure suction pipes are installed under the fiber receiving and conveying curtain 61 to suck the solvent vapor in the spinning area. The gas-liquid filtration separation mechanism 63 is equipped with an activated carbon adsorption device. The solvent vapor is separated from the solvent by the gas-liquid filtration separation mechanism 63 and dried, and finally discharged to the outdoor environment by the negative pressure suction pump 64.
[0101] Step 3: The ultrafine fiber porous material intermediate is further transported on the fiber receiving conveying curtain 61 to the thermal fusion device 7 for fine post-processing. The sound wave frequency output by the ultrasonic control system is set to 30kHz, and a hexagonal honeycomb lattice with an equivalent diameter of 0.2mm is selected. The pressure of the air pressure control mechanism 71 is set to 8MPa. The air pressure control mechanism 71 is connected to the pneumatic pressure transmission rod 72 to push the pressurizing component 73 to pressurize the ultrafine fiber porous material intermediate. The ultrafine fibers between the pressurizing component 73 and the micro-lattice fusion composite mechanism 75 are melt-bonded under the action of ultrasound and pressure.
[0102] Step 4: The ultrafine fiber porous material intermediate after thermal fusion treatment is transported to the drying, shaping / packaging integrated device 9 for drying, shaping and packaging. The temperature of the hot air drying unit 91 is set to 40°C, and the air after drying and impurity removal enters the hot air drying unit 91. After the air is heated, it is transported to the ultrafine fiber porous material intermediate on the fiber material transmission roller 92 to dry the ultrafine fiber porous material intermediate. The transmission speed of the fiber material transmission roller 92 is 5m / min; as the fiber material transmission roller 92 rotates, the ultrafine fiber porous material intermediate enters the cold air cooling and shaping area. The cold air temperature is 20°C, so that the ultrafine fiber porous material intermediate is quickly cooled and shaped. The cooled fiber material is transported to the fiber material receiving station 95 for packaging, and finally a dense ultrafine fiber porous material with good morphology is obtained, and the average fiber diameter is 50nm.
[0103] Application Example 2
[0104] The ultrafine fiber body material is prepared using the continuous production system in Example 1, and the preparation steps are as follows:
[0105] The first step: turn on the turbine stirring roller 16, set the rotation speed of the turbine stirring roller 16 to 2500rpm, and sequentially feed 5kg of N,N-dimethylacetamide, 2.5kg of polyurethane, and 1.5kg of polysulfone from the automatic feeding mechanism 13 into the solution preparation device 1; at the same time, set the output frequency of the high-frequency ultrasonic mechanism 14 to 70kHz, and the output frequency of the sub-high-frequency ultrasonic mechanism 15 to 40kHz, and dissolve the polymer under the joint action of the turbine stirring roller 16, the high-frequency ultrasonic mechanism 14, and the sub-high-frequency ultrasonic mechanism 15; Then, the power mechanism 11 is turned on to drive the solution propulsion piston to move downward, so that the dissolved high-viscosity polyurethane / polysulfone solution flows into the liquid storage tank body 21 of the gelation inhibition device 2; the variable frequency heating layer 23 is turned on for heating, and the tank body temperature is set to 80°C. Six screw stirring rollers 25 are arranged equidistantly in a rectangular array in the liquid storage tank body 21, and the spacing between the stirring rollers is 18 cm. The rotation speed of the screw stirring rollers 25 is 500 rpm. The polyurethane / polysulfone solution can be stably stored in the liquid storage tank body 21 for 220 hours without gelation.
