Polyglycolic acid-containing resin composition and film comprising same
By combining polyglycolic acid, zinc-containing ionomer and vinyl terpolymer, and adjusting the proportion of the resin composition, the problems of high melting point and low melt strength of PGA resin in film processing are solved, and high gas barrier is achieved. Breakable, biodegradable and processable membrane, suitable for environmentally friendly materials.
Patent Information
- Application Number
- CN202410272230.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-22
AI Technical Summary
PGA resin has a high melting point and low melt strength, which makes film processing difficult and makes it difficult to realize a barrier film with high gas barrier properties, biodegradability and durability.
By combining polyglycolic acid with zinc-containing ionomers and vinyl terpolymers, the molecular weight and proportion of the resin composition are adjusted, the melt viscosity and flow index are increased, the processability is improved, and the gas barrier is improved through the cross-linked structure safety and biodegradability.
It improves the biodegradability, gas blocking and processability of the membrane, reduces gas permeability, and is suitable for environmentally friendly materials in the field of green technology.
Smart Images

Figure CN118813014A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a polyglycolic acid-containing resin composition and a film comprising the same. Background Art
[0002] Biodegradable resins are resins that can be degraded by bacteria, microorganisms and other organic organisms. As environmental regulations are increasingly strengthened as existing non-degradable polymers increase environmental pollution, their demand is increasing as an alternative to non-degradable resins. In addition, they are recently used in a variety of industrial fields such as the packaging materials industry, the electronics industry, the automobile industry, the building materials industry, the marine industry, the stationery industry, and the pulp and paper industry.
[0003] Examples of biodegradable resins include polyglycolic acid (PGA), polybutylene succinate (PBS), polyhydroxyalkanoate (PHA), and polylactic acid (PLA). Among them, PGA is a synthetic resin produced by polymerizing glycolic acid, has excellent biodegradability, and has excellent gas barrier properties as a linear resin.
[0004] In addition, PGA resin has an ester bond inside and has high crystallinity, so it has excellent mechanical strength and high brittleness. Therefore, attempts have been made to develop a barrier film with high gas barrier properties, excellent biodegradability and durability using PGA resin.
[0005] However, PGA resin has a high melting point and low melt strength and is easily decomposed by heat and moisture, so there is a problem of difficulty in general film processing.
[0006] Therefore, it is necessary to develop a resin that has improved biodegradability, gas barrier properties, and durability and facilitates film processability by compounding or blending PGA resin with other polymers. Summary of the invention
[0007] Technical issues
[0008] An object of the present disclosure is to provide a polyglycolic acid-containing resin composition that provides enhanced barrier properties.
[0009] An object of the present disclosure is to provide a film formed of the resin composition and having improved barrier properties.
[0010] Technical Solution
[0011] The polyglycolic acid-containing resin composition according to an exemplary embodiment may include polyglycolic acid (poly(glycolic acid)), a zinc ionomer (Zn ionomer) and a vinyl terpolymer.
[0012] In some embodiments, the zinc-containing ionomer may include a terpolymer of ethylene, zinc (meth)acrylate, and (meth)acrylic acid.
[0013] In some embodiments, the vinyl terpolymer may include a copolymer of ethylene, glycidyl methacrylate, and alkyl acrylate.
[0014] In some embodiments, the content of the polyglycolic acid may be 60 wt % to 98 wt % of the total weight of the resin composition containing polyglycolic acid.
[0015] In some embodiments, the zinc-containing ionomer may be contained in an amount of 1 wt % to 39 wt % of the total weight of the polyglycolic acid-containing resin composition.
[0016] In some embodiments, the vinyl terpolymer may be present in an amount of 1 wt % to 39 wt % based on the total weight of the polyglycolic acid-containing resin composition.
[0017] In some embodiments, the sum of the content of the zinc-containing ionomer and the content of the vinyl terpolymer may be 2 wt % to 40 wt % of the total weight of the polyglycolic acid-containing resin composition.
[0018] In some embodiments, the content of the polyglycolic acid may be greater than the sum of the content of the zinc-containing ionomer and the content of the vinyl terpolymer.
[0019] In some embodiments, the sum of the content of the polyglycolic acid, the content of the zinc-containing ionomer, and the content of the vinyl terpolymer may be greater than 95 wt % of the total weight of the resin composition containing polyglycolic acid.
