Efficient leaching method for carbonate type uranium ore difficult to treat
Through high-temperature oxidative decomposition and the addition of alkali leaching reagents, the processing difficulties caused by sulfides and clay minerals in carbonate uranium ores are solved, the uranium leaching rate and extraction efficiency are improved, and the uranium content in the tailings is reduced. Efficient uranium ore leaching was achieved.
Patent Information
- Application Number
- CN202310427880.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-22
AI Technical Summary
Carbonate uranium ores contain sulfides and clay minerals, which makes hydrometallurgical processing difficult. Acid leaching requires a large amount of sulfuric acid. Alkaline leaching is less effective and has a low leaching rate, so it cannot be effectively developed and utilized.
Decompose the sulfide wrapped in the ore through high-temperature oxidation to expose uranium minerals, and add alkali and leaching aid reagents to adjust the slurry liquid-to-solid ratio and reaction conditions to increase the uranium leaching rate and reduce the uranium content in the tailings, using the ion exchange method Recycle uranium.
The leaching rate of uranium is increased, the amount of alkali used for subsequent leaching and the uranium content in the tailings are reduced, and the uranium extraction efficiency is improved.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of uranium ore processing, and in particular to a method for efficiently leaching refractory carbonate uranium ore. Background Art
[0002] Among the proven uranium resources in my country, carbonate uranium ore accounts for a certain proportion, with a total reserve of tens of thousands of tons. Some of the uranium ores have complex mineral properties. In addition to being rich in carbonate minerals, they also contain high levels of sulfides and clay minerals. The uranium in the ore is closely related to sulfides, clay minerals, carbonates and other minerals. This type of uranium ore is difficult to process by hydrometallurgy. When acid leaching is used, a large amount of sulfuric acid and a high residual acidity are required. However, excessive residual acidity, the dissolution of a large number of impurities and the expansion of clay minerals bring difficulties to subsequent extraction. When conventional alkaline leaching is used, the uranium leaching effect is poor and the leaching rate is low. Therefore, this type of uranium ore has not been effectively developed and utilized. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a method for efficiently leaching refractory carbonate uranium ore, which can efficiently leach uranium from refractory carbonate uranium ore containing sulfide and clay minerals.
[0004] The present invention provides a method for efficiently leaching refractory carbonate uranium ore, comprising the following steps:
[0005] Step 1: crushing and grinding carbonate uranium ore containing clay minerals and sulfides;
[0006] Step 2: Add the ground ore in step 1 to the slurry, adjust the slurry-to-solid ratio, and react for a period of time. During the reaction, ensure that oxygen is introduced;
[0007] Step 3: Add alkali and leaching agent, continue the reaction, and ensure that oxygen is introduced;
[0008] Step 4: The ore pulp is separated into solid and liquid, and the obtained leaching solution is used to recover uranium by ion exchange method. The leaching tailings are dried and analyzed for uranium content.
[0009] Preferably, in the step 1, the ore is ground to a particle size of -100 mesh to -300 mesh.
[0010] Preferably, in step 2, the liquid-to-solid ratio of the slurry is 0.5:1 to 5:1.
[0011] Preferably, in the step 2, the reaction temperature is 120°C to 180°C.
[0012] Preferably, in the step 2, the reaction time is 0.5 to 2 hours.
[0013] Preferably, in step 2, the oxygen partial pressure is 0.2 MPa to 1.0 MPa.
[0014] Preferably, in step three, the alkali is a mixture of sodium carbonate and sodium bicarbonate, the mass ratio of the two is 2:1 to 5:1, and the amount of the alkali is 4% to 10% of the mass of the slurry.
[0015] Preferably, the dosage of the leaching aid is 0.2% to 1.2% of the mass of the slurry.
[0016] Preferably, in the step three, the reaction temperature is 120° C. to 180° C., and the reaction time is 1 to 5 hours.
[0017] Preferably, in step three, the oxygen partial pressure is 0.2 MPa to 1.0 MPa.
[0018] Compared with the prior art, the method for efficiently leaching a difficult-to-treat carbonate uranium ore of the present invention first decomposes the sulfides encapsulating the uranium minerals in the ore by high-temperature oxidation to expose the uranium minerals, thereby increasing the uranium leaching rate and reducing the amount of alkali used in subsequent leaching; after the sulfides are decomposed, alkali and leaching aids are added to effectively reduce the uranium content in the tailings and increase the uranium leaching rate. DETAILED DESCRIPTION
[0019] In order to further understand the present invention, the embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the present invention.