[0106] Step 2: The solution is introduced into the infusion pipe 26. Under a certain pressure, the solution flows from the infusion pipe 26 to the liquid supply pipe 41 in the electrostatic air jet spinning module 4. The spacing between the spinning nozzles 44 is set to 25 mm. A vortex spinning nozzle with a jet diameter of 10 mm and a spinneret diameter of 5 mm is selected. 64 spinning nozzles 44 are distributed on a single spinning plate. Six spinning plates 43 are used. The liquid output of a single spinneret is set to 80 ml / h. The air flow rate in a single spinneret is 11 m / s, and the air flow temperature is 80°C. A spinning voltage of 60 kV is applied to each spinning plate 43. The humidity control mechanism 51 is turned on to adjust the relative ambient humidity of the spinning area to 90%. The polyurethane / polysulfone spinning solution is polarized and stretched under the action of voltage and airflow, and rapidly phase-separated due to humidity to form curly fibers, which are accumulated to form a fluffy structure of an ultrafine fiber porous material intermediate. The conveying speed of the fiber receiving and conveying curtain 61 is set to 0.1m / min, and the suction pressure generated by the negative pressure suction pump 64 is set to 0.1MPa. Three negative pressure suction pipes are installed under the fiber receiving and conveying curtain 61 to suck the solvent vapor in the spinning area. The gas-liquid filtration separation mechanism 63 is equipped with an activated carbon adsorption device. The solvent vapor is separated from the solvent by the gas-liquid filtration separation mechanism 63 and dried, and finally discharged to the outdoor environment by the negative pressure suction pump 64.
[0107] Step 3: The ultrafine fiber porous material intermediate is further transported on the fiber receiving conveying curtain 61 to the glue spraying bonding device 8 for fine post-processing. The conveying speed of the conveyor belt 81 is set to 3m / min, the rectangular glue spraying box 82 supplies glue, the number of atomizing nozzles 83 is 5, the nozzle diameter is 0.5mm, and the glue spraying amount of a single nozzle is 50mL / min. Then, the fiber material is sandwiched between the conveyor belt 81 and the limiting roller 84, and a gap of 4cm is left between the conveyor belt 81 and the limiting roller 84, that is, the thickness of the ultrafine fiber porous material intermediate is controlled to 4cm; then the cutting mechanism 86 cuts the ultrafine fiber porous material intermediate.
[0108] Step 4: The ultrafine fiber porous material intermediate after the post-treatment of spray glue bonding is transported to the drying, shaping / packaging integrated device 9 for drying, shaping and packaging. The temperature of the hot air drying unit 91 is set to 120°C, and the air after drying and impurity removal enters the hot air drying unit 91. After the air is heated, it is transported to the ultrafine fiber porous material intermediate on the fiber material transmission roller 92 to dry the ultrafine fiber material and soften the glue and low melting point fiber. The transmission speed of the fiber material transmission roller 92 is 4m / min; then the ultrafine fiber porous material intermediate enters the cold air cooling and shaping area, and the cold air temperature is 5°C, so that the softened ultrafine fiber porous material intermediate is quickly annealed, cooled and shaped. The cooled fiber material is transported to the fiber material receiving station 95 for packaging, and finally a fluffy ultrafine fiber porous material with good morphology is obtained, and the average fiber diameter is 10000nm.
[0109] Application Example 3
[0110] The ultrafine fiber body material is prepared using the continuous production system in Example 1, and the preparation steps are as follows:
[0111] The first step is to turn on the turbine stirring roller 16, set the speed of the turbine stirring roller 16 to 100 rpm, first add aluminum isopropoxide and ethylene dichloride, then add acetic acid, acetylacetone and titanium isopropoxide in sequence, and finally add water into the solution preparation device 1; at the same time, set the output frequency of the high-frequency ultrasonic mechanism 14 to 80 kHz, the output frequency of the sub-high-frequency ultrasonic mechanism 15 to 20 kHz, and dissolve the polymer under the joint action of the turbine stirring roller 16, the high-frequency ultrasonic mechanism 14 and the sub-high-frequency ultrasonic mechanism 15; then The power mechanism 11 is turned on to drive the solution propulsion piston to move downward, so that the dissolved silicon-based inorganic sol flows into the liquid storage tank body 21 of the gelation inhibition device 2; the variable frequency heating layer 23 is turned on for heating, and the tank body temperature is set to 20°C. Three screw-type stirring rollers 25 equidistantly arranged in a triangular array are set in the liquid storage tank body 21. The spacing between the stirring rollers is 25 cm, and the rotation speed of the screw-type stirring rollers 25 is 200 rpm. The silicon-based inorganic sol can be stably stored in the liquid storage tank body 21 for 310 hours without gelation.
