Polypropylene composition fiber and application

By using silicon carbide whiskers modified with silane coupling agents in polypropylene composite materials, the wear resistance and cut resistance of the fibers are improved, and the problems of insufficient wear resistance and cut resistance of polypropylene composite materials are solved and expanded Its application scope in the field of labor protection supplies has been expanded.

CN118814293APending Publication Date: 2024-10-22HUIHONG NANTONG SAFETY PRODS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410988610.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

It is difficult to effectively control the wear resistance and cutting resistance of existing polypropylene composite materials, which limits their application scope in the field of labor protection supplies.

Method used

Using a combination of silicon carbide whiskers modified with silane coupling agents and homopolypropylene, a polypropylene combination with excellent wear resistance and cutting resistance was prepared by heating the blended spinning materials and performing spinning, heat drawing and shaping. Material fiber.

Benefits of technology

The strength, draft modulus, wear resistance and cutting resistance of the polypropylene composite fiber are significantly improved, and the service life is extended, making it more suitable for use in the field of labor protection products.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and particularly relates to a polypropylene composition fiber and application thereof.The fiber is prepared from a polypropylene composition, the polypropylene composition comprises homo-polypropylene and modified silicon carbide whiskers with the homo-polypropylene content being 0.5-5 wt%, and the modified silicon carbide whiskers are modified silicon carbide whiskers with the homo-polypropylene content being 0.5-5 wt%. The modified silicon carbide whisker is a silicon carbide whisker modified by a silane coupling agent, and the silicon carbide whisker modified by the silane coupling agent is prepared from a silicon carbide whisker and a silane coupling agent. The polypropylene composition fiber disclosed by the invention has excellent wear resistance and cutting resistance, and the service life of the polypropylene composition fiber is effectively prolonged, so that the polypropylene composition fiber is more easily applied to the field of labor protection appliances, and the application range of the polypropylene composition fiber in the field of labor protection appliances is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a polypropylene composite fiber and application thereof. Background Art

[0002] Polymer materials are materials based on polymer compounds, and are also materials composed of compounds with relatively high molecular weight, including rubber, plastics, fibers, coatings, adhesives and polymer-based composite materials. Polypropylene is a thermoplastic resin (thermoplastic plastic) made by polymerization of propylene. It is relatively stable to water, with a water absorption rate of only 0.01% in water, a molecular weight of about 80,000 to 150,000, and good formability. However, due to the large shrinkage rate (1 to 2.5%), thick-walled products are prone to dents. For some parts with high dimensional accuracy, it is difficult to meet their technical requirements. The surface gloss of the product is good. At present, composite materials made of polypropylene as raw material and adding a certain proportion of auxiliary materials have the advantages of light weight, good coverage, high toughness, good chemical resistance, antimicrobial resistance and low price. They are widely used in ropes, fishing nets, textiles and clothing and other industries, but the mechanical properties of composite materials are still relatively poor and cannot meet the needs of practical applications.

[0003] There are studies on the mechanical performance problems of composite materials in the prior art, such as patent application CN106380694A-Carbon fiber reinforced polypropylene composite material and preparation method thereof, CN105061892A-A fiber reinforced polypropylene material and application of its pipeline, etc., which improve the mechanical properties of composite materials by adding fibers, whiskers or powdered inorganic particles as reinforcements, solving the problem that the current composite materials cannot meet the actual application requirements due to relatively poor mechanical properties. However, although the existing polypropylene composite materials guarantee the performance of tensile strength, tensile modulus and linear density, it is difficult to effectively control the wear resistance and cutting resistance of polypropylene composite materials, which affects the service life of polypropylene composite materials, thereby limiting the application scope of polypropylene composite materials in the field of labor protection products. Therefore, a new technical solution is needed to solve the above technical problems. Summary of the invention

[0004] The object of the present invention is to provide a polypropylene composite fiber and its application, so as to solve the problem mentioned in the above background technology that it is difficult to effectively control the wear resistance and cut resistance of the current polypropylene composite materials, which affects the service life of the polypropylene composite materials, thereby limiting the application scope of the polypropylene composite materials in the field of labor protection products.