[0020] In some embodiments, the melt viscosity of the polyglycolic acid-containing resin composition measured at 230° C., 5% strain, and 0.1 Hz vibration frequency may be 200 Pa·s to 10000 Pa·s.
[0021] In some embodiments, the melt flow index (Melt Flow Index) of the polyglycolic acid-containing resin composition measured at 230° C. and a load of 2.16 kg may be 1 g / 10 min to 200 g / 10 min.
[0022] A film according to an exemplary embodiment may be formed of the polyglycolic acid-containing resin composition.
[0023] In some embodiments, the thickness of the film may be 50 μm to 250 μm.
[0024] In some embodiments, the oxygen permeability of the film measured at 50% relative humidity and 25° C. may be 200 g / m 2 · Below the day.
[0025] In some embodiments, the oxygen permeability of the film may satisfy the following formula 1:
[0026] [Formula 1]
[0027] OTR(PGA-Poly)<0.1(x·OTR(PGA)+(1-x)·OTR(Poly))
[0028] In Formula 1, OTR(PGA-Poly) is the oxygen permeability of a film formed from the resin composition containing polyglycolic acid, OTR(PGA) is the oxygen permeability of a film containing only polyglycolic acid, OTR(Poly) is the oxygen permeability of a film containing only a resin containing zinc ionomer or a vinyl terpolymer, and x is 0.6≤x<1.
[0029] Technical Effects
[0030] The polyglycolic acid-containing resin composition according to an exemplary embodiment may include polyglycolic acid (PGA), zinc ionomer (Zn ionomer, ZnIO) and vinyl terpolymer. Therefore, the polyglycolic acid-containing resin composition may improve durability against impact due to increased molecular weight, and may improve processability due to reduced melt flow index.
[0031] The polyglycolic acid-containing resin composition may contain a predetermined amount of PGA, thereby increasing the biodegradability and gas barrier properties of a film including the polyglycolic acid-containing resin composition and improving processability.
[0032] The film according to the exemplary embodiment may include the polyglycolic acid-containing resin composition. Therefore, the gas permeation path inside the film may become complicated, and the gas permeability may be reduced.
[0033] The polyglycolic acid-containing resin composition and film disclosed herein can be widely used in the field of green technology, such as biodegradable resins, biodegradable food packaging films, biodegradable sanitary products, and other biodegradable plastics that can utilize biodegradable compositions, etc. The polyglycolic acid-containing resin composition and film disclosed herein inhibit soil pollution, water pollution, air pollution, etc., and can be used in environmentally friendly materials such as eco-friendly disposable products. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 is a graph showing measured values of oxygen permeability and estimated values of oxygen permeability of films according to exemplary embodiments. DETAILED DESCRIPTION
[0035] According to an exemplary embodiment, a polyglycolic acid-containing resin composition and a film comprising the polyglycolic acid-containing resin composition are provided, wherein the polyglycolic acid-containing resin composition comprises polyglycolic acid (poly(glycolicacid), PGA), a zinc ionomer (Zn ionomer, ZnIO) and a vinyl terpolymer.
[0036] The present disclosure is described in detail below with reference to the accompanying drawings, but this is only an example, and the present disclosure is not limited to the specific embodiments described exemplarily.
[0037] According to an exemplary embodiment, the polyglycolic acid-containing resin composition may include PGA, ZnIO, and a vinyl terpolymer.
[0038] The PGA is a biodegradable polymer having a linear structure with an ester bond, and can have high biodegradability. In addition, the PGA polymer can have high crystallinity through hydrogen bonds between the PGA polymers. Therefore, the gas barrier property of the resin composition containing polyglycolic acid can be improved.
[0039] The ZnIO is a kind of polymer containing transition metal zinc, and has low hygroscopicity and water content. In addition, the structural stability of the resin composition containing polyglycolic acid can be improved through the coordination bond with the ester group of the PGA.
[0040] The vinyl terpolymer is a polymer obtained by copolymerizing three basic monomers including monomers derived from ethylene. The vinyl terpolymer can improve structural stability by cross-linking with the PGA and the ZnIO.
[0041] In some embodiments, the ZnIO may include a terpolymer of ethylene, zinc (meth)acrylate, and (meth)acrylic acid.