[0112] Step 2: The silicon-based inorganic sol is introduced into the liquid infusion pipe 26. Under a certain pressure, the silicon-based inorganic sol flows from the liquid infusion pipe 26 to the liquid supply pipe 41 in the electrostatic air jet spinning module 4; the spacing between the spinning nozzles 44 is set to 25 mm, and a conical spinning nozzle with a jet diameter of 0.5 mm and a spinneret diameter of 0.1 mm is selected. 88 spinning nozzles 44 are distributed on a single spinning plate, and 8 spinning plates 43 are used. The liquid output of a single spinneret is set to 60 ml / h, the air flow rate in a single spinneret is 5 m / s, and the air flow temperature is 25°C. A spinning voltage of 40 kV is applied to each spinning plate 43, and the humidity control mechanism 51 is turned on to adjust the relative ambient humidity of the spinning area to 30%. The silicon-based inorganic sol is polarized and stretched under the action of voltage and airflow, and due to the humidity-induced rapid phase separation and the rapid activation of the inorganic sol, curly fibers are formed, and the ultrafine fiber porous material intermediate with a fluffy structure is accumulated. The conveying speed of the fiber receiving and conveying curtain 61 is set to 2m / min, and the suction pressure generated by the negative pressure suction pump 64 is set to 5MPa. Five negative pressure suction pipes are installed under the fiber receiving and conveying curtain 61 to suck the solvent vapor in the spinning area. The gas-liquid filtration separation mechanism 63 is equipped with an activated carbon adsorption device. The solvent vapor is separated from the solvent by the gas-liquid filtration separation mechanism 63 and dried, and finally discharged to the outdoor environment by the negative pressure suction pump 64.
[0113] Step 3: The ultrafine fiber porous material intermediate is further transported on the fiber receiving conveying curtain 61 to the glue spraying bonding device 8 for fine post-processing. The conveying speed of the conveyor belt 81 is set to 1m / min, the rectangular glue spraying box 82 supplies glue, the number of atomizing nozzles 83 is 3, the nozzle diameter is 0.5mm, and the glue spraying amount of a single nozzle is 12mL / min. Then, the fiber material is sandwiched between the conveyor belt 81 and the limiting roller 84, and a gap of 3cm is left between the conveyor belt 81 and the limiting roller 84, that is, the thickness of the ultrafine fiber porous material intermediate is controlled to 3cm, and then the cutting mechanism 86 cuts the fiber material.
[0114] Step 4: The ultrafine fiber porous material intermediate after spraying and bonding is transported to the atmosphere-changing heat treatment device 10 for high-temperature calcination. The frequency of the microwave generator 105 is set to 300000 MHz, and the organic components in the fiber are pre-broken under the action of microwaves; the multi-component gas conveying device 102 supplies oxygen, and the temperature of the upper heating roller 104 and the lower heating roller 103 is set to 800°C. The organic components are thermally decomposed under high temperature environment, and the transmission speed of the conveying roller 101 is 2m / min. The generated waste gas is discharged from the gas outlet; the inorganic components in the fiber undergo grain growth at high temperature to obtain a ceramic fiber material with soft / elastic properties, and the average fiber diameter is 700nm, and finally the winding roller is wound and stored.