[0020] The embodiment of the present invention discloses a method for efficiently leaching refractory carbonate uranium ore, comprising the following steps:
[0021] Step 1: crushing and grinding carbonate uranium ore containing clay minerals and sulfides;
[0022] Preferably, the ore is ground to a particle size of -100 mesh to -300 mesh.
[0023] Step 2: Add the ground ore in step 1 to the slurry, adjust the slurry-to-solid ratio, and react for a period of time. During the reaction, ensure that oxygen is introduced;
[0024] The liquid-to-solid ratio of the slurry is preferably 0.5:1 to 5:1, more preferably 1.5:1 to 2:1.
[0025] The reaction temperature is 120°C to 180°C, more preferably 150°C to 170°C.
[0026] The reaction time is 0.5 to 2 hours, more preferably 1 to 1.5 hours.
[0027] The oxygen partial pressure is 0.2MPa~1.0MPa.
[0028] Through high-temperature oxidation, the sulfides encapsulating uranium minerals in the ore are decomposed, the uranium minerals are exposed, the uranium leaching rate is increased, and the amount of alkali used in subsequent leaching is reduced.
[0029] Step 3: Add alkali and leaching agent, continue the reaction, and ensure that oxygen is introduced;
[0030] After the sulfide is decomposed in step 2, the uranium content in the tailings is effectively reduced by adding alkali and leaching aids to increase the final uranium leaching rate.
[0031] The alkali is a mixture of sodium carbonate and sodium bicarbonate, the mass ratio of the two is 2:1-5:1, and the amount of the alkali is 4%-10% of the mass of the ore pulp.
[0032] The dosage of the leaching aid is 0.2% to 1.2% of the mass of the ore pulp.
[0033] The reaction temperature is 120° C. to 180° C., and the reaction time is 1 to 5 hours.
[0034] The oxygen partial pressure is 0.2MPa~1.0MPa.
[0035] Step 4: The ore pulp is separated into solid and liquid, and the obtained leaching solution is used to recover uranium by ion exchange method. The leaching tailings are dried and analyzed for uranium content.
[0036] In order to further understand the present invention, the method for efficient leaching of refractory carbonate uranium ore provided by the present invention is described in detail below in conjunction with embodiments, and the protection scope of the present invention is not limited by the following embodiments.
[0037] Example 1
[0038] The uranium grade of a carbonate uranium mine is 0.111%, the sulfide content is 6.35%, the CO2 content is 16.53%, and the ore contains medium clay minerals such as chlorite, illite, and montmorillonite. The chlorite content is 36.43% and the illite content is 11.67%.
[0039] (1) crushing and grinding the refractory carbonate uranium ore to obtain an ore particle size of -200 mesh;
[0040] (2) 100 g of the ore ground to a certain particle size in step (1) was added to a reaction vessel, the slurry liquid-to-solid ratio was adjusted to 1.5:1, and the reaction was carried out at 160° C. for 1 h with an oxygen partial pressure of 0.5 MPa;
[0041] (3) After step (2) is completed, add alkali and leaching agent, the amount of alkali is 7% of the mass of the ore pulp, the mass ratio of sodium carbonate to sodium bicarbonate is 3:1, the amount of leaching agent is 0.3% of the mass of the ore pulp, and react at 160° C. for 3 hours, and the oxygen partial pressure is 0.5 MPa;
[0042] (4) After step (3) is completed, the slurry is subjected to solid-liquid separation, the obtained leaching solution is used to recover uranium by ion exchange, and the leaching tailings are dried and analyzed for uranium content.
[0043] Experimental effect: After adopting the process of the present invention, the uranium content in the leaching tailings can be effectively reduced. The uranium content of the leaching tailings is 0.013%, and the uranium leaching rate of the slag is 88.3%.
[0044] Example 2
[0045] The uranium grade of a carbonate uranium mine is 0.111%, the sulfide content is 6.35%, the CO2 content is 16.53%, and the ore contains medium clay minerals such as chlorite, illite, and montmorillonite. The chlorite content is 36.43% and the illite content is 11.67%.
