Method and system for graded fluidized selective reduction of pyrolusite

By classifying soft manganese ore powder in the fluidized furnace tube, the problem of incomplete reduction of coarse particles and easy over-reduction of fine particles is solved, the preparation of different manganese products is realized, the resource utilization rate and energy optimization are improved, and the cost is reduced pollution and energy consumption.

CN118813985APending Publication Date: 2024-10-22ZHONGYE-CHANGTIAN INT ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310422613.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the existing technology, during the fluidized reduction process of pyrolusite, the coarse particles are not completely reduced and the fine particles are easily over-reduced, resulting in difficulty in leaching manganese in the subsequent sulfuric acid leaching process, low resource utilization, and high energy consumption in traditional processes. , serious environmental pollution problems.

Method used

By setting up a screen in the fluidized furnace tube, the pyrolusite powder is divided into coarse particles and fine particles and processed in the reduction zone under different temperatures and reducing atmospheres. The coarse particles are precisely controlled to generate MnO, and the fine particles are generated into metallic Mn. Avoid the presence of MnO2 and realize the preparation of different manganese products.

Benefits of technology

It improves resource utilization, reduces energy consumption, simplifies the process, reduces pollution, and the process is simple and easy to control, with good economic and environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118813985A_ABST
    Figure CN118813985A_ABST
Patent Text Reader

Abstract

The invention discloses a method and a system for graded fluidized selective reduction of pyrolusite. Coarse-particle pyrolusite and fine-particle pyrolusite are controlled to be subjected to different degrees of reduction roasting treatment in different reduction areas of a fluidized furnace tube at different temperatures and different reduction atmospheres, the coarse-particle pyrolusite is accurately controlled to be reduced to obtain a MnO product, and the fine-particle pyrolusite is accurately controlled to be reduced to obtain a metal Mn product. The existence of insoluble manganese in the process of preparing the high-purity manganese sulfate product through subsequent leaching treatment is avoided, products of different manganese systems are obtained, and optimal control over the product and energy is achieved. The pyrolusite grading fluidization selective reduction method and the pyrolusite grading fluidization selective reduction system have the advantages of being simple in structure, low in manufacturing cost, high in reduction efficiency, low in energy consumption, convenient to operate and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to metal mineral smelting and processing, in particular to a method for selective reduction of pyrolusite by graded fluidization and a reduction system used in the method, and belongs to the technical field of metal mineral smelting and processing. Background Art

[0002] Manganese ore is one of the scarce resources in my country, and the existing resources are more poor than rich, with rich ore resources accounting for only 6.43%, and the impurity content of the resources is high. Therefore, it is necessary to make full use of the poor manganese oxide ore resources and improve the quality of manganese ore products. How to use these manganese oxide ore resources at low cost and efficiently to provide high-quality raw materials for electrolytic manganese oxide has become a bottleneck restricting the development of the manganese industry.

[0003] Pyrolusite (mainly manganese-containing minerals are MnO2) is an important raw material for producing manganese sulfate. About 60% of manganese sulfate in the world is processed by pyrolusite. Pyrolusite is insoluble in sulfuric acid and must be reduced to manganese monoxide (MnO) before reacting with sulfuric acid to produce manganese sulfate. The traditional process is to use coal as a reducing agent to carry out reduction roasting of pyrolusite, so that the MnO2 in the pyrolusite is converted into MnO, and then leached with sulfuric acid, but this method has the problems of high energy consumption, poor operating conditions, and serious environmental pollution. The newly developed process two-ore roasting method also has many shortcomings. The two-ore roasting method is to convert MnO2 into MnSO4, FeS2 into Fe2O3, and then leached with water, which needs to be roasted for a long time under a high sulfur-manganese ratio, which not only causes FeS2 to be unable to be fully utilized, but also has a large amount of slag, which is difficult to handle, and there are also problems such as difficult flue gas treatment.

[0004] In my country, the process of reducing roasting-sulfuric acid leaching-concentration crystallization is mainly used to produce manganese sulfate with pyrolusite as raw material. The reduction roasting equipment for producing manganese monoxide by traditional process is the traditional reverberatory furnace, which has high heat consumption, small processing capacity, low manganese recovery rate and poor working conditions. In the 1980s, Yunnan, Hunan and Guangdong and other places had successively built rotary kilns to try this aspect, but due to the fine particle size of raw materials, rotary kiln structure and technical problems, the kiln had a serious sticking phenomenon, and most rotary kilns could not be used normally for production. In recent years, a heat recovery type microwave reduction roasting process for manganese oxide ore has been developed. The microwave heating furnace is used for the reduction roasting process of manganese oxide ore. Due to the high power consumption (210-240kw·h) and coal consumption (180kg / ton), as well as the microwave source, processing capacity and labor protection problems have not been solved, it is currently difficult to promote and apply in production.