[0115] Application Example 4
[0116] The ultrafine fiber membrane was prepared using the continuous production system in Example 1, and the preparation steps were as follows:
[0117] The first step is to start the turbine stirring roller 16, set the speed of the turbine stirring roller 16 to 4000 rpm, and sequentially feed 7 kg of N,N-dimethylformamide and 5.5 kg of polyacrylonitrile from the automatic feeding mechanism 13 into the solution preparation device 1; at the same time, set the output frequency of the high-frequency ultrasonic mechanism 14 to 50 kHz, and the output frequency of the sub-high-frequency ultrasonic mechanism 15 to 30 kHz, and dissolve the polymer under the joint action of the turbine stirring roller 16, the high-frequency ultrasonic mechanism 14, and the sub-high-frequency ultrasonic mechanism 15; then start the power mechanism 11 to drive The solution pushes the piston to move downward, so that the dissolved high-viscosity polyacrylonitrile solution flows into the liquid storage tank body 21 of the gelation inhibition device 2; the heating method of the liquid storage tank body 21 is circulating hot air heating, and the variable frequency heating layer 23 is turned on for heating, and the tank body temperature is set to 120°C. Six screw stirring rollers 25 arranged equidistantly in a honeycomb shape are arranged in the liquid storage tank body 21, and the spacing between the stirring rollers is 10 cm. The rotation speed of the screw stirring rollers 25 is 400 rpm. The polyacrylonitrile solution can be stably stored in the liquid storage tank body 21 for 300 hours without gelation.
[0118] Step 2: The solution is introduced into the infusion pipe 26. Under a certain pressure, the solution flows from the infusion pipe 26 to the liquid supply pipe 41 in the electrostatic air jet spinning module 4; the spacing between the spinning nozzles 44 is set to 50 mm, and a differential nozzle with an air jet diameter of 10 mm and a spinneret diameter of 5 mm is selected. 40 spinning nozzles 44 are distributed on a single spinning plate, and 8 spinning plates 43 are used. The liquid output of a single spinneret is set to 30 ml / h, the air flow rate in a single spinneret is 18 m / s, and the air flow temperature is 40°C. A spinning voltage of 50 kV is applied to each spinning plate 43, and the humidity control mechanism 51 is turned on to adjust the relative ambient humidity of the spinning area to 50%. The polyacrylonitrile spinning solution is polarized and stretched under the action of voltage and airflow, and deposited on the fiber receiving and conveying curtain 61 to obtain a dense ultrafine fiber porous material intermediate. The conveying speed of the fiber receiving and conveying curtain 61 is set to 0.5m / min, and the suction pressure generated by the negative pressure suction pump 64 is set to 1MPa. Eight negative pressure suction pipes are installed under the fiber receiving and conveying curtain 61 to suck the solvent vapor in the spinning area. The gas-liquid filtration separation mechanism 63 is equipped with an activated carbon adsorption device. The solvent vapor is separated from the solvent by the gas-liquid filtration separation mechanism 63 and dried, and finally discharged to the outdoor environment by the negative pressure suction pump 64.
[0119] Step 3: The ultrafine fiber porous material intermediate is further transported on the fiber receiving conveying curtain 61 to the thermal fusion device 7 for fine post-processing. The sound wave frequency output by the ultrasonic control system is set to 5kHz, and a grid-shaped dot matrix with an equivalent diameter of 0.2mm is selected. The pressure of the air pressure control mechanism 71 is set to 2MPa. The air pressure control mechanism 71 is connected to the pneumatic pressure transmission rod 72 to push the pressurizing component 73 to pressurize the ultrafine fiber porous material intermediate. The ultrafine fibers between the pressurizing component 73 and the micro-dot matrix welding composite mechanism 75 are melt-bonded under the action of ultrasound and pressure.
[0120] Step 4: The ultrafine fiber porous material intermediate after thermal fusion treatment is transported to the atmosphere-changing heat treatment device 10 for high-temperature calcination. The frequency of the microwave generator 105 is set to 300MHz, and the organic components in the fiber are pre-broken under the action of microwaves; the multi-component gas conveying device 102 supplies nitrogen, the temperature of the upper heating roller 104 and the lower heating roller 103 is set to 600°C, and the transmission speed of the conveying roller 101 is 1m / min. The organic components are carbonized in a high-temperature oxygen-free environment to obtain a carbon fiber material with fewer pore defects, and the average fiber diameter is 350nm, and finally the winding roller is wound and stored.