[0005] To achieve the above object, the present invention provides the following technical solution: a polypropylene composition fiber, the fiber is prepared from a polypropylene composition, the raw material components of the polypropylene composition include homopolypropylene with a viscosity average molecular weight of 100,000 to 300,000 and modified silicon carbide whiskers containing 0.5 to 5 wt% of homopolypropylene, the modified silicon carbide whiskers are silicon carbide whiskers modified by a silane coupling agent, and the silicon carbide whiskers modified by a silane coupling agent are prepared from silicon carbide whiskers and a silane coupling agent.

[0006] Furthermore, the specific preparation steps of the silane coupling agent modified silicon carbide whisker are: ultrasonically dispersing the silicon carbide whisker in a solvent for 20 to 40 minutes, adding a silane coupling agent, stirring at 60 to 80° C. for 2 to 6 hours, and drying to obtain the silane coupling agent modified silicon carbide whisker, wherein the solvent is a mixture of one or more of water, methanol, ethyl acetate, acetone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, tetrahydrofuran, and dimethyl sulfoxide, the weight ratio of the silicon carbide whisker to the silane coupling agent is 1:0.1 to 0.5, the silicon carbide whisker is a β crystal and its diameter and length are 100 to 600 nm and 3 to 20 μm, respectively, the silane coupling agent is a mixture of one or two of an alkyl silane coupling agent and an amino silane coupling agent, and the weight ratio of the alkyl silane coupling agent to the amino silane coupling agent is 2:3 to 3:2.

[0007] Furthermore, the specific preparation steps of the fiber are: firstly, the polypropylene composition is heated in a mixer to obtain a blended spinning material, and then the blended spinning material is spun, heat-drawn and shaped to obtain the polypropylene composition fiber.

[0008] In addition to the above technical solutions, the above polypropylene composition fibers are also used to prepare cut-resistant fabrics, including gloves, clothing, cloth, etc.

[0009] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention adopts silicon carbide whiskers modified by silane coupling agent, which can not only weaken the interaction between silicon carbide whiskers, effectively avoid whisker agglomeration, and improve the dispersibility of silicon carbide in polypropylene, but also enable the silicon carbide whiskers dispersed in polypropylene to absorb energy transmitted from the outside, increase its tensile strength and tensile modulus, and effectively improve the strength and safety performance of polypropylene composite fiber. By dispersing and modifying silicon carbide whiskers in polypropylene, the polypropylene composite fiber has excellent wear resistance and cutting resistance, and effectively prolongs the service life of the polypropylene composite fiber, so that the polypropylene composite fiber is more easily applied to the field of labor protection products, and the application scope of the polypropylene composite fiber in the field of labor protection products is guaranteed; 2. The present invention regulates silicon carbide whiskers so that the polypropylene composition can more easily form uniform and regular fibrous crystal nuclei under the premise of having good dispersibility, and the fibrous crystal nuclei can effectively promote the chain segments to grow into an orderly arranged crystal structure along their orientation on their surface, so that the polypropylene composition fiber can not only improve its tensile strength and tensile modulus, but also help to improve its wear resistance and cutting resistance; 3. The present invention adds a silane coupling agent to the silicon carbide whisker, so that the silicon carbide can be coated by the silane coupling agent, effectively avoiding direct contact between the silicon carbide and the human body, so that the polypropylene composite fiber improves the product performance while ensuring its safety and no toxic side effects; 4. The cut-resistant fabric prepared by the polypropylene composition fiber of the present invention also has excellent wear resistance and cut resistance, thereby greatly improving the service life of the fabric and ensuring the use scope of the fabric in the field of labor protection products. DETAILED DESCRIPTION

[0010] The following examples are used to further illustrate the content of the present invention, but do not limit the application of the present invention. The raw materials used are all commercially available products.

