Piston rod for high-strength corrosion-resistant high-pressure oil cylinder and preparation method of piston rod

Through the combination technology of nickel-manganese coating and laser cladding layer, the problems of high operating temperature and high cost in the existing technology are solved, the preparation of high-strength, corrosion-resistant and low-cost piston rod is realized, and the hardness and hardness of the piston rod are significantly improved. Corrosion resistance.

CN118814162APending Publication Date: 2024-10-22JIANGYIN JINWAN ALLOY MATERIAL CO LTD

Patent Information

Application Number
CN202410797231.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the existing surface treatment methods for high-strength and corrosion-resistant precision piston rods, the operating temperature is too high and the holding time is too long, resulting in high production costs.

Method used

A combination of nickel-manganese plating and laser cladding technology is used to prepare high-strength, corrosion-resistant, high-pressure cylinder piston rods through electroplating and laser cladding. The raw materials for the nickel-manganese plating include butyne glycol ethoxy compounds and sodium chloride. , boric acid, manganese sulfate, saccharin and nickel sulfate hexahydrate. The raw materials of the laser cladding layer include copper powder and chromium powder. The thickness ratio of the nickel-manganese plating layer and the laser cladding layer is 1:1.

Benefits of technology

Effectively improve the surface hardness and wear resistance of the piston rod, reduce the self-corrosion current density, improve the corrosion resistance, reduce production costs, and avoid operating at high temperatures for too long.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004902137550000061
    Figure BDA0004902137550000061
  • Figure BDA0004902137550000071
    Figure BDA0004902137550000071
Patent Text Reader

Abstract

The invention discloses a piston rod for a high-strength corrosion-resistant high-pressure oil cylinder and a preparation method of the piston rod, and particularly relates to the technical field of piston rods. The nickel-manganese plating layer and the laser cladding layer are manufactured on the surface of the piston rod, so that the surface hardness of the piston rod can be effectively improved, the high-strength and high-pressure resistance of the piston rod is ensured, the surface wear resistance of the piston rod can be effectively improved, and the corrosion resistance of the surface of the piston rod can be effectively improved; the butynediol ethyoxyl compound obviously inhibits the cathode reduction reaction of metal ions, grains are refined, and a flat and high-microhardness coating can be obtained; in the preparation process of the nickel-manganese plating layer, electroplating treatment is adopted, the operation temperature is low, the dangerous situation that the operation temperature is too high does not exist, and the production cost can be effectively reduced; and laser cladding treatment is adopted for preparing the laser cladding layer, so that the processing operation time can be effectively shortened, and the situation that the high-temperature holding time is too long during operation can be effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of piston rods, and more specifically, to a high-strength, corrosion-resistant, high-pressure oil cylinder piston rod and a preparation method thereof. Background Art

[0002] The piston rod is a connecting component that supports the piston to do work, and is mainly used in oil cylinders and cylinder motion actuators; the function of the piston rod is to connect the piston and the crosshead, transmit the force applied to the piston and drive the piston to move; the piston rod is a mechanical part made of high-strength material, and usually needs to have a certain toughness and hardness to withstand high pressure and high-speed movement.

[0003] The patent (CN113249680B) discloses a surface treatment method for a high-strength, corrosion-resistant, precision piston rod, including: ultrasonic cleaning of the piston rod, heat preservation at 800-1000°C and then cooling to about 500°C, nitriding the preheated piston rod in a carbonitriding agent containing iron-doped graphene, urea, chromium oxide, molybdenum oxide, vanadium oxide, nickel oxide, borax, charcoal, and oxides of titanium, cobalt, and niobium; heating the nitrided piston rod to 1050-1100°C for quenching, then soaking and cooling in a coolant, and finally tempering. The method of the present invention helps to significantly refine the grains, improve the strength and uniformity of the surface hardness of the piston rod, and is conducive to maintaining a high precision for a long time. The addition of other transition metal oxides can make the piston rod obtain exceptionally excellent salt spray corrosion resistance and wear resistance.