[0005] Fluidized reduction process has attracted attention as a relatively efficient and reasonable technology for processing pyrolusite resources. However, in the process of fluidized reduction of pyrolusite, due to the presence of coarse particles and fine particles, the coarse particles are not completely reduced and still exist in the form of MnO2, which is difficult to be leached in the subsequent sulfuric acid leaching process; the fine particles require a low reduction temperature in the reduction process, and are easily over-reduced and exist in the form of metallic Mn, resulting in energy waste. It is also difficult to be leached in the subsequent sulfuric acid leaching process, and the resource utilization rate is low. Therefore, it is of great significance to study a feasible new process to replace the traditional process, reduce pollution, and improve resource utilization. Summary of the invention

[0006] In view of the problem in the prior art that the coarse particles are not completely reduced and the fine particles are easily excessively reduced in the treatment of pyrolusite by the fluidized reduction process, which results in the difficulty of leaching the manganese element in the subsequent sulfuric acid leaching process and the low resource utilization rate, the present invention provides a method for the graded fluidized selective reduction of pyrolusite and a reduction system for the method. The present invention controls the coarse particles of pyrolusite and the fine particles of pyrolusite to be subjected to reduction roasting treatment with different reduction degrees in a fluidized furnace tube at different temperatures and different reducing atmospheres, accurately controls the coarse particles of pyrolusite to obtain the MnO product, and the fine particles of pyrolusite to obtain the metal Mn product, avoids the presence of MnO2 which is difficult to leach, obtains products of different manganese series, and realizes the optimization control of products and energy.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is specifically described as follows:

[0008] According to a first embodiment of the present invention, a method for selective reduction of pyrolusite by graded fluidization is provided:

[0009] A method for selective reduction of pyrolusite by fluidization, comprising the following steps:

[0010] 1) crushing pyrolusite to obtain pyrolusite powder, and inputting the obtained pyrolusite powder and reducing gas from the lower feed port of the fluidized bed furnace tube.

[0011] 2) In the fluidized bed furnace tube, according to the direction of the material, the fluidized bed furnace tube is divided into a lower reduction zone and an upper reduction zone by a screen. Under the pushing action of the reducing gas (referring to a mixed gas containing reducing gas (such as CO, H2) and inert gas (such as N2)), the coarse pyrolusite powder is reduced and roasted in the lower reduction zone, and the fine pyrolusite powder is reduced and roasted in the upper reduction zone.

[0012] 3) According to the changes in the contents of O and Mn in the coarse pyrolusite powder in the lower reduction zone, the content of the reducing gas (such as CO, H2) introduced into the lower reduction zone is adjusted, so that the coarse pyrolusite powder in the lower reduction zone is reduced to MnO. According to the changes in the contents of O and Mn in the fine pyrolusite powder in the upper reduction zone, the content of the reducing gas introduced into the upper reduction zone is adjusted, so that the fine pyrolusite powder in the upper reduction zone is reduced to Mn.

[0013] Preferably, the method further comprises:

[0014] 4) The MnO obtained in step 3) is discharged from the coarse particle discharge port located in the middle of the fluidized bed furnace tube, and used to prepare manganese sulfate after cooling. The Mn obtained in step 3) is discharged from the fine particle discharge port located at the top of the fluidized bed furnace tube, and used to prepare metallic manganese after cooling.

[0015] Preferably, in step 1), the particle size of the pyrolusite powder is not greater than 1 mm, preferably 0.1-1 mm, more preferably 0.15-1 mm.

[0016] Preferably, in step 2), the particle size of the coarse pyrolusite powder is 0.2-1 mm, preferably 0.4-1 mm, more preferably 0.6-1 mm. The particle size of the fine pyrolusite powder is not more than 0.6 mm, preferably not more than 0.4 mm, more preferably not more than 0.2 mm.

[0017] Preferably, the reducing gas is a mixed gas containing CO and / or H2, preferably a mixed gas consisting of CO and / or H2 and an inert gas, and more preferably a mixed gas consisting of CO and / or H2 and nitrogen.

[0018] Preferably, in the mixed gas, the total content of CO and / or H2 is not less than 3% of the total amount of the mixed gas, preferably not less than 5%, and more preferably not less than 8%.