[0042] The ethylene, (meth)acrylic acid zinc and (meth)acrylic acid terpolymer has zinc ions (Zn 2+ ) and carboxylate anions (-COO - ) ion-bonded polymer. The zinc ion of the terpolymer of ethylene, zinc (meth)acrylate and (meth)acrylic acid is a transition metal ion and can be coordinated and bonded with the ester group of the PGA. Therefore, the terpolymer of ethylene, zinc (meth)acrylate and (meth)acrylic acid is included in the resin composition containing polyglycolic acid, thereby improving durability and melt strength.
[0043] In one embodiment, the content of the ethylene monomer of the terpolymer of ethylene, zinc (meth)acrylate and (meth)acrylic acid is not limited, but for example, can be 70 wt % to 98 wt %, 73 wt % to 95 wt %, or 76 wt % to 92 wt % of the total weight of the terpolymer of ethylene, zinc (meth)acrylate and (meth)acrylic acid.
[0044] In one embodiment, the content of the zinc (meth)acrylate monomer of the terpolymer of ethylene, zinc (meth)acrylate and (meth)acrylic acid is not limited, but for example, may be 1 wt % to 20 wt %, 1 wt % to 17 wt %, or 1 wt % to 14 wt % of the total weight of the terpolymer of ethylene, zinc (meth)acrylate and (meth)acrylic acid.
[0045] In one embodiment, the content of the (meth)acrylic acid monomer of the terpolymer of ethylene, zinc (meth)acrylate and (meth)acrylic acid is not limited, but for example, can be 1 wt % to 29 wt %, 4 wt % to 26 wt %, or 7 wt % to 23 wt % of the total weight of the terpolymer of ethylene, zinc (meth)acrylate and (meth)acrylic acid.
[0046] In some embodiments, the vinyl terpolymer may include a copolymer of ethylene, glycidyl methacrylate, and alkyl acrylate (EAG).
[0047] The EAG is a vinyl polymer containing a glycidyl group. The glycidyl group of the EAG is contained in the resin composition containing polyglycolic acid and can be bonded to a carboxyl group of at least one of the PGA and ZnIO.
[0048] Therefore, the polyglycolic acid-containing resin composition can be extended and the polymer structure can be complicated. Therefore, the melt strength and durability of the polyglycolic acid-containing resin composition can be improved, and the processability can be improved.
[0049] In one embodiment, the content of the ethylene monomer of the EAG is not limited, but for example may be 50 wt % to 88 wt %, 55 wt % to 82 wt %, or 57 wt % to 78 wt % of the total weight of the EAG.
[0050] In one embodiment, the content of the glycidyl methacrylate monomer of the EAG is not limited, but for example may be 1 wt % to 30 wt %, 3 wt % to 25 wt %, or 5 wt % to 20 wt % of the total weight of the EAG.
[0051] In one embodiment, the content of the alkyl acrylate monomer of the EAG is not limited, but for example may be 10 wt % to 48 wt %, 15 wt % to 42 wt %, or 17 wt % to 38 wt % of the total weight of the EAG.
[0052] In some embodiments, the content of the PGA can be 60 wt % to 98 wt %, 60 wt % to 93 wt %, 60 wt % to 88 wt %, or 65 wt % to 85 wt % of the total weight of the polyglycolic acid-containing resin composition.
[0053] When the content is within the above range, PGA can be distributed in the entire area of the polyglycolic acid-containing resin composition. Therefore, the polyglycolic acid-containing resin composition can improve the melt strength, durability and processability of the polyglycolic acid-containing resin composition while maintaining low gas permeability. In addition, the biodegradability of the polyglycolic acid-containing resin composition can be improved by PGA.
[0054] In some embodiments, the content of ZnIO can be 1 wt % to 39 wt %, 5 wt % to 38 wt %, 7 wt % to 30 wt % or 8 wt % to 20 wt % of the total weight of the polyglycolic acid-containing resin composition.
[0055] When the content is within the above range, the gas permeability of the polyglycolic acid-containing resin composition can be prevented from increasing due to the increase of the ZnIO and the decrease of the PGA. In addition, the zinc ions of the ZnIO are coordinated with the ester groups of the PGA, thereby improving the durability of the polyglycolic acid-containing resin composition. In addition, the hygroscopicity of the polyglycolic acid-containing resin composition is reduced, thereby preventing the polymer structure from collapsing due to the high biodegradability of the polyglycolic acid-containing resin composition. Therefore, the structural stability of the polyglycolic acid-containing resin composition can be improved.