[0121] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A continuous production system of ultrafine fiber porous materials based on electrostatic air-jet spinning. It is characterized in that include: A solution stabilization configuration subsystem, comprising a gelation inhibition device (2), and a solution preparation device (1) disposed above the gelation inhibition device (2); An electrostatic air-jet spinning subsystem comprises an electrostatic air-jet spinning module (4), a non-solvent control device (5) and a fiber receiving / solvent recovery integrated device (6) which are sequentially connected from top to bottom, and a pressure-stabilizing air supply device (3) which is connected to the electrostatic air-jet spinning module (4); A fine post-processing subsystem, comprising a first post-processing device and a second post-processing device connected to each other, wherein the ultrafine fiber porous material spun by the electrostatic air jet spinning module (4) is transported to the first post-processing device for post-processing, and then transported to the second post-processing device for processing; Wherein, the first post-processing device comprises a thermal welding device (7) and / or a spray adhesive bonding device (8); the second post-processing device comprises a drying, shaping / packaging integrated device (9) and / or a variable atmosphere heat treatment device (10).
2. According to claim 1, a continuous production system of ultrafine fiber porous materials based on electrostatic air spinning, It is characterized in that The solution preparation device (1) comprises: polymer dissolution cavity; An automatic feeding mechanism (13) is disposed obliquely above the polymer dissolving chamber and is in communication with the chamber; A solution advancing piston (12) disposed above the polymer dissolving chamber, and a power mechanism (11) connected to the solution advancing piston (12); A high-frequency ultrasonic mechanism (14), a sub-high-frequency ultrasonic mechanism (15) and a turbine-type stirring roller (16) are sequentially arranged in the polymer dissolving cavity from top to bottom.
3. According to claim 1, a continuous production system of ultrafine fiber porous materials based on electrostatic air spinning, It is characterized in that The gelation inhibition device (2) comprises: Liquid storage tank body (21); A stirring roller transmission mechanism (24), a variable frequency heating layer (23) and a heat insulation and thermal protection layer (22) are sequentially arranged on the outer wall of the liquid storage tank body (21) from the inside to the outside; A plurality of screw-type stirring rollers (25) are arranged in the liquid storage tank body (21), and both ends of the stirring rollers (25) penetrate the liquid storage tank body (21) in the radial direction of the liquid storage tank body (21) and are connected to the stirring roller transmission mechanism (24).
4. According to claim 1, a continuous production system of ultrafine fiber porous materials based on electrostatic air spinning, It is characterized in that The pressure-stabilizing gas supply device (3) comprises: Air compressor (31); An air storage bin (33) is provided with a first pipeline for connecting the air storage bin (33) and the air compressor (31), wherein an air filter (32) is provided in the first pipeline; A temperature and humidity control chamber (34) is connected to the air storage bin (33) by a second pipeline for connecting the two, and an electric control valve (36) for controlling the ventilation volume is provided on the second pipeline; an air supply pipeline (35) for connecting the temperature and humidity control chamber (34) and the electrostatic air jet spinning module (4) is provided between the temperature and humidity control chamber (34) and the electrostatic air jet spinning module (4); The electrostatic air jet spinning module (4) comprises: Spinning plate (43); a high voltage power supply (45) connected to the spinneret (43); An air supply pipeline (42) is arranged in the spinning plate (43), wherein one end of the air supply pipeline (42) is connected to the pressure-stabilizing air supply device (3), and the other end branches into a plurality of air supply branches; A liquid supply pipeline (41) is arranged in the spinning plate (43), wherein one end of the liquid supply pipeline (41) is connected to the gelation inhibition device (2), and the other end branches into a plurality of liquid supply branches; A plurality of spinning nozzles (44) are arranged at intervals on the lower end surface of the spinning plate (43), each of the spinning nozzles (44) is provided with a gas pipeline and a liquid pipeline which are independent and arranged in an array, the gas pipeline is connected to the gas supply branch, and the liquid pipeline is connected to the liquid supply branch; The non-solvent control device (5) comprises a moisture control mechanism (51) located between the electrostatic air-jet spinning module (4) and the fiber receiving / solvent recovery integrated device (6); The fiber receiving / solvent recovery integrated device (6) comprises: A fiber receiving conveying curtain (61) is used to convey the ultrafine fiber porous material spun by the electrostatic air jet spinning module (4) to a first post-processing device for post-processing; A negative pressure suction pipe (62) disposed below the fiber receiving and conveying curtain (61); A gas-liquid filtering and separating mechanism (63) connected to the negative pressure suction pipeline (62); A negative pressure suction pump (64) connected to the gas-liquid filtering and separating mechanism (63).