[0004] The surface treatment method for the high-strength, corrosion-resistant precision piston rod in the above patent document has an operating temperature that is too high and the high operating temperature is maintained for too long, resulting in excessively high production and processing costs. Summary of the invention

[0005] In order to overcome the above-mentioned defects of the prior art, an embodiment of the present invention provides a high-strength, corrosion-resistant, high-pressure oil cylinder piston rod and a preparation method thereof.

[0006] A high-strength, corrosion-resistant piston rod for a high-pressure oil cylinder comprises a piston rod substrate, a nickel-manganese coating and a laser cladding layer, wherein the nickel-manganese coating is arranged on the surface of the piston rod substrate, and the laser cladding layer is arranged on the surface of the nickel-manganese coating.

[0007] Furthermore, the raw materials of the nickel-manganese plating layer include, by weight percentage, 0.054-0.064% of butynediol ethoxylate, 5.81-5.87% of sodium chloride, 13.60-13.64% of boric acid, 2.30-2.37% of manganese sulfate, 0.37-0.41% of saccharin, 0.30-0.33% of sodium dodecyl sulfate, and the rest is nickel sulfate hexahydrate.

[0008] Furthermore, the raw materials of the laser cladding layer include, by weight percentage, 4.9-5.1% copper powder, 14.8-15.2% chromium powder, and the rest nickel powder.

[0009] Furthermore, the raw materials of the nickel-manganese plating layer include, by weight percentage, 0.058-0.060% of butine diol ethoxylate, 5.83-5.85% of sodium chloride, 13.61-13.63% of boric acid, 2.32-2.35% of manganese sulfate, 0.38-0.40% of saccharin, 0.31-0.32% of sodium dodecyl sulfate, and the rest is nickel sulfate hexahydrate; the raw materials of the laser cladding layer include, by weight percentage, 4.95-5.05% of copper powder, 14.9-15.1% of chromium powder, and the rest is nickel powder.

[0010] Furthermore, the raw materials of the nickel-manganese plating layer include, by weight percentage, 0.059% of butine diol ethoxylate, 5.84% of sodium chloride, 13.62% of boric acid, 2.34% of manganese sulfate, 0.39% of saccharin, 0.32% of sodium dodecyl sulfate, and the rest is nickel sulfate hexahydrate; the raw materials of the laser cladding layer include, by weight percentage, 5.0% of copper powder, 15.0% of chromium powder, and the rest is nickel powder.

[0011] Furthermore, the thickness ratio of the nickel-manganese plating layer to the laser cladding layer is 1:1.

[0012] The present invention also provides a method for preparing a high-strength, corrosion-resistant, high-pressure oil cylinder piston rod, and the specific preparation steps are as follows:

[0013] Step 1: Weigh butynediol ethoxylate, sodium chloride, boric acid, manganese sulfate, saccharin, sodium dodecyl sulfate, nickel sulfate hexahydrate in the raw materials for nickel-manganese plating, and copper powder, chromium powder, and nickel powder in the raw materials for laser cladding layer;

[0014] Step 2: adding the sodium chloride, boric acid, manganese sulfate and nickel sulfate hexahydrate in step 1 into deionized water, performing ultrasonic treatment for 10 to 20 minutes, then adding butynediol ethoxylate, saccharin and sodium dodecyl sulfate, and continuing ultrasonic treatment for 10 to 20 minutes to obtain a plating solution;

[0015] Step 3: ball milling the copper powder, chromium powder and nickel powder in step 1 for 20 to 40 minutes to obtain a mixed powder;

[0016] Step 4: placing the piston rod substrate into a plating solution for electroplating to form a nickel-manganese coating on the surface of the piston rod substrate, and annealing the piston rod with the nickel-manganese coating to obtain a piston rod with an annealed nickel-manganese coating;

[0017] Step 5: The mixed powder is subjected to laser cladding treatment by a laser, and a laser cladding layer is produced on the surface of the annealed nickel-manganese coating to obtain a high-strength, corrosion-resistant, high-pressure cylinder piston rod.

[0018] Furthermore, in step 2, the ultrasonic frequency is 1.4-1.6 MHz, the ultrasonic power is 400-600 W, and the weight ratio of nickel sulfate hexahydrate to deionized water is 1:4.9-5.1; in step 3, a planetary ball mill is used for ball milling, the orbital speed is 360-480 r / min, and the rotation speed is 720-960 r / min.