[0019] Preferably, the flow rate of the reducing gas introduced into the fluidized bed furnace tube is 0.2-3 m / s, preferably 0.3-2.5 m / s, more preferably 0.4-2 m / s.

[0020] Preferably, the reduction temperature in the lower reduction zone is 700-1000° C., preferably 750-950° C., more preferably 800-900° C. The reduction time in the lower reduction zone is 0.1-3 h, preferably 0.3-2.5 h, more preferably 0.5-2 h.

[0021] Preferably, the reduction temperature in the upper reduction zone is 500-800° C., preferably 550-750° C., more preferably 600-700° C. The reduction time in the upper reduction zone is 0.1-3 h, preferably 0.3-2.5 h, more preferably 0.5-2 h.

[0022] Preferably, in step 3), according to the change of the content of O and Mn in the crude pyrolusite powder in the lower reduction zone, the content of the reducing gas introduced into the lower reduction zone is adjusted so that the crude pyrolusite powder in the lower reduction zone is reduced to MnO, specifically: the oxygen-manganese ratio in the crude pyrolusite powder in the lower reduction zone is detected in real time and recorded as a1, then:

[0023] When 1<a1, the content of CO and / or H2 in the reducing gas is increased, and the increase amount is 3*(a1+1)*100%.

[0024] When 0.5<a1≤1, the current working condition remains unchanged.

[0025] When 0<a1≤0.5, the content of CO and / or H2 in the reducing gas is reduced by 4*(a1+2)*100%.

[0026] Preferably, in step 3), according to the change of the content of O and Mn in the fine manganese ore powder in the upper reduction zone, the content of the reducing gas introduced into the upper reduction zone is adjusted so that the fine manganese ore powder in the upper reduction zone is reduced to Mn, specifically: the oxygen-manganese ratio in the fine manganese ore powder in the upper reduction zone is detected in real time and recorded as a2, then:

[0027] When a2=0, the current operating condition remains unchanged.

[0028] When a2>0, the content of CO and / or H2 in the reducing gas is increased by 5*(a2+3)*100%.

[0029] According to a second embodiment of the present invention, a system for graded fluidized selective reduction of pyrolusite or a system for the method described in the first embodiment is provided:

[0030] A system for graded fluidized selective reduction of pyrolusite, the fluidized selective reduction system comprising a furnace tube and a screen. The screen is arranged in the tube cavity of the furnace tube, and the tube cavity of the furnace tube is divided into a lower chamber and an upper chamber, and the screen is provided with sieve holes. An air inlet is arranged at the bottom end of the furnace tube, a feed inlet is arranged on the lower side wall of the furnace tube, a coarse material outlet is arranged on the middle side wall of the furnace tube, and a fine material outlet is arranged at the top end of the furnace tube. The air inlet, feed inlet and coarse material outlet are all connected to the lower chamber, and the fine material outlet is connected to the upper chamber. An element content detection device and a heating device with temperature control are also independently arranged in the lower chamber and the upper chamber.

[0031] Preferably, the screen is movably arranged in the tube cavity of the furnace tube and can be moved in the vertical direction. That is, the position of the screen in the furnace tube can be adjusted and fixed. For example, it can be flexibly adjusted and fixed by elastic parts or buckles.

[0032] Preferably, a gas supply port communicating with the upper chamber is also provided at the upper portion of the furnace tube.

[0033] Preferably, a plurality of screens are arranged in the tube cavity of the furnace tube, the lower chamber is formed below the plurality of screens, and the upper chamber is formed above the plurality of screens. It should be noted that the apertures of the screen holes of the plurality of screens may be the same or different, and are adjusted according to specific circumstances.

[0034] Preferably, the mesh size of the sieve is not greater than 0.6 mm, preferably not greater than 0.4 mm, and more preferably not greater than 0.2 mm.

[0035] In the prior art, in the fluidized reduction process of the existing pyrolusite, the coarse particle material and the fine particle material are mixed together and reduced and roasted in a furnace tube. In the reduction process at the same temperature, the same time and the same reducing atmosphere, the coarse particle material is not completely reduced and still exists in the form of MnO2, and the MnO2 is difficult to be leached in the subsequent sulfuric acid leaching process; or the fine particle material is easily excessively reduced and exists in the form of metallic Mn, and Mn is mixed in MnO and is also difficult to be leached in the subsequent sulfuric acid leaching process, resulting in a waste of energy and low resource utilization.