[0011] The invention provides a polypropylene composite fiber, which is prepared from a polypropylene composite. The polypropylene composite comprises a raw material component of homopolypropylene with a viscosity average molecular weight of 100,000 to 300,000 and a modified silicon carbide whisker containing 0.5 to 5 wt% (wt% is the weight content percentage) of homopolypropylene, and the modified silicon carbide whisker is a silicon carbide whisker modified by a silane coupling agent and is prepared from silicon carbide whiskers and a silane coupling agent.

[0012] The silicon carbide (SiC) in the silicon carbide whisker of the present invention is a binary compound of Group IV-IV, the only and extremely stable compound among Group IV elements, and is mainly composed of carbon atoms and silicon atoms bonded by covalent bonds, and has a hexahedral crystal structure similar to diamond. The SiC crystal structure is composed of two densely arranged sublattices, namely, a Si atom sublattice and a C atom sublattice, and the displacement of the latter along the main symmetry axis is one quarter of the distance between two adjacent layers of Si atoms. The silicon carbide group is centered on a carbon atom and four Si atoms are connected by covalent bonds. Since the Si atom is shared with adjacent groups, that is, one Si atom belongs to four such groups at the same time, the chemical formula composed of the simplest atomic ratio of each group being 1:1 is SiC. The minimum distance between Si atoms and C atoms is 0.189nm. Each Si (or C) atom is surrounded by four C (or Si) atoms and bonded together by directional strong tetrahedral sp3 bonds. This structure determines the good chemical and thermal stability of SiC, as well as its wide bandgap, excellent corrosion resistance, excellent mechanical properties and heat transfer properties. Silicon carbide is a hard material with a Mohs hardness of 9.2 to 9.5. The typical structure of SiC can be divided into two categories: one is the cubic SiC crystal type with zinc blende structure, collectively referred to as β-SiC; the other is the large periodic structure of hexagonal or rhombus structure, typically 6H, 4H, and R, collectively referred to as α-SiC. Silicon carbide powder includes hexagonal or rhombohedral α-SiC and cubic β-SiC and β-SiC whiskers. Silicon carbide powder and plastic, metal, ceramic composite materials can significantly improve their various properties. Due to its high thermal stability, high strength, high thermal conductivity and other characteristics, it is widely used in atomic energy materials, chemical devices, high temperature processing, electrical and electronic materials, semiconductor fields, electric heating components and resistors, etc. It can also be used for abrasives, grinding tools, advanced refractory materials, fine ceramics; the crystal phase of SiC powder is that the raw materials SiO2 and C are continuously precipitated through gas-liquid-solid at high temperature. SiC crystal nuclei are superimposed, and finally they grow along the ab axis of the SiC six-section ring plane perpendicular to the c axis to form a hexagonal crystal system. According to the reaction conditions, SiC nanowires, rods or nanosheets can be formed; The preparation methods of silicon carbide nanopowders can be mainly divided into three categories: solid phase method, liquid phase method and gas phase method. The carbon thermal reduction method is to use the mixed powder of SiO2 and Si powder to release SiO gas under high temperature, and react with activated carbon to produce β-SiC; the mechanical alloying method is to mix Si powder and C powder according to n(Si):n(C)=1:1, and encapsulate the grinding balls and grinding powder in a grinding tank filled with hydrogen at a ball-powder mass ratio of 40:1, and perform mechanical ball milling on a WL-1 planetary ball mill. After grinding for 25 hours, SiC powder with an average grain size of about 6nm was obtained; Sol-gel method: tetraethoxysilane and methyltriethoxysilane were used as silicon sources, phenolic resin, starch, etc. were used as carbon sources, and the formed gel was carbonized at 800℃ in nitrogen to obtain SiC precursor, and then heated at 1550℃ in hydrogen to obtain 5-20nm SiC; Polymer thermal decomposition method: Low molecular weight polycarbosilane (LPS) was used as raw material, and SiC ultrafine powder was prepared by gas phase thermal cracking process; To sum up, the silicon carbide whiskers of the present invention are cubic whiskers and belong to the same crystal form as diamond. They are the whisker products with the highest hardness, the largest modulus, the largest tensile strength, and the highest heat resistance temperature among the whiskers synthesized so far. They are divided into two forms, α-type and β-type. Among them, the β-type has better performance than the α-type and has higher hardness (Mohs hardness of 9.5 or above), better toughness and conductivity. Therefore, in this embodiment, β-type silicon carbide whiskers are selected (the silicon carbide whiskers purchased are SiCW-80 products or SiCW-90 products produced by Qinhuangdao Yinuo High-tech Materials Development Co., Ltd.).