5. According to claim 1, a continuous production system of ultrafine fiber porous materials based on electrostatic air spinning, It is characterized in that The thermal welding device (7) comprises: Box; A pneumatic pressure transmission rod (72) passing through the upper end surface of the box body, wherein the end outside the box body is provided with a pneumatic pressure control mechanism (71), and the end inside the box body is provided with a pressurizing component (73); A micro-lattice welding composite mechanism (75) disposed in the box and below the pressurizing component (73); An ultrasonic control system (74) connected to the micro-lattice welding composite mechanism (75) controls the ultrasonic vibration of the micro-lattice welding composite mechanism to achieve material welding; The glue spraying bonding device (8) comprises a conveyor belt (81), and further comprises: A glue spray box (82) is arranged above the conveyor belt (81), and an atomizing nozzle (83) is arranged on the lower end surface thereof, and a gap exists between the atomizing nozzle (83) and the upper end surface of the conveyor belt (81); A limiting roller (84) having a gap between itself and the upper end surface of the conveyor belt (81); A grabbing mechanism (85) for stacking the fiber material sprayed with glue; The cutting mechanism (86) is used to cut the fiber materials stacked together from the fiber materials not stacked together.
6. According to claim 1, a continuous production system of ultrafine fiber porous materials based on electrostatic air spinning, It is characterized in that The drying, shaping and packaging integrated device (9) comprises: Fiber material transmission roller (92); A hot air drying unit (91) connected to the fiber material driving roller (92); A fiber material receiving platform (95) is arranged above the fiber material driving roller (92), and a cold air setting unit (93) and a cold air setting gun (94) are arranged above the fiber material receiving platform (95); specifically, the cold air setting unit (93) is located above the fiber material receiving platform, and the cold air setting gun (94) is located at the outlet, and the cold air output is controlled from multiple directions to set the fiber material; The atmosphere-changing heat treatment device (10) comprises: A conveying roller (101), a lower heating roller (103) and a winding roller (106) arranged along the transport direction of the fiber material; An upper heating roller (104) disposed above the lower heating roller (103); A microwave generator (105) disposed above the lower heating roller (103); A multi-component gas delivery device (102) is arranged below the lower heating roller (103).