[0036] In the present invention, the present invention aims at the shortcomings of uneven reaction of different particles and energy waste in the fluidized reduction process of pyrolusite, and based on the characteristic that pyrolusite can be reduced into MnO and Mn in steps, a new process for preparing different manganese products by zoning reduction of pyrolusite is proposed. First, after pyrolusite is ground into powder, it enters the fluidized roasting system from the lower part of the high-temperature furnace tube, and the reaction gas (reducing gas) enters the system from the lower part of the furnace tube synchronously at a certain airflow speed, and the running direction is from bottom to top. Under the blowing of airflow, the pyrolusite powder passes through the grading screen arranged in the middle of the furnace tube and enters different positions of the furnace tube. The fine-grained pyrolusite powder is blown by the airflow through the sieve hole to the reduction zone at the upper part of the furnace tube, and the coarse-grained pyrolusite is retained in the reduction zone at the lower part of the furnace tube. Coarse-grained pyrolusite undergoes reduction reaction in the lower reduction zone of the furnace tube, and fine-grained pyrolusite undergoes reduction reaction in the upper reduction zone of the furnace tube. In the process, the airflow speeds in the lower reduction zone and the upper reduction zone of the furnace tube are adjusted respectively to control the materials to be suspended in the set temperature interval and reduction interval; the reducing gas and pyrolusite powders of different particle sizes undergo reduction reaction under the set temperature and time conditions in the respective reduction zones to generate MnO and Mn respectively, and the MnO and Mn are blown to the outside of the furnace tube by the airflow due to the weight loss of reduction and enter the water cooling system for cooling and then collected, and are used to prepare manganese sulfate and metallic manganese respectively.

[0037] In the present invention, by arranging independent real-time detection devices of O element and Mn element in the upper reduction zone and the lower reduction zone of the furnace tube respectively (such devices belong to the prior art, such as online iron content analyzer, etc.), the content of reducing gas in each reduction zone is adjusted according to the detected oxygen-manganese ratio result, so as to ensure the proper reduction of coarse particle material and fine particle material. The technical route of the present invention realizes the purpose of preparing different manganese products by partitioning reduction of pyrolusite materials of different particle sizes according to the process characteristics that MnO2 can be further reduced to generate metallic Mn after being reduced to MnO, and reduces carbon emissions. The process flow of the present invention is simple, easy to control, has good economic and environmental benefits, and can open up a more stable and efficient way for the development, promotion and utilization of pyrolusite.

[0038] In the present invention, after the pyrolusite is ground into powder, it is transported to the inside of the fluidized furnace tube from the feed port located at the lower side of the fluidized furnace tube and the air inlet at the bottom respectively with the reaction gas (reducing gas), and moves from bottom to top under the blowing action of the airflow, wherein the coarser material is intercepted by the screen in the middle of the furnace tube, and is suspended in the lower reduction zone of the furnace tube for reduction roasting treatment, and the reduced coarse material is discharged from the coarse material outlet located in the middle of the furnace tube (connected to the middle and upper part of the lower reduction zone of the furnace tube). Since the finer material is relatively light, it passes through the screen and forms a suspension in the upper reduction zone of the furnace tube for reduction roasting treatment, and the reduced fine material is discharged from the fine material outlet located at the top of the furnace tube (connected to the top of the upper reduction zone of the furnace tube). It should be noted that, during the reduction roasting process of the coarse material and the fine material, the proper reduction of the coarse particle material and the fine particle material is achieved by adjusting the content of the reducing gas according to the change of the oxygen-manganese ratio in the coarse material or the fine material, that is, the coarse particle material reacts in the reduction zone at the lower part of the furnace tube to generate MnO, and the fine particle material reacts in the reduction zone at the upper part of the furnace tube to generate Mn.

[0039] In the present invention, in the lower reduction zone of the furnace tube, pyrolusite powder and reaction gas (reducing gas) enter the lower part of the lower reduction zone at the same time, and by adjusting the flow rate of the reaction gas continuously entering, the fine particles (particle size is not more than 0.6mm, preferably not more than 0.4mm, more preferably not more than 0.2mm) in the pyrolusite powder can be further blown into the upper reduction zone of the furnace tube, and the coarse particles (particle size is 0.2-1mm, preferably 0.4-1mm, more preferably 0.6-1mm) remain in the lower reduction zone. Then, the roasting temperature in the lower reduction zone is adjusted to 700-1000°C (preferably 750-950°C, more preferably 800-900°C) for reduction roasting, and the roasting treatment time is such that all MnO2 in the coarse particles is reduced to MnO (generally 0.1-3h). During the reduction roasting process in this area, the changes in the contents of O and Mn in the coarse particle material are detected in real time by an element detection instrument, and the content of the reducing gas introduced into the lower reduction zone is adjusted according to the changes in the oxygen-manganese ratio in the coarse particle material, so that the coarse pyrolusite powder in the lower reduction zone is reduced to MnO. The monitoring and adjustment process is specifically as follows: the oxygen-manganese ratio in the coarse pyrolusite powder in the lower reduction zone is detected in real time and recorded as a1, then:

[0040] When 1<a1, the content of CO and / or H2 in the reducing gas is increased, and the increase amount is 3*(a1+1)*100%.