[0056] In some embodiments, the content of the vinyl terpolymer (e.g., EAG) can be 1 wt % to 39 wt %, 2 wt % to 35 wt %, 5 wt % to 33 wt %, or 7 wt % to 27 wt % of the total weight of the polyglycolic acid-containing resin composition.
[0057] When the content is within the above range, the vinyl terpolymer (eg, EAG) can be stably cross-linked with the carboxyl groups of the PGA and the ZnIO, thereby further improving the melt strength and processability of the polyglycolic acid-containing resin composition.
[0058] In one embodiment, the sum of the content of the ZnIO and the content of the vinyl terpolymer may be 2 wt % to 40 wt %, 5 wt % to 40 wt %, 10 wt % to 35 wt % or 10 wt % to 30 wt % of the total weight of the polyglycolic acid-containing resin composition.
[0059] When the content is within the above range, the PGA content in the polyglycolic acid-containing resin composition may be 60 wt % or more, 65 wt % or more, or 70 wt % or more. Therefore, the biodegradability of the polyglycolic acid-containing resin composition is not reduced, while its gas permeability can be reduced and processability can be improved.
[0060] In some embodiments, the content of the PGA may be greater than the sum of the content of the ZnIO and the content of the vinyl terpolymer, thereby simultaneously improving the biodegradability, gas barrier properties and durability of the polyglycolic acid-containing resin composition.
[0061] As described above, the melt viscosity and the melt flow index (Melt Flow Index) can be adjusted by adjusting the contents of PGA, ZnIO and the vinyl terpolymer contained in the polyglycolic acid-containing resin composition.
[0062] In some embodiments, the sum of the content of the polyglycolic acid, the content of the zinc-containing ionomer and the content of the vinyl terpolymer may be greater than 95 wt %, greater than 98 wt % or greater than 99 wt % of the total weight of the polyglycolic acid-containing resin composition.
[0063] In one embodiment, the polyglycolic acid-containing resin composition may be composed of the polyglycolic acid, the zinc-containing ionomer and the vinyl terpolymer. For example, the sum of the content of the polyglycolic acid, the content of the zinc-containing ionomer and the content of the vinyl terpolymer may be 100 wt % of the total weight of the polyglycolic acid-containing resin composition.
[0064] In some embodiments, the melt viscosity of the polyglycolic acid-containing resin composition may be 50 Pa·s to 10000 Pa·s, 100 Pa·s to 8000 Pa·s, or 200 Pa·s to 6000 Pa·s.
[0065] The melt viscosity is a value obtained by measuring a test piece prepared by pressing the polyglycolic acid-containing resin composition into a thickness of 2 mm at 230° C. under a strain of 5% and a vibration frequency of 0.1 Hz.
[0066] In one embodiment, the melt flow index of the polyglycolic acid-containing resin composition may be 1 g / 10 min to 200 g / 10 min, 1 g / 10 min to 100 g / 10 min, or 2 g / 10 min to 50 g / 10 min.
[0067] The melt flow index is measured and calculated according to ASTM D1238 under the conditions of a temperature of 230° C. and a load of 2.16 kg.
[0068] The melt viscosity and melt flow index are maintained within the range, so the flexibility of the polyglycolic acid-containing resin composition can be improved compared to the flexibility of PGA. Therefore, for example, the processability can be improved in foaming-expansion molding, injection molding, compression molding, casting film molding, and blown film molding. Therefore, the processability from the polyglycolic acid-containing resin composition to a film can be improved.
[0069] The polyglycolic acid-containing resin composition may be formed by drying and kneading a mixture of PGA, ZnIO and a vinyl terpolymer.
[0070] In an exemplary embodiment, PGA, ZnIO and vinyl terpolymer may be fed into a hopper dryer.
[0071] PGA can be put into a hopper dryer maintained at a temperature of 60° C. to 100° C., 70° C. to 90° C., or 75° C. to 85° C. for drying. ZnIO can be put into a hopper dryer maintained at a temperature of 30° C. to 70° C., 40° C. to 60° C., or 45° C. to 55° C. for drying. Vinyl terpolymers (e.g., EAG) can be put into a hopper dryer maintained at a temperature of 20° C. to 60° C., 30° C. to 50° C., or 35° C. to 45° C. for drying.