[0013] The silane coupling agent of the present invention is a type of organic silicon compound that contains two groups of different chemical properties in the molecule at the same time. Common silane coupling agents are hydrolyzable Y-functional silane coupling agents, and their general structural formula is Y-CH2SiRnX(3-n), wherein X is a hydrolyzable organic functional group, such as chloro, acetoxy, methoxy and ethoxy. X is easily hydrolyzed, and the resulting silanol groups are easily bonded to the hydroxyl groups on the surface of inorganic substances. Y is a non-hydrolyzable, reactive organic functional group that can react with organic matter, or an inert organic functional group that does not react with organic matter, such as hexenyl, epoxy, amino, thiol, thiocyanate, phenyl or long-chain alkyl. Therefore, the silane coupling agent of this embodiment is selected from one or a mixture of alkyl silane coupling agents and amino silane coupling agents, and the weight ratio of the mixture is 2:3 to 3:2; The general formula of the alkylsilane coupling agent is: Y-CH2SinX(3-n), Y is an alkyl group, and examples thereof include: 1,2-bis(triethoxysilyl)ethane, 1,2-bis(trimethoxysilyl)ethane, methyltriethoxysilane, methyltrimethoxysilane, propyltriethoxysilane, propyltrimethoxysilane, octyltriethoxysilane, octyltrimethoxysilane, dodecyltriethoxysilane, dodecyltrimethoxysilane, hexadecyltrimethoxysilane, octadecyltrimethoxysilane, dimethyldiethoxysilane, dimethyldimethoxysilane, isooctyltriethoxysilane, methyltriacetoxysilane, methyltributylidene oxime silane, etc.; The general formula of aminosilane coupling agent is: Y-CH2SinX(3-n), Y is amino, and examples thereof include: γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β(aminoethyl)-γ-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, γ-aminopropylmethyldiethyl Oxysilane, 3-aminopropylmethyldimethoxysilane, N-n-butyl-3-aminopropyltrimethoxysilane, 3-ureapropyltrimethoxysilane, bis-[3-(triethoxysilyl)-propyl]-amine, 3-anilinopropyltrimethoxysilane, diethylenetriaminepropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, 3-ureapropyltriethoxysilane, bis-[3-(trimethoxysilyl)-propyl]-amine, etc.; In summary, the silane coupling agent of the present invention can be a mixture of dodecylsilane coupling agent (the dodecylsilane coupling agent purchased is UP-312 product or UP-313 product produced by Nanjing Youpu Chemical Co., Ltd.) and 3-aminopropyltrimethoxysilane (the 3-aminopropyltrimethoxysilane purchased is KH-540 product produced by Qingdao Hengda Zhongcheng Technology Co., Ltd.).

[0014] The silicon carbide whisker modified by a silane coupling agent is prepared by functional group coupling, that is, the silicon carbide whisker is ultrasonically dispersed in a solvent (the solvent is one or a mixture of water, methanol, ethyl acetate, acetone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, tetrahydrofuran and dimethyl sulfoxide) for 20 to 40 minutes, and then a silane coupling agent is added, the temperature is controlled at 60 to 80° C., and after stirring for 2 to 6 hours, the silicon carbide whisker modified by a silane coupling agent is dried to obtain the silicon carbide whisker, wherein the weight ratio of