7. A method for preparing ultrafine fiber porous material, It is characterized in that The preparation is carried out using the continuous production system as described in any one of claims 1 to 6, and the preparation method comprises the following steps: Step 1: Turn on the turbine stirring roller (16) and sequentially feed the raw materials from the automatic feeding mechanism (13) into the solution preparation device (1); dissolve the raw materials under the joint action of the turbine stirring roller (16), the high-frequency ultrasonic mechanism (14) and the sub-high-frequency ultrasonic mechanism (15); then turn on the power mechanism (11) to drive the solution propulsion piston to move downward, so that the raw material solution flows into the liquid storage tank (21) of the gelation inhibition device (2); turn on the variable frequency heating layer (23) for heating, and set a plurality of screw stirring rollers (25) in the liquid storage tank (21), so that the raw material solution can be stably stored in the liquid storage tank (21) for at least 200 hours without gelation; Step 2: Turn on the humidity control mechanism (51) to adjust the relative humidity of the spinning area, and then pass the raw material solution into the liquid infusion pipe (26). Under the action of pressure, the solution flows from the liquid infusion pipe (26) to the liquid supply pipe (41) in the electrostatic air jet spinning module (4), and is extruded into filaments through the spinning nozzle (44). The raw material solution is polarized and stretched under the action of voltage and airflow to obtain an ultrafine fiber porous material intermediate; multiple negative pressure suction pipes (62) are installed under the fiber receiving and conveying curtain (61) to suck the solvent vapor in the spinning area, and the gas-liquid filtration separation mechanism (63) is equipped with an adsorption device. The solvent vapor is separated from the solvent vapor by the gas-liquid filtration separation mechanism (63) and dried, and finally discharged to the outdoor environment by the negative pressure suction pump (64); Step 3: Select one of the following: ① The ultrafine fiber porous material is continuously transported on the fiber receiving conveying curtain (61) to the thermal fusion bonding device (7) for fine post-processing. The air pressure control mechanism (71) is connected to the pneumatic pressure transmission rod (72) to push the pressurizing component (73) to pressurize the ultrafine fiber porous material intermediate. The ultrafine fibers between the pressurizing component (73) and the micro-lattice fusion bonding composite mechanism (75) are melt-bonded under the action of ultrasound and pressure to obtain an ultrafine fiber porous material intermediate that has undergone thermal fusion post-processing. ② The ultrafine fiber porous material is further conveyed on the fiber receiving conveying curtain (61) to the glue spraying and bonding device (8) for fine post-processing. The glue in the glue spraying box (82) is evenly sprayed on the inside and outside of the ultrafine fiber porous material through the atomizing nozzle (83). Then, the ultrafine fiber porous material is clamped between the conveyor belt (81) and the limiting roller (84). The fiber material is cut by the cutting mechanism (86) to obtain an ultrafine fiber porous material intermediate that has been post-processed by glue spraying and bonding. Step 4: Choose one of the following: ① The ultrafine fiber porous material intermediate that has been subjected to thermal fusion treatment or the ultrafine fiber porous material intermediate that has been subjected to glue spraying and bonding treatment is transported to a drying, shaping / packaging integrated device (9) for drying, shaping and packaging; the air after drying and impurity removal enters a hot air drying unit (91), and the air is heated and then transported to the ultrafine fiber porous material intermediate on a fiber material transmission roller (92) to dry the ultrafine fiber material intermediate and soften the glue and low melting point fiber; Then, the ultrafine fiber porous material intermediate enters a cold air cooling and shaping area, so that the softened ultrafine fiber porous material intermediate is quickly annealed, cooled and shaped. The cooled fiber material intermediate is transported to a fiber material receiving station (95) for packaging, thereby obtaining an ultrafine fiber porous material. ② The ultrafine fiber porous material intermediate that has been post-processed by thermal fusion or the ultrafine fiber porous material intermediate that has been post-processed by spray bonding is transported to a variable atmosphere heat treatment device (10) for high-temperature calcination. The organic components in the fiber are pre-broken under the action of microwaves. The multi-component gas delivery equipment (102) supplies one or more of air, oxygen or nitrogen. The organic components are thermally decomposed or carbonized in a high-temperature environment. If there are inorganic components in the fiber, the inorganic components undergo grain growth in a high-temperature environment to obtain an ultrafine fiber porous material.