[0019] Furthermore, before placing the piston rod in the plating solution, the piston rod is first placed in deionized water for ultrasonic cleaning; in step 4, the plating solution temperature is maintained at 33-39°C, the plating solution pH value is 3.8-4.2, and the current density is 1.5-1.7A / dm 2 , the electroplating time is 5.5-6.5h; the annealing temperature is 290-310°C; in step five, a high-speed laser combined with coaxial powder feeding is used for laser cladding, the laser power is 2100-2300W, the defocus is 0, and the scanning rate is 500-600mm / min.

[0020] Further, in step 2, the ultrasonic frequency is 1.5 MHz, the ultrasonic power is 500 W, and the weight ratio of nickel sulfate hexahydrate to deionized water is 1:5.0; in step 3, a planetary ball mill is used for ball milling, the revolution speed is 420 r / min, and the rotation speed is 840 r / min; in step 4, the plating solution temperature is maintained at 36°C, the plating solution pH value is 4.0, and the current density is 1.6 A / dm 2 , the electroplating time is 6.0h; the annealing temperature is 300℃; in step five, a high-speed laser combined with coaxial powder feeding is used for laser cladding, the laser power is 2200W, the defocus is 0, and the scanning rate is 550mm / min.

[0021] Technical effects and advantages of the present invention:

[0022] 1. The high-strength, corrosion-resistant, high-pressure oil cylinder piston rod prepared by the raw material formula of the present invention has a nickel-manganese coating and a laser cladding layer on the surface of the piston rod, which can effectively improve the surface hardness of the piston rod, ensure the high-strength and high-pressure resistance of the piston rod, effectively improve the surface wear resistance of the piston rod, improve the self-corrosion potential of the piston rod surface, and reduce the self-corrosion current density of the piston rod surface, thereby effectively improving the corrosion resistance of the piston rod surface; the addition of butynediol ethoxylate causes the cathode polarization potential to shift to a more negative direction, significantly inhibits the cathode reduction reaction of metal ions, refines the grains, and helps to obtain a smooth, high-microhardness coating; in the preparation process of the nickel-manganese coating, electroplating treatment is used, the operating temperature is low, there is no dangerous situation of excessively high operating temperature, and the production cost can be effectively reduced; laser cladding treatment is used in the preparation of the laser cladding layer, which can effectively shorten the processing operation time and effectively avoid the situation where the high temperature is maintained for too long;

[0023] 2. In the process of preparing a high-strength, corrosion-resistant, high-pressure oil cylinder piston rod of the present invention, sodium chloride, boric acid, manganese sulfate, and nickel sulfate hexahydrate are added to deionized water for ultrasonic treatment, butyne glycol ethoxylate, saccharin, and sodium dodecyl sulfate are added for continued ultrasonic treatment, which can effectively ensure the uniformity of raw material distribution inside the plating solution, thereby ensuring the electroplating treatment effect; ultrasonic cleaning treatment of the piston rod substrate in deionized water can effectively remove impurities and dirt on the surface of the piston rod substrate, ensuring the bonding effect of the subsequent nickel-manganese plating layer and the surface of the piston rod substrate, and electroplating the piston rod in the plating solution A nickel-manganese coating can be formed on the surface of the piston rod substrate, and the piston rod with the nickel-manganese coating on the surface is annealed to obtain a piston rod with an annealed nickel-manganese coating, which can further enhance the hardness of the nickel-manganese coating. In the entire preparation method, electroplating is used in the preparation process of the nickel-manganese coating, and the operating temperature is low. There is no danger of excessively high operating temperature, and there is no need to operate for a long time under high temperature conditions, which can effectively reduce production costs. Laser cladding is used in the preparation of the laser cladding layer, which can effectively shorten the processing operation time and effectively avoid the situation where the high temperature is maintained for too long. DETAILED DESCRIPTION

[0024] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Embodiment 1:

[0026] The present invention provides a high-strength, corrosion-resistant, high-pressure oil cylinder piston rod, comprising a piston rod substrate, a nickel-manganese coating and a laser cladding layer, wherein the nickel-manganese coating is disposed on the surface of the piston rod substrate, and the laser cladding layer is disposed on the surface of the nickel-manganese coating;

[0027] The preparation method of the high-strength, corrosion-resistant, high-pressure oil cylinder piston rod comprises the following specific preparation steps:

[0028] Step 1: weighing butynediol ethoxylate, sodium chloride, boric acid, manganese sulfate, saccharin, sodium dodecyl sulfate, nickel sulfate hexahydrate in the raw materials for the nickel-manganese plating layer, and copper powder, chromium powder, and nickel powder in the raw materials for the laser cladding layer; the raw materials for the nickel-manganese plating layer include, by weight percentage, 0.054% butynediol ethoxylate, 5.81% sodium chloride, 13.60% boric acid, 2.30% manganese sulfate, 0.37% saccharin, 0.30% sodium dodecyl sulfate, and 77.566% nickel sulfate hexahydrate; the raw materials for the laser cladding layer include, by weight percentage, 4.9% copper powder, 14.8% chromium powder, and 80.3% nickel powder;

[0029] Step 2: adding the sodium chloride, boric acid, manganese sulfate and nickel sulfate hexahydrate in step 1 into deionized water, performing ultrasonic treatment for 15 minutes, then adding butynediol ethoxylate, saccharin and sodium dodecyl sulfate, and continuing ultrasonic treatment for 15 minutes to obtain a plating solution; the ultrasonic frequency is 1.4 MHz, the ultrasonic power is 400 W, and the weight ratio of nickel sulfate hexahydrate to deionized water is 1:5.0;

[0030] Step 3: ball-milling and blending the copper powder, chromium powder and nickel powder in step 1 for 30 minutes to obtain a mixed powder; using a planetary ball mill for ball milling, with an orbital speed of 360 r / min and a rotational speed of 720 r / min;

[0031] Step 4: Before placing the piston rod in the plating solution, first place the piston rod in deionized water for ultrasonic cleaning; place the piston rod substrate in the plating solution for electroplating to form a nickel-manganese coating on the surface of the piston rod substrate, and anneal the piston rod with the nickel-manganese coating on the surface to obtain a piston rod with an annealed nickel-manganese coating; the plating solution temperature is maintained at 33°C, the plating solution pH value is 3.8, and the current density is 1.5A / dm 2 , the electroplating time is 5.5h; the annealing temperature is 290℃;

[0032] Step 5: The mixed powder is subjected to laser cladding treatment by a laser, and a laser cladding layer is formed on the surface of the annealed nickel-manganese coating to obtain a high-strength, corrosion-resistant, high-pressure oil cylinder piston rod; a high-speed laser combined with coaxial powder feeding is used for laser cladding, with a laser power of 2100W, a defocus amount of 0, and a scanning rate of 500mm / min;

[0033] The thickness ratio of the nickel-manganese coating and the laser cladding layer is 1:1.

[0034] Embodiment 2:

[0035] Different from Example 1, the raw materials of the nickel-manganese plating layer include, by weight percentage, 0.064% of butine diol ethoxylate, 5.87% of sodium chloride, 13.64% of boric acid, 2.37% of manganese sulfate, 0.41% of saccharin, 0.33% of sodium dodecyl sulfate, and 77.316% of nickel sulfate hexahydrate; the raw materials of the laser cladding layer include, by weight percentage, 5.1% of copper powder, 15.2% of chromium powder, and 79.7% of nickel powder.

[0036] Embodiment 3:

[0037] Different from Examples 1-2, the raw materials of the nickel-manganese plating layer include, by weight percentage, 0.059% of butine diol ethoxylate, 5.84% of sodium chloride, 13.62% of boric acid, 2.34% of manganese sulfate, 0.39% of saccharin, 0.32% of sodium dodecyl sulfate, and 77.431% of nickel sulfate hexahydrate; the raw materials of the laser cladding layer include, by weight percentage, 5.0% of copper powder, 15.0% of chromium powder, and 80.0% of nickel powder.