[0072] The PGA, ZnIO and vinyl terpolymer can be dried for 10 to 14 hours, 11 to 13 hours, or 11 hours and 30 minutes to 12 hours and 30 minutes, for example. Within the above range, the PGA, ZnIO and vinyl terpolymer are fully dried, so that the side reaction of the PGA, ZnIO and vinyl terpolymer in the mixing process can be suppressed.
[0073] The dried PGA, ZnIO and vinyl terpolymer can be put into the cavity of an internal mixer. The cavity of the internal mixer can be maintained at 220°C to 260°C, 225°C to 250°C, or 230°C to 240°C, for example.
[0074] When the dried PGA, ZnIO and vinyl terpolymer are put into an internal mixer, the rotor inside the internal mixer may be rotated at, for example, 10 rpm to 70 rpm, 20 rpm to 60 rpm, or 30 rpm to 50 rpm.
[0075] When the content is within the above range, PGA, ZnIO and the vinyl terpolymer can be initially kneaded without being agglomerated with each other.
[0076] After the dried PGA, ZnIO and vinyl terpolymer are added, the mixing can be performed while maintaining the rotation speed of the rotor at, for example, 60 rpm to 100 rpm, 70 rpm to 90 rpm, or 75 rpm to 85 rpm. The mixing can be performed for, for example, 1 minute to 5 minutes, 2 minutes to 4 minutes, or 2 minutes 30 seconds to 3 minutes 30 seconds.
[0077] When the content of PGA, ZnIO and vinyl terpolymer is within the above range, the PGA, ZnIO and vinyl terpolymer can be evenly distributed and mixed.
[0078] The kneaded product obtained by kneading as above can be recovered to obtain a resin composition containing polyglycolic acid.
[0079] Although the mixing process is described as being performed by a sealed mixer, the mixing process is not limited to being performed by a sealed mixer. For example, the dried PGA, ZnIO and vinyl terpolymer can be put into a single-shaft extruder or a twin-shaft extruder and melted and mixed to complete the mixing. The mixed resin composition discharged from the discharge port of the single-shaft extruder or the twin-shaft extruder can be cut in a pelletizer to obtain a polyglycolic acid-containing resin composition in the form of pellets.
[0080] According to an exemplary embodiment, a film may be formed from the above-mentioned resin composition containing polyglycolic acid, thereby reducing the gas permeability of the film and improving biodegradability and durability.
[0081] In some embodiments, the thickness of the film may be 50 μm to 250 μm, 100 μm to 200 μm, or 120 μm to 180 μm. Within the above range, the gas permeability of the film may be substantially reduced.
[0082] In one embodiment, the oxygen permeability of the film may be 200 g / m2 Less than 100g / m 2 Less than 30g / m 2 The lower limit of the oxygen permeability of the film is not limited, but for example, the oxygen permeability of the film may be 1 g / m 2 · More than 2g / m 2 · More than 5g.m 2 More than 10g / m 2 · More than one day.
[0083] The oxygen permeability may be measured under the conditions of a relative humidity of 50% and a temperature of 25°C.
[0084] When the film is within the above range, the barrier property against gas (for example, oxygen) is improved when the film is used as a barrier film, and thus the product inside the barrier film can be sufficiently protected.
[0085] When the PGA content in the polyglycolic acid-containing resin composition is 60 wt % or more, it can be uniformly located in the entire region of the polyglycolic acid-containing resin composition. Therefore, due to the high gas barrier properties of PGA, the film containing the polyglycolic acid-containing resin composition can maintain high gas barrier properties.
[0086] Therefore, the polyglycolic acid-containing resin composition containing 60 wt% or more of PGA can maintain a low oxygen permeability. For example, the measured oxygen permeability of the polyglycolic acid-containing resin composition can be lower than the arithmetic mean of the oxygen permeabilities of the polymer components contained in the polyglycolic acid-containing resin composition.
[0087] In some embodiments, the oxygen permeability of the film may satisfy the following formula 1:
[0088] [Formula 1]
[0089] OTR(PGA-Poly)<0.1(x·OTR(PGA)+(1-x)·OTR(Poly))
[0090] In Formula 1, OTR(PGA-Poly) is the oxygen permeability of a film formed from the resin composition containing polyglycolic acid, OTR(PGA) is the oxygen permeability of a film containing only polyglycolic acid, OTR(Poly) is the oxygen permeability of a film containing only a resin containing zinc ionomer or a vinyl terpolymer, and x is 0.6≤x<1.