8. The method for preparing a porous ultrafine fiber material according to claim 7, It is characterized in that The preparation method satisfies at least one of the following conditions: ① The output frequency range of the high-frequency ultrasonic mechanism (14) is 80 to 130 kHz; ② The output frequency range of the sub-high frequency ultrasonic mechanism (15) is 20 to 80 kHz; ③ The turbine stirring roller (16) is located inside the solution preparation device (1) and has a rotation speed of 100 to 6000 rpm, which is suitable for stirring high-viscosity solutions with a viscosity range of 20 to 40000 mPa·s; ④ The spinning solution can remain in an ungelled state for 200 to 400 hours; ⑤ The rotation speed of the screw stirring rollers (25) is 200 to 700 rpm, the number of the screw stirring rollers (25) is 2 to 10, and the arrangement is selected from one or more of a rectangular array, a triangular array, a trapezoidal array, a diamond array, a fractal array or a honeycomb array; ⑥ The temperature and humidity control chamber (34) in the pressure-stabilizing air supply device (3) comprises an insulating layer (341), and a freeze-drying component (342) and a heating component (343) arranged in the insulating layer (341), wherein the freeze-drying component (342) is located below the heating component (343), and the temperature range of the air flow blown out by the pressure-stabilizing air supply device (3) is -10 to 80°C ⑦ The spinning nozzle (44) in the electrostatic air jet spinning module (4) is selected from one or more of a coaxial nozzle, a differential nozzle, a conical beam nozzle or a vortex nozzle; the spacing between two adjacent spinning nozzles (44) is 20 to 50 mm; the number of the spinning nozzles (44) is 30 to 120; the diameter of the jet nozzle of the spinning nozzle (44) is 0.5 to 10 mm, and the diameter of the spinneret hole is 0.1 to 5 mm; the air flow velocity of the jet nozzle is 0 to 25 m / s; the liquid output of each spinneret hole is 5 to 80 ml / h; the spinning voltage range is 0 to 150 kV; ⑧ The relative humidity of the spinning area is adjusted to 10-99%; ⑨ The fiber receiving conveying curtain (61) in the fiber receiving / solvent recovery integrated device (6) is grounded, and the material is selected from one or more of metal, plastic, rubber or fiber reinforced composite material, and the moving speed of the fiber receiving conveying curtain (61) is 0.1-10 m / min; ⑩ The frequency of the sound waves output by the ultrasonic control system (74) in the thermal welding device (7) can be adjusted in the range of 5 to 30 kHz, and the lattice of the micro-lattice welding composite structure (75) is selected from one or more of a honeycomb shape, a grid shape, a triangle shape or a diamond shape; The glue spraying amount of a single atomizing nozzle (83) in the glue spraying bonding device (8) is in the range of 0 to 50 mL / min, the diameter of the atomized glue is 1 to 10 μm, and the gap between the conveyor belt (81) and the limiting roller (84) is in the range of 0.1 to 20 cm; The temperature of the air flow blown out by the hot air drying unit (91) in the drying, shaping / packaging integrated device (9) is below the melting point of the ultrafine fiber porous material, and the controllable temperature range is 40 to 200°C; the temperature of the air flow blown out by the cold air shaping unit (93) is in the range of 5 to 20°C; The heating temperature of the lower heating roller (103) and the upper heating roller (104) in the variable atmosphere heat treatment device (10) is 60 to 800°C; The frequency of the microwave generator (105) is 300-300000 MHz.
9. The method for preparing a porous ultrafine fiber material according to claim 7, It is characterized in that The ultrafine fiber porous material is one or more of a polymer fiber membrane, a polymer fiber body material, a ceramic fiber membrane, a ceramic fiber body material, a carbon fiber membrane or a carbon fiber body material.
10. The method for preparing a porous ultrafine fiber material according to claim 9, It is characterized in that The diameter of the ultrafine fiber porous material is 50 to 10000 nm.
Citation Information
Patent Citations
Automatic-rotating electrostatic spinning device assisted by high-pressure airflow and provided with nozzle
CN103628149A
Method and device for producing polymer nano fibers through high-speed airflow and high-voltage static
CN104313708A
Gap-adjustable electrostatic-spinning nozzle and array-type spinning system
CN105543985A
Arc-shaped array electrostatic spinning sprayer with sheath gas restriction function
CN109267160A
Device and method using melt-blow and electrostatic spinning to prepare composite ultrafine fiber bundle
CN106555277A
Cited By
Precise control system and method for wool type fiber spinning process
CN120509218A
Cold-proof warm-keeping clothes fabric as well as preparation method and application thereof
CN121019060A
Large-scale continuous manufacturing system for elastic ceramic nanofiber flocculus
CN122189943A
Large-scale continuous manufacturing system for porous nanofiber-based elastic ceramic flocculus
CN122485018A