[0038] Embodiment 4:

[0039] The difference from Example 3 is that in step 2, the ultrasonic frequency is 1.5 MHz, the ultrasonic power is 500 W, and the weight ratio of nickel sulfate hexahydrate to deionized water is 1:5.0; in step 3, a planetary ball mill is used for ball milling, the revolution speed is 420 r / min, and the rotation speed is 840 r / min; in step 4, the plating solution temperature is maintained at 36 ° C, the plating solution pH value = 4.0, and the current density is 1.6 A / dm 2 , the electroplating time is 6.0h; the annealing temperature is 300℃; in step five, a high-speed laser combined with coaxial powder feeding is used for laser cladding, the laser power is 2200W, the defocus is 0, and the scanning rate is 550mm / min.

[0040] Comparative Example 1:

[0041] Different from Example 4, the raw materials of the nickel-manganese plating layer include, by weight percentage, 5.84% sodium chloride, 13.62% boric acid, 2.34% manganese sulfate, 0.39% saccharin, 0.32% sodium dodecyl sulfate, and 77.49% nickel sulfate hexahydrate.

[0042] Comparative Example 2:

[0043] Different from Example 4, the raw materials of the nickel-manganese coating include, by weight percentage: the raw materials of the nickel-manganese coating include, by weight percentage: 0.0197% of butine diol ethoxylate, 5.84% of sodium chloride, 13.62% of boric acid, 2.34% of manganese sulfate, 0.39% of saccharin, 0.32% of sodium dodecyl sulfate, and 77.4703% of nickel sulfate hexahydrate.

[0044] Comparative Example 3:

[0045] Different from Example 4, the raw materials of the nickel-manganese plating layer include, by weight percentage, 0.0393% of butynediol ethoxylate, 5.84% of sodium chloride, 13.62% of boric acid, 2.34% of manganese sulfate, 0.39% of saccharin, 0.32% of sodium dodecyl sulfate, and 77.4507% of nickel sulfate hexahydrate.

[0046] In the above comparative examples and embodiments: butynediol ethoxylate was purchased from Wuhan Xinxinjiali Biotechnology Co., Ltd., brand: Xinxinjiali; sodium chloride was purchased from Qingdao Yufengda Fine Chemical Co., Ltd.; boric acid was purchased from Jinan Chuangshi Chemical Co., Ltd., item number: HG075; manganese sulfate was purchased from Wuhan Xinxinjiali Biotechnology Co., Ltd., brand: Xinxinjiali; saccharin was purchased from Shanghai Yuanye Biotechnology Co., Ltd., item number: B24318; sodium dodecyl sulfate was purchased from Wuhan Xinxinjiali Biotechnology Co., Ltd., brand: Xinxinjiali; nickel sulfate hexahydrate was purchased from Shandong Xinhe New Materials Co., Ltd., item number: 002; copper powder was purchased from Hebei Wenlun Metal Materials Co., Ltd., 200 mesh; chromium powder was purchased from Hebei Wenlun Metal Materials Co., Ltd., 200 mesh; nickel powder was purchased from Hebei Wenlun Metal Materials Co., Ltd., 200 mesh; the material of the piston rod base is 45# steel;

[0047] The nickel-manganese plating layer and the laser cladding layer of the piston rod of the high-strength, corrosion-resistant, high-pressure oil cylinder in the comparative example and the embodiment of the present invention were tested;

[0048] Hardness test: The hardness of the nickel-manganese coating and the laser cladding layer was tested using an HVS-1000A automatic turret micro-Vickers hardness tester. The indentation load was 100g, the test force holding time was 10s, and the average value of 5 test points was taken for each sample. The test results are shown in Tables 1 and 2.

[0049] Friction coefficient and wear test: The friction coefficient of the cladding layer surface was tested with a pin-on-disc friction and wear tester at room temperature, and the wear was measured with a balance. The test results are shown in Table 2.