[0091] The film can be used as a barrier film for packaging materials of various products such as food packaging materials and battery packaging materials.
[0092] The above-mentioned film may be made of a resin composition containing polyglycolic acid.
[0093] According to an exemplary embodiment, the film may be manufactured by pressurizing the resin composition containing polyglycolic acid through a press.
[0094] In some embodiments, the press can be maintained at 200° C. to 260° C., 210° C. to 250° C., 220° C. to 240° C., or 225° C. to 235° C. Within the above ranges, a film including the resin composition containing polyglycolic acid can be molded and deformed.
[0095] In some embodiments, the polyglycolic acid-containing resin composition may be compressed at a pressure of 10 MPa to 30 MPa, 15 MPa to 25 MPa, or 18 MPa to 22 MPa for 1 minute to 3 minutes, or 1 minute 30 seconds to 2 minutes 30 seconds.
[0096] When the thickness is within the above range, the film can be manufactured to have the above thickness, and thus a film having a reduced oxygen permeability and a thin thickness can be manufactured.
[0097] Although the above-mentioned film manufacturing is described as manufacturing a film by pressurizing a press, the film manufacturing method is not limited thereto. For example, the resin composition containing polyglycolic acid melted in an extruder can be extruded from a t-die to a chill roll to be cooled and manufactured into a film (e.g., a cast film manufacturing method). For example, the resin composition containing polyglycolic acid can be cooled and manufactured into a film (e.g., a blown film manufacturing method) in a ring-shaped die (e.g., a spiral die, etc.) through an air ring (air ring) in contact with air.
[0098] The embodiments of the present disclosure are further described with reference to specific experimental examples. The embodiments and comparative examples included in the experimental examples are merely examples of the present disclosure and are not intended to limit the scope of the claims. Various changes and modifications can be made to the embodiments within the scope of the present disclosure and the technical concept, which is obvious to those skilled in the art. Naturally, such changes and modifications are also included in the scope of the appended claims.
[0099] Examples and Comparative Examples
[0100] Example 1
[0101] (1) Preparing raw materials for a resin composition containing polyglycolic acid
[0102] Poly(glycolic acid) (PGA) was dried in a hopper dryer set at 80° C. for 12 hours to prepare dried PGA.
[0103] The dried terpolymer of ethylene, zinc acrylate and acrylic acid was prepared by drying the terpolymer of ethylene, zinc acrylate and acrylic acid for 12 hours in a hopper dryer set at 50° C. The contents of the ethylene monomer, zinc acrylate monomer and acrylic acid monomer in the terpolymer of ethylene, zinc acrylate and acrylic acid were approximately 86.5 wt %, 6.75 wt % and 6.75 wt %, respectively.
[0104] A terpolymer of ethylene, glycidyl methacrylate and methyl acrylate (EAG) was dried in a hopper dryer set at 40° C. for 12 hours to prepare a dried EAG. The contents of the ethylene monomer, glycidyl methacrylate monomer and methyl acrylate monomer in the EAG were 68 wt %, 8 wt % and 24 wt %, respectively.
[0105] The hopper dryer adopts Mitsui hot air dryer.
[0106] (2) Preparation of a resin composition containing polyglycolic acid
[0107] Dried PGA, dried terpolymer of ethylene, zinc acrylate and acrylic acid and dried EAG were added into the cavity of a closed mixer at a ratio of 80 wt%, 10 wt% and 10 wt% respectively. The internal temperature of the closed mixer cavity was maintained at 230° C. and the rotor of the closed mixer was rotated at a speed of 40 rpm.
[0108] Thereafter, the rotor speed was increased to 80 rpm and kneading was performed for 3 minutes, thereby preparing and recovering a polyglycolic acid-containing resin composition as a kneading product.
[0109] The internal mixer used was a Brabender measuring mixer W50.
[0110] (3) Film manufacturing
[0111] The polyglycolic acid-containing resin composition was pressed at a pressure of 20 MPa for 2 minutes using a press machine set at 230° C. to produce a film.