[0041] When 0.5<a1≤1, the current working condition remains unchanged.

[0042] When 0<a1≤0.5, the content of CO and / or H2 in the reducing gas is reduced by 4*(a1+2)*100%.

[0043] In the present invention, in the upper reduction zone of the furnace tube, after the fine particles in the pyrolusite powder are blown to the upper reduction zone of the furnace tube, the roasting temperature in the upper reduction zone is adjusted to 500-800°C (preferably 550-750°C, more preferably 600-700°C) for reduction roasting, and the roasting treatment time is such that all the MnO2 in the fine particles is reduced to Mn (generally 0.1-3h). During the reduction roasting process in this area, the changes in the content of O and Mn in the fine particles are detected in real time by an element detection instrument, and the content of the reducing gas introduced into the upper reduction zone is adjusted according to the changes in the oxygen-manganese ratio in the fine particles, so that the fine pyrolusite powder in the upper reduction zone is reduced to Mn. The monitoring and adjustment process is specifically as follows: the oxygen-manganese ratio in the fine pyrolusite powder in the upper reduction zone is detected in real time, and is recorded as a2, then:

[0044] When a2=0, the current operating condition remains unchanged.

[0045] When a2>0, the content of CO and / or H2 in the reducing gas is increased by 5*(a2+3)*100%.

[0046] In the present invention, the system for graded fluidized selective reduction of pyrolusite is a supporting system for the method for graded fluidized selective reduction of pyrolusite, and the existing common fluidized furnace tube is modified, that is, at least one screening device (a screen with screen holes) is added in the middle of the tube cavity of the furnace tube, and an air inlet and an air supply port are respectively provided at corresponding positions of the lower reduction zone and the upper reduction zone, and the graded and partitioned coarse particle materials and fine particle materials in the pyrolusite are realized under the joint action of the screen and the reaction gas, and selective reduction treatments of different temperatures and different reduction degrees are carried out in different reduction zones, that is, the reaction temperature and reaction time of pyrolusite of different particle sizes are dynamically and reasonably controlled, so that the coarse particle materials are reduced to prepare MnO products, and the fine particle materials are reduced to prepare metal Mn products, thereby realizing the optimized control of products and energy.

[0047] In the present invention, each material inlet and outlet is independently provided with a valve opening control valve, and each gas inlet and outlet is independently provided with a flow regulating valve. The valve opening control valve, the flow regulating valve, the heating device and the element content detection device can all be connected to the intelligent control cabinet, and automatic material inlet and outlet, gas inlet and outlet, element content detection and independent regional temperature control can be performed through pre-set programs.

[0048] In the present invention, the lower reduction zone and the upper reduction zone of the furnace tube can both uniformly convey the reaction gas from the lower part of the furnace tube, or can convey the reaction gas separately and independently, which can be adjusted according to actual working conditions.

[0049] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0050] 1: The present invention adds a screen in the furnace tube to grade pyrolusite of different particle sizes into different positions of the furnace tube, so that the coarse particle material realizes MnO2 reduction to MnO in the high temperature zone at the lower part of the furnace tube; the fine particle material realizes MnO2 reduction to MnO in the low temperature zone at the upper part of the furnace tube and then further reduces to generate metallic Mn. The method utilizes the difference in reaction rate of pyrolusite of different particle sizes, sets sieves of different particle sizes inside the furnace tube, and combines the characteristics of high temperature at the lower part and low temperature at the upper part of the high temperature furnace tube to realize the zoning reduction of materials of different particle sizes, prepare different manganese products, avoid the presence of insoluble manganese in the subsequent leaching process to prepare high-purity manganese sulfate products, and also greatly reduce energy consumption.

[0051] 2: The system for graded fluidized selective reduction of pyrolusite provided by the present invention has a simple structure and low manufacturing cost. While meeting the requirements of graded and zoned reduction of the method of the present invention, it also has the characteristics of high reduction efficiency, low energy consumption, and convenient operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 The process flow chart of the method of the present invention is shown in FIG.