[0050] Self-corrosion potential and self-corrosion current density detection: The surface of the cladding layer after immersion in isotonic solution for 3 hours was electrochemically tested using a three-electrode electrochemical workstation; the test results are shown in Table 2:

[0051] Table 1:

[0052]

[0053] Table 2:

[0054]

[0055] It can be seen from the above table that the high-strength, corrosion-resistant, high-pressure cylinder piston rod of the present invention has a nickel-manganese coating and a laser cladding layer on the surface of the piston rod, which can effectively improve the surface hardness of the piston rod, ensure the high-strength and high-pressure resistance of the piston rod, effectively improve the surface wear resistance of the piston rod, increase the self-corrosion potential of the piston rod surface, and reduce the self-corrosion current density on the piston rod surface, thereby effectively improving the corrosion resistance of the piston rod surface; in the preparation process of the nickel-manganese coating, electroplating treatment is adopted, the operating temperature is relatively low, there is no dangerous situation of excessively high operating temperature, and the production cost can be effectively reduced; laser cladding treatment is adopted in the preparation of the laser cladding layer, which can effectively shorten the processing operation time and effectively avoid the situation where the high temperature is maintained for too long.

[0056] In the preparation process of the nickel-manganese coating of the present invention, a butynediol ethoxy compound is added. Due to the carbon-carbon triple bond and complex functional group (ethoxy group) of the butynediol ethoxy compound, the butynediol ethoxy compound has a strong ability to gain or lose electrons and can be adsorbed on the surface of the coating in an approximately parallel manner. During the electroplating process, the butynediol ethoxy compound is stably adsorbed on the surface of the coating, which slows down the ion reduction rate and inhibits the electrodeposition process. The high coverage rate of the butynediol ethoxy compound on the cathode surface can effectively reduce the difference in the growth rate of the coating, thereby helping to obtain a flat surface structure. With the butynediol ethoxy compound The increase of the concentration of the substance causes the cathode polarization to shift negatively. The shift of the cathode polarization potential to a more negative direction will increase the nucleation rate of electrocrystallization and play a role in refining the grains. The adsorption of butynediol ethoxy compounds on the cathode surface is directly related to the adsorption of butynediol ethoxy compounds. The adsorption of butynediol ethoxy compounds can block the active growth sites on the surface of the coating. When the growth sites are blocked, the nucleation rate of electrocrystallization will be increased, resulting in grain refinement. The addition of butynediol ethoxy compounds significantly increases the microhardness of the coating. The hardness of the coating with the addition of butynediol ethoxy compounds is more affected by the annealing treatment. The butynediol ethoxy compounds in the plating solution are helpful in The formation of twins in the coating is conducive to the formation of more low-energy twin boundaries and dislocations. Low-temperature annealing leads to a decrease in the dislocation density inside the grains. To achieve the same strain, additional stress is required to activate new dislocations, which increases the difficulty of generating grain boundary dislocations and thus improves the microhardness. Butynediol ethoxylates can effectively level the Ni-Mn coating, increase the microhardness, and reduce the grain size. Under annealing treatment, the presence of butynediol ethoxylates in the plating solution can maintain a certain grain size of the coating and significantly enhance the annealing hardening ability of the coating. The addition of butynediol ethoxylates can The cathodic polarization potential shifts to a more negative direction, significantly inhibiting the cathodic reduction reaction of metal ions, refining the grains, and helping to obtain a flat, high-microhardness coating. By comparing the hardness and structure of the Ni-Mn coating after annealing at 300°C, it is found that the coating obtained from the plating solution containing butynediol ethoxylate has a smaller grain coarsening trend and more obvious annealing hardening. The highest scanning rate, although it cools faster during single-pass cladding and is more likely to form fine cellular crystals or equiaxed crystals, will be affected by heat again before the phase transformation of the newly clad structure grains during multi-pass cladding, allowing the grains near the overlap area to continue to grow. As the scanning rate decreases, the size of large grains will become larger and larger, but the number will not increase significantly.During the preparation process of the laser cladding layer, a laser cladding operation is adopted to produce a laser cladding layer on the surface of the nickel-manganese coating. Although the hardness of the laser cladding layer is lower than that of the nickel-manganese coating, it is significantly higher than the hardness of the piston rod substrate. Under the dual protection treatment of the nickel-manganese coating and the laser cladding layer, the high strength and high pressure resistance of the piston rod can be effectively improved; the friction coefficient and wear amount of the laser cladding layer are low, which can effectively ensure the wear resistance of the piston rod. The higher self-corrosion potential and lower self-corrosion current density on the surface of the laser cladding layer can effectively improve the corrosion resistance of the piston rod surface;.