[0046] (1) crushing and grinding the refractory carbonate uranium ore to obtain an ore particle size of -200 mesh;
[0047] (2) 5000 g of the ore ground to a certain particle size in step (1) was added to a reaction vessel, the slurry liquid-to-solid ratio was adjusted to 1.5:1, and the reaction was carried out at 160° C. for 1 h with an oxygen partial pressure of 0.5 MPa;
[0048] (3) After step (2) is completed, add alkali and leaching agent, the amount of alkali is 7% of the mass of the ore pulp, the mass ratio of sodium carbonate to sodium bicarbonate is 3:1, the amount of leaching agent is 0.3% of the mass of the ore pulp, and react at 160° C. for 3 hours, and the oxygen partial pressure is 0.5 MPa;
[0049] (4) After step (3) is completed, the slurry is subjected to solid-liquid separation, the obtained leaching solution is used to recover uranium by ion exchange, and the leaching tailings are dried and analyzed for uranium content.
[0050] Experimental results: After adopting the process of the present invention, the uranium content in the leaching tailings can be effectively reduced. The uranium content of the leaching tailings is 0.015%, and the uranium leaching rate of the slag is 86.5%.
[0051] Comparative Example 1
[0052] The uranium grade of a carbonate uranium mine is 0.111%, the sulfide content is 6.35%, the CO2 content is 16.53%, and the ore contains medium clay minerals such as chlorite, illite, and montmorillonite. The chlorite content is 36.43% and the illite content is 11.67%.
[0053] (1) crushing and grinding the refractory carbonate uranium ore to obtain an ore particle size of -200 mesh;
[0054] (2) 100 g of the ore ground to a certain particle size in step (1) was added to a reaction vessel, the slurry liquid-to-solid ratio was adjusted to 1.5:1, alkali and leaching aids were added, the alkali dosage was 8%, the sodium carbonate:sodium bicarbonate ratio was 3:1, the leaching aid dosage was 0.3%, and the reaction was carried out at 160° C. for 4 h, and the oxygen partial pressure was 0.5 MPa;
[0055] (3) After step (2) is completed, the ore pulp is subjected to solid-liquid separation, the obtained leaching solution is used to recover uranium by ion exchange, and the leaching tailings are dried and analyzed for uranium content.
[0056] Test results: The uranium content of the leached tailings is 0.023%, and the uranium leaching rate based on the slag is 79.3%.
[0057] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0058] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for efficient leaching of refractory carbonate uranium ore, characterized in that: The following steps are involved: Step 1: crushing and grinding carbonate uranium ore containing clay minerals and sulfides; Step 2: Add the ground ore in step 1 to the slurry, adjust the slurry-to-solid ratio, and react for a period of time. During the reaction, ensure that oxygen is introduced; Step 3: Add alkali and leaching agent, continue the reaction, and ensure that oxygen is introduced; Step 4: The ore pulp is separated into solid and liquid, and the obtained leaching solution is used to recover uranium by ion exchange method. The leaching tailings are dried and analyzed for uranium content.
2. The method for efficient leaching of refractory carbonate uranium ore according to claim 1, characterized in that: In the step 1, the ore is ground to a particle size of -100 mesh to -300 mesh.
3. The method for efficient leaching of refractory carbonate uranium ore according to claim 1, characterized in that: In the step 2, the liquid-to-solid ratio of the slurry is 0.5:1 to 5:
1.
4. The method for efficient leaching of refractory carbonate uranium ore according to claim 1, characterized in that: In the step 2, the reaction temperature is 120°C to 180°C.
5. The method for efficient leaching of refractory carbonate uranium ore according to claim 4, characterized in that: In the step 2, the reaction time is 0.5 to 2 hours.
6. The method for efficient leaching of refractory carbonate uranium ore according to claim 5, characterized in that: In the step 2, the oxygen partial pressure is 0.2 MPa to 1.0 MPa.
7. The method for efficient leaching of refractory carbonate uranium ore according to claim 1, characterized in that: In the step three, the alkali is a mixture of sodium carbonate and sodium bicarbonate, the mass ratio of the two is 2:1 to 5:1, and the amount of the alkali is 4% to 10% of the mass of the slurry.
8. The method for efficient leaching of refractory carbonate uranium ore according to claim 1, characterized in that: The dosage of the leaching aid is 0.2% to 1.2% of the mass of the ore pulp.
9. The method for efficient leaching of refractory carbonate uranium ore according to claim 1, characterized in that: In the step 3, the reaction temperature is 120° C. to 180° C., and the reaction time is 1 to 5 hours.
10. The method for efficient leaching of refractory carbonate uranium ore according to claim 9, characterized in that: In the step 3, the oxygen partial pressure is 0.2 MPa to 1.0 MPa.