[0112] Examples 2 to 7 and Comparative Examples 1 to 6
[0113] The polyglycolic acid-containing resin compositions and films of Examples 2 to 7 and Comparative Examples 1 to 6 were prepared by the same method as Example 1, except that the type of PGA used and the weight ratio of the dry PGA, dry ethylene, zinc acrylate and acrylic acid terpolymer, and dry EAG introduced into the cavity of the internal mixer were adjusted as shown in Table 1 below.
[0114]
Table 1
[0115]
[0116] The types of PGA listed in Table 1 are as follows.
[0117] PGA Type
[0118] A: Polyglycolic acid having a number average molecular weight (Mn) of 35,000 to 45,000 and a weight average molecular weight (Mw) of 80,000 to 95,000 as measured by gel permeation chromatography (GPC)
[0119] B: Polyglycolic acid having a number average molecular weight (Mn) of 70,000 to 80,000 and a weight average molecular weight (Mw) of 160,000 to 180,000 as measured by gel permeation chromatography (GPC)
[0120] The gel permeation chromatography method is to dissolve polyglycolic acid in hexafluoroisopropylalcohol (HFIP), filter the solution with a polytetrafluoroethylene (PTFE) filter, and inject it into Tosoh's EcoSEC HLC-8320GPC for measurement, using polymethylmethacrylate (PMMA) as a standard substance.
[0121] Experimental Example 1
[0122] Figure 1 It is a graph showing the measured value and estimated value of the oxygen permeability of the film according to the sum of the content of the terpolymer of ethylene, zinc acrylate and acrylic acid and the content of EAG contained in the polyglycolic acid-containing resin composition.
[0123] The estimated value of oxygen permeability represents a value obtained by arithmetically averaging the oxygen permeabilities of PGA, the terpolymer of ethylene, zinc acrylate and acrylic acid, and EAG contained in the polyglycolic acid-containing resin composition according to weight ratio.
[0124] The measured value of oxygen permeability is a value obtained by measuring the oxygen permeability of a film comprising the polyglycolic acid-containing resin composition. The measured value of oxygen permeability of the film is the measured value of Example 1, Example 2, Example 5, and Example 6.
[0125] See also Figure 1 It was calculated that the estimated value of the oxygen permeability of the film increases linearly with the sum of the content of the terpolymer of ethylene, zinc acrylate and acrylic acid and the content of EAG.
[0126] However, the oxygen permeability of the film is measured to maintain a low oxygen permeability when the sum of the content of the terpolymer of ethylene, zinc acrylate and acrylic acid and the content of EAG is less than 40 wt% (PGA exceeds 60 wt%). In addition, when the sum of the content of the terpolymer of ethylene, zinc acrylate and acrylic acid and the content of EAG exceeds 40 wt%, the oxygen permeability increases in proportion to the content.
[0127] Experimental Example 2
[0128] (1) Measurement of melt viscosity
[0129] The polyglycolic acid-containing resin compositions prepared according to the above examples and comparative examples were pressed into a thickness of 2 mm at a temperature of 230° C., and then the melt viscosity was measured using a viscosity meter (TA ARES).
[0130] The viscosity meter was set to 230° C., 5% strain, and a vibration frequency of 0.1 Hz to 400 Hz, and the viscosity value measured at a vibration frequency of 0.1 Hz was measured as the melt viscosity.
[0131] Table 2 below shows the evaluation results.
[0132] (2) Measurement of Melt Flow Index
[0133] The melt flow index of the polyglycolic acid-containing resin composition prepared according to the above examples and comparative examples was measured at a temperature of 230° C. and a load of 2.16 kg in accordance with ASTM D1238.
[0134] The evaluation results are shown in Table 2 below.
[0135] (3) Measurement of oxygen permeability
[0136] The films produced according to the above-mentioned Examples and Comparative Examples were mounted on an oxygen permeability meter (MOCONOX TRANS model 2 / 61) and the oxygen permeability was measured.
[0137] The oxygen permeability measured is a value at a point where the permeability becomes stable after measurement for 12 hours under the conditions of a relative humidity of 50% and a temperature of 25°C.
[0138] The upper limit of the oxygen permeability is 1200 g / m 2 · days, the oxygen permeability of the films that were not measured because they exceeded the upper limit was marked as "exceeded".
[0139] Table 2 below shows the evaluation results.
[0140]
Table 2
[0141]
[0142] Referring to Table 2, the film according to the example shows a 200 g / m 2 · Oxygen permeability below 3000 ℃.