[0057] In step 2, sodium chloride, boric acid, manganese sulfate, and nickel sulfate hexahydrate are added to deionized water for ultrasonic treatment, and then butynediol ethoxylate, saccharin, and sodium dodecyl sulfate are added to continue ultrasonic treatment, which can effectively ensure the uniformity of raw material distribution inside the plating solution, thereby ensuring the electroplating treatment effect; in step 3, copper powder, chromium powder, and nickel powder are ball-milled and blended, which can effectively ensure the uniformity of raw material mixing of the mixed powder, thereby ensuring the uniformity of internal structure distribution of the laser molten plating layer in subsequent laser cladding treatment; in step 4, the piston rod substrate is ultrasonically cleaned in deionized water, which can effectively remove impurities and dirt on the surface of the piston rod substrate, ensure the bonding effect of the subsequent nickel-manganese plating layer and the surface of the piston rod substrate, and the piston rod is placed in the plating solution. Electroplating treatment is performed to form a nickel-manganese coating on the surface of the piston rod substrate, and the piston rod with the nickel-manganese coating on the surface is annealed to obtain a piston rod with an annealed nickel-manganese coating, which can further enhance the hardness of the nickel-manganese coating; in step five, a laser cladding layer is formed on the surface of the annealed nickel-manganese coating using the mixed powder to obtain a high-strength, corrosion-resistant, high-pressure cylinder piston rod; in the entire preparation method, electroplating treatment is used in the preparation process of the nickel-manganese coating, and the operating temperature is relatively low, there is no dangerous situation of excessively high operating temperature, and there is no need to operate for a long time under high temperature conditions, which can effectively reduce production costs; laser cladding treatment is used in the preparation of the laser cladding layer, which can effectively shorten the processing operation time and effectively avoid the situation where the high temperature is maintained for too long.

[0058] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A high-strength, corrosion-resistant, high-pressure cylinder piston rod, characterized in that: The invention comprises a piston rod substrate, a nickel-manganese coating and a laser cladding layer. The nickel-manganese coating is arranged on the surface of the piston rod substrate, and the laser cladding layer is arranged on the surface of the nickel-manganese coating.

2. The high-strength, corrosion-resistant, high-pressure oil cylinder piston rod according to claim 1, characterized in that: The raw materials of the nickel-manganese plating layer include, by weight percentage, 0.054-0.064% of butynediol ethoxylate, 5.81-5.87% of sodium chloride, 13.60-13.64% of boric acid, 2.30-2.37% of manganese sulfate, 0.37-0.41% of saccharin, 0.30-0.33% of sodium dodecyl sulfate, and the rest is nickel sulfate hexahydrate.

3. The high-strength, corrosion-resistant, high-pressure oil cylinder piston rod according to claim 2, characterized in that: The raw materials of the laser cladding layer include, by weight percentage, 4.9-5.1% copper powder, 14.8-15.2% chromium powder, and the rest nickel powder.

4. The high-strength, corrosion-resistant, high-pressure oil cylinder piston rod according to claim 3, characterized in that: The raw materials of the nickel-manganese plating layer include, by weight percentage, 0.058-0.060% of butynediol ethoxylate, 5.83-5.85% of sodium chloride, 13.61-13.63% of boric acid, 2.32-2.35% of manganese sulfate, 0.38-0.40% of saccharin, 0.31-0.32% of sodium dodecyl sulfate, and the rest is nickel sulfate hexahydrate; the raw materials of the laser cladding layer include, by weight percentage, 4.95-5.05% of copper powder, 14.9-15.1% of chromium powder, and the rest is nickel powder.