[0053] Figure 2 This is a structural diagram of the system for staged fluidized selective reduction according to the present invention.

[0054] Figure numerals: 1: furnace tube; 101: lower chamber; 102: upper chamber; 2: screen; 3: air inlet; 4: feed inlet; 5: coarse material outlet; 6: fine material outlet; 7: element content detection device; 8: heating device; 9: air supply port. DETAILED DESCRIPTION

[0055] The technical solution of the present invention is illustrated below by way of example, and the scope of protection requested by the present invention includes but is not limited to the following embodiments.

[0056] A system for graded fluidized selective reduction of pyrolusite, the fluidized selective reduction system comprising a furnace tube 1 and a screen 2. The screen 2 is arranged in the tube cavity of the furnace tube 1, and divides the tube cavity of the furnace tube 1 into a lower chamber 101 and an upper chamber 102, and screen holes are provided on the screen 2. An air inlet 3 is arranged at the bottom end of the furnace tube 1, a feed inlet 4 is arranged on the lower side wall of the furnace tube 1, a coarse material outlet 5 is arranged on the middle side wall of the furnace tube 1, and a fine material outlet 6 is arranged at the top of the furnace tube 1. The air inlet 3, the feed inlet 4, and the coarse material outlet 5 are all connected to the lower chamber 101, and the fine material outlet 6 is connected to the upper chamber 102. An element content detection device 7 and a heating device 8 with respective temperature control are also independently arranged in the lower chamber 101 and the upper chamber 102.

[0057] Preferably, a plurality of screens 2 are arranged in the tube cavity of the furnace tube 1 , and a lower chamber 101 is formed below the plurality of screens 2 , and an upper chamber 102 is formed above the plurality of screens 2 .

[0058] Preferably, the screen 2 is movably arranged in the tube cavity of the furnace tube 1 and can move in the vertical direction.

[0059] Preferably, a gas supply port 9 communicating with the upper chamber 102 is further provided at the upper portion of the furnace tube 1 .

[0060] Preferably, the mesh size of the screen 2 is not greater than 0.6 mm, preferably not greater than 0.4 mm, and more preferably not greater than 0.2 mm.

[0061] Example 1

[0062] A system for graded fluidized selective reduction of pyrolusite, the fluidized selective reduction system comprising a furnace tube 1 and a screen 2. The screen 2 is arranged in the tube cavity of the furnace tube 1, and divides the tube cavity of the furnace tube 1 into a lower chamber 101 and an upper chamber 102, and screen holes are provided on the screen 2. An air inlet 3 is arranged at the bottom end of the furnace tube 1, a feed inlet 4 is arranged on the lower side wall of the furnace tube 1, a coarse material outlet 5 is arranged on the middle side wall of the furnace tube 1, and a fine material outlet 6 is arranged at the top of the furnace tube 1. The air inlet 3, the feed inlet 4, and the coarse material outlet 5 are all connected to the lower chamber 101, and the fine material outlet 6 is connected to the upper chamber 102. An element content detection device 7 and a heating device 8 with respective temperature control are also independently arranged in the lower chamber 101 and the upper chamber 102.

[0063] Example 2

[0064] The embodiment 1 is repeated, except that the screen 2 is movably arranged in the tube cavity of the furnace tube 1 and can move in the vertical direction.

[0065] Example 3

[0066] Example 2 is repeated, except that a gas supply port 9 communicating with the upper chamber 102 is further provided on the upper portion of the furnace tube 1 .

[0067] Example 4

[0068] Example 3 is repeated, except that a plurality of screens 2 are arranged in the tube cavity of the furnace tube 1 , the lower part of the plurality of screens 2 is a lower chamber 101 , and the upper part of the plurality of screens 2 is an upper chamber 102 .

[0069] Example 5

[0070] Example 4 was repeated except that the mesh size of the mesh 2 was 0.6 mm.

[0071] Example 6

[0072] Example 4 was repeated except that the mesh size of the mesh 2 was 0.4 mm.

[0073] Example 7

[0074] Example 4 was repeated except that the mesh size of the mesh 2 was 0.2 mm.

[0075] Application Example 1

[0076] For a certain African pyrolusite with a MnO2 content of 28.67%, the pyrolusite is ground into powder and transported to a fluidized pipe. At the same time, a reaction gas containing reducing gas is transported into the pipe for reduction roasting reaction, wherein: the sieve hole diameter of the middle screen of the furnace tube is 0.4mm, and the number of screens is 1. The reducing gas in the initial reaction gas is CO, the content of reducing gas is 40%, the content of inert gas N2 is 60%, and the conveying flow rate of the initial reaction gas is 1.0m / s. The temperature of the coarse particle reduction reaction at the bottom of the furnace tube is adjusted to 900℃, and the reaction time is 1.5h; the temperature of the fine particle reduction reaction at the top of the furnace tube is adjusted to 700℃, and the reaction time is 1.0h.