[0143] In Examples 4 and 5 in which the PGA content was reduced to 60 wt %, the oxygen permeability increased.
[0144] The oxygen permeability increased in Example 6 where the PGA content was reduced to less than 60 wt%.
[0145] In Example 7 in which the molecular weight of PGA was increased, the melt viscosity increased and the melt flow index decreased.
[0146] In Comparative Example 1 using only PGA, the melt viscosity of the polyglycolic acid-containing resin composition was reduced and the melt flow index was increased.
[0147] In Comparative Example 2 using only a ternary copolymer of ethylene, zinc acrylate, and acrylic acid, the oxygen permeability exceeded 1200 g / m 2 ·sky.
[0148] In Comparative Example 3 using only EAG, the oxygen permeability exceeded 1200 g / m 2 ·sky.
[0149] In Comparative Example 4, which used a resin composition containing no PGA and kneading a terpolymer of ethylene, zinc acrylate, and acrylic acid and EAG, the oxygen permeability exceeded 1200 g / m 2 ·sky.
Claims
1. A resin composition containing polyglycolic acid, comprising: Polyglycolic acid; Zinc-containing ionomers; and Vinyl terpolymer.
2. The polyglycolic acid-containing resin composition according to claim 1, wherein: The zinc-containing ionomer includes a terpolymer of ethylene, zinc (meth)acrylate and (meth)acrylic acid.
3. The polyglycolic acid-containing resin composition according to claim 1, wherein: The vinyl terpolymer includes a copolymer of ethylene, glycidyl methacrylate and alkyl acrylate.
4. The polyglycolic acid-containing resin composition according to claim 1, wherein: The polyglycolic acid is present in an amount of 60 to 98 wt % based on the total weight of the polyglycolic acid-containing resin composition.
5. The polyglycolic acid-containing resin composition according to claim 1, wherein: The zinc-containing ionomer is contained in an amount of 1 to 39 wt % based on the total weight of the polyglycolic acid-containing resin composition.
6. The polyglycolic acid-containing resin composition according to claim 1, wherein: The vinyl terpolymer is present in an amount of 1 to 39 wt % based on the total weight of the polyglycolic acid-containing resin composition.
7. The polyglycolic acid-containing resin composition according to claim 1, wherein: The sum of the content of the zinc-containing ionomer and the content of the vinyl terpolymer is 2 wt % to 40 wt % of the total weight of the polyglycolic acid-containing resin composition.
8. The polyglycolic acid-containing resin composition according to claim 1, wherein: The content of the polyglycolic acid is greater than the sum of the content of the zinc-containing ionomer and the content of the vinyl terpolymer.
9. The polyglycolic acid-containing resin composition according to claim 1, wherein: The sum of the content of the polyglycolic acid, the content of the zinc-containing ionomer and the content of the vinyl terpolymer is greater than 95% by weight of the total weight of the polyglycolic acid-containing resin composition.
10. The polyglycolic acid-containing resin composition according to claim 1, wherein: The melt viscosity of the polyglycolic acid-containing resin composition measured at 230° C., 5% strain, and 0.1 Hz vibration frequency is 200 Pa·s to 10000 Pa·s.
11. The polyglycolic acid-containing resin composition according to claim 1, wherein: The polyglycolic acid-containing resin composition has a melt flow index of 1 g / 10 min to 200 g / 10 min measured at 230° C. and a load of 2.16 kg.
12. A film formed from the polyglycolic acid-containing resin composition of claim 1.
13. The membrane of claim 12, wherein: The thickness of the film is 50 μm to 250 μm.
14. The membrane of claim 13, wherein: The oxygen permeability of the film measured at 50% relative humidity and 25°C is 200 g / m 2 · Below the day.
15. The film according to claim 12, wherein The oxygen permeability of the film satisfies the following formula 1: [Formula 1] OTR(PGA-Poly)<0.1(x·OTR(PGA)+(1-x)·OTR(Poly)) In Formula 1, OTR(PGA-Poly) is the oxygen permeability of a film formed from the resin composition containing polyglycolic acid, OTR(PGA) is the oxygen permeability of a film containing only polyglycolic acid, OTR(Poly) is the oxygen permeability of a film containing only a resin containing a zinc ionomer or a vinyl terpolymer, and x is 0.6≤x<1.