5. The high-strength, corrosion-resistant, high-pressure oil cylinder piston rod according to claim 3, characterized in that: The raw materials of the nickel-manganese plating layer include, by weight percentage, 0.059% of butynediol ethoxylate, 5.84% of sodium chloride, 13.62% of boric acid, 2.34% of manganese sulfate, 0.39% of saccharin, 0.32% of sodium dodecyl sulfate, and the rest is nickel sulfate hexahydrate; the raw materials of the laser cladding layer include, by weight percentage, 5.0% of copper powder, 15.0% of chromium powder, and the rest is nickel powder.

6. The high-strength, corrosion-resistant, high-pressure oil cylinder piston rod according to claim 1, characterized in that: The thickness ratio of the nickel-manganese plating layer to the laser cladding layer is 1:

1.

7. A method for preparing a high-strength, corrosion-resistant, high-pressure oil cylinder piston rod, characterized in that: The specific preparation steps are as follows: Step 1: Weigh butynediol ethoxylate, sodium chloride, boric acid, manganese sulfate, saccharin, sodium dodecyl sulfate, nickel sulfate hexahydrate in the raw materials for nickel-manganese plating, and copper powder, chromium powder, and nickel powder in the raw materials for laser cladding layer; Step 2: adding the sodium chloride, boric acid, manganese sulfate and nickel sulfate hexahydrate in step 1 into deionized water, performing ultrasonic treatment for 10 to 20 minutes, then adding butynediol ethoxylate, saccharin and sodium dodecyl sulfate, and continuing ultrasonic treatment for 10 to 20 minutes to obtain a plating solution; Step 3: ball milling the copper powder, chromium powder and nickel powder in step 1 for 20 to 40 minutes to obtain a mixed powder; Step 4: placing the piston rod substrate into a plating solution for electroplating to form a nickel-manganese coating on the surface of the piston rod substrate, and annealing the piston rod with the nickel-manganese coating to obtain a piston rod with an annealed nickel-manganese coating; Step 5: The mixed powder is subjected to laser cladding treatment by a laser, and a laser cladding layer is produced on the surface of the annealed nickel-manganese coating to obtain a high-strength, corrosion-resistant, high-pressure cylinder piston rod.

8. The method for preparing a high-strength, corrosion-resistant, high-pressure oil cylinder piston rod according to claim 7, characterized in that: In step 2, the ultrasonic frequency is 1.4-1.6 MHz, the ultrasonic power is 400-600 W, and the weight ratio of nickel sulfate hexahydrate to deionized water is 1:4.9-5.1; in step 3, a planetary ball mill is used for ball milling, the orbital speed is 360-480 r / min, and the rotation speed is 720-960 r / min.

9. The method for preparing a high-strength, corrosion-resistant, high-pressure oil cylinder piston rod according to claim 8, characterized in that: Before placing the piston rod in the plating solution, the piston rod is first placed in deionized water for ultrasonic cleaning; in step 4, the plating solution temperature is maintained at 33-39°C, the plating solution pH value is 3.8-4.2, and the current density is 1.5-1.7A / dm 2 , the electroplating time is 5.5-6.5h; the annealing temperature is 290-310°C; in step five, a high-speed laser combined with coaxial powder feeding is used for laser cladding, the laser power is 2100-2300W, the defocus is 0, and the scanning rate is 500-600mm / min.

10. The method for preparing a high-strength, corrosion-resistant, high-pressure oil cylinder piston rod according to claim 9, characterized in that: In step 2, the ultrasonic frequency is 1.5 MHz, the ultrasonic power is 500 W, and the weight ratio of nickel sulfate hexahydrate to deionized water is 1:5.0; in step 3, a planetary ball mill is used for ball milling, the revolution speed is 420 r / min, and the rotation speed is 840 r / min; in step 4, the plating solution temperature is maintained at 36°C, the plating solution pH value is 4.0, and the current density is 1.6 A / dm 2 , the electroplating time is 6.0h; the annealing temperature is 300℃; in step five, a high-speed laser combined with coaxial powder feeding is used for laser cladding, the laser power is 2200W, the defocus is 0, and the scanning rate is 550mm / min.

Citation Information

Patent Citations

  • Surface treatment method for high-strength and corrosion-resistant precision piston rods

    CN113249680B

Cited By

  • A heterogeneous metal deposition method for a molten salt reactor using a hybrid DED process

    KR103051040B1