[0077] In the lower reduction zone of the furnace tube: for the coarse-grained pyrolusite at the lower part of the furnace tube, at the initial stage of the reaction, it is detected that a1=2.3, then it is judged that at this time, all the manganese elements in the lower reduction zone exist in the form of MnO2, so it is judged that the reducing gas content contained in the reaction gas in the lower reduction zone is insufficient. At this time, the reducing gas content that needs to be increased is 9.9%, that is, the reducing gas content contained in the reaction gas introduced into the lower reduction zone of the furnace tube is adjusted to increase to 49.9% (the content of inert gas N2 is reduced to 50.1%); after increasing the reducing gas content, the reaction is continued until the detected O / Mn interval is 0.5<a1≤1.0, and the reducing gas content contained in the current reaction gas is kept unchanged until the reaction is completed. The TMn content in the product obtained after the reaction is complete is 36.16%, and the Mn content is 2.6%. 2+ The content is 35.89%, Mn2+ / TMn=99.25%.

[0078] In the upper reduction zone of boiler tube: at the fine-grained pyrolusite on boiler tube top, in the initial stage of reaction, detect a2=1.1, then judge that the upper reduction zone reduces MnO at this moment For the reaction of metallic Mn is not thorough, therefore judge that the reducing gas content contained by reaction gas in the upper reduction zone is not enough, and the reducing gas content that needs to increase by the air supply port is 20.5% at this moment; Promptly regulate the content of reducing gas contained by the reaction gas passing into the upper reduction zone of boiler tube to increase to 60.5% (inert gas N Content is reduced to 39.5%), continue to react after improving the reducing gas content, until the value a2=0 of the O / Mn of the detection detected, keep the reducing gas content contained by the current reaction gas constant until reaction is completed, and in the product that obtains after reacting completely, TMn content is 36.92%, Mn 2+ The content is 0.0%, the metal Mn content is 36.92%, the metal Mn / TMn=100.00%, and the reduction reaction to metal manganese is thorough.

[0079] Application Example 2

[0080] Example 1 was repeated except that the reducing gas was H2;

[0081] After the reaction in the reduction zone at the top of the furnace tube is complete, the product obtained has a TMn content of 38.20% and a Mn content of 38.20%. 2+ The content is 37.96%, Mn 2+ / TMn=99.37%.

[0082] After the reaction in the reduction zone at the top of the furnace tube is complete, the product obtained has a TMn content of 37.85% and a Mn content of 37.85%. 2+ The content is 0.0%, the metal Mn content is 37.85%, the metal Mn / TMn=100.00%, and the reduction reaction to metal manganese is thorough.

Claims

1. A method for selective reduction of pyrolusite by fluidization, characterized in that: The method comprises the following steps: 1) crushing the pyrolusite to obtain pyrolusite powder, and inputting the obtained pyrolusite powder and reducing gas from the lower feed port of the fluidized bed furnace tube; 2) In the fluidized bed furnace tube, according to the direction of the material, the fluidized bed furnace tube is divided into a lower reduction zone and an upper reduction zone by a screen. Under the pushing action of the reducing gas, the coarse pyrolusite powder is reduced and roasted in the lower reduction zone, and the fine pyrolusite powder is reduced and roasted in the upper reduction zone; 3) According to the changes in the contents of O and Mn in the coarse pyrolusite powder in the lower reduction zone, the content of the reducing gas introduced into the lower reduction zone is adjusted so that the coarse pyrolusite powder in the lower reduction zone is reduced to MnO; according to the changes in the contents of O and Mn in the fine pyrolusite powder in the upper reduction zone, the content of the reducing gas introduced into the upper reduction zone is adjusted so that the fine pyrolusite powder in the upper reduction zone is reduced to Mn.

2. The method according to claim 1, characterized in that: The method further includes: 4) The MnO obtained in step 3) is discharged from the coarse particle discharge port located in the middle of the fluidized bed furnace tube, and is used to prepare manganese sulfate after cooling; the Mn obtained in step 3) is discharged from the fine particle discharge port located at the top of the fluidized bed furnace tube, and is used to prepare metallic manganese after cooling.

3. The method according to claim 1 or 2, characterized in that: In step 1), the particle size of the pyrolusite powder is not greater than 1 mm, preferably 0.1-1 mm, more preferably 0.15-1 mm; and / or In step 2), the particle size of the coarse pyrolusite powder is 0.2-1 mm, preferably 0.4-1 mm, more preferably 0.6-1 mm; the particle size of the fine pyrolusite powder is not greater than 0.6 mm, preferably not greater than 0.4 mm, more preferably not greater than 0.2 mm.

4. The method according to any one of claims 1 to 3, characterized in that: The reducing gas is a mixed gas containing CO and / or H2, preferably a mixed gas consisting of CO and / or H2 and an inert gas, more preferably a mixed gas consisting of CO and / or H2 and nitrogen; Preferably, in the mixed gas, the total content of CO and / or H2 is not less than 3% of the total amount of the mixed gas, preferably not less than 5%, and more preferably not less than 8%.

5. The method according to claim 4, characterized in that: The flow rate of the reducing gas introduced into the fluidized bed furnace tube is 0.2-3 m / s, preferably 0.3-2.5 m / s, and more preferably 0.4-2 m / s.

6. The method according to any one of claims 1 to 5, characterized in that: The reduction temperature in the lower reduction zone is 700-1000°C, preferably 750-950°C, more preferably 800-900°C; the reduction time in the lower reduction zone is 0.1-3h, preferably 0.3-2.5h, more preferably 0.5-2h; and / or The reduction temperature in the upper reduction zone is 500-800°C, preferably 550-750°C, and more preferably 600-700°C; the reduction time in the upper reduction zone is 0.1-3h, preferably 0.3-2.5h, and more preferably 0.5-2h.

7. The method according to any one of claims 1 to 6, characterized in that: In step 3), according to the changes in the contents of O and Mn in the crude pyrolusite powder in the lower reduction zone, the content of the reducing gas introduced into the lower reduction zone is adjusted so that the crude pyrolusite powder in the lower reduction zone is reduced to MnO. Specifically, the oxygen-manganese ratio in the crude pyrolusite powder in the lower reduction zone is detected in real time and recorded as a1, then: When 1<a1, the content of CO and / or H2 in the reducing gas is increased by 3*(a1+1)*100%; When 0.5<a1≤1, the current working condition remains unchanged; When 0<a1≤0.5, the content of CO and / or H2 in the reducing gas is reduced by 4*(a1+2)*100%.

8. The method according to any one of claims 1 to 7, characterized in that: In step 3), according to the changes in the contents of O and Mn in the fine manganese ore powder in the upper reduction zone, the content of the reducing gas introduced into the upper reduction zone is adjusted so that the fine manganese ore powder in the upper reduction zone is reduced to Mn. Specifically, the oxygen-manganese ratio in the fine manganese ore powder in the upper reduction zone is detected in real time and recorded as a2, then: When a2=0, the current working condition remains unchanged; When a2>0, the content of CO and / or H2 in the reducing gas is increased by 5*(a2+3)*100%.

9. A fluidized selective reduction system for the method according to any one of claims 1 to 8, characterized in that: The fluidized selective reduction system comprises a furnace tube (1) and a screen (2); the screen (2) is arranged in the tube cavity of the furnace tube (1) and divides the tube cavity of the furnace tube (1) into a lower chamber (101) and an upper chamber (102); the screen (2) is provided with screen holes; an air inlet (3) is arranged at the bottom end of the furnace tube (1), a feed inlet (4) is arranged on the lower side wall of the furnace tube (1), a coarse material outlet (5) is arranged on the middle side wall of the furnace tube (1), and a fine material outlet (6) is arranged at the top end of the furnace tube (1); the air inlet (3), the feed inlet (4) and the coarse material outlet (5) are all connected to the lower chamber (101), and the fine material outlet (6) is connected to the upper chamber (102); an element content detection device (7) and a heating device (8) with respective temperature control are also independently arranged in the lower chamber (101) and the upper chamber (102); Preferably, the screen (2) is movably arranged in the tube cavity of the furnace tube (1) and can move in the vertical direction; Preferably, a gas supply port (9) connected to the upper chamber (102) is also provided at the upper part of the furnace tube (1).

10. The system according to claim 9, characterized in that: A plurality of screens (2) are arranged in the tube cavity of the furnace tube (1), the lower part of the plurality of screens (2) is a lower chamber (101), and the upper part of the plurality of screens (2) is an upper chamber (102); Preferably, the mesh size of the sieve (2) is not greater than 0.6 mm, preferably not greater than 0.4 mm, and more preferably not greater than 0.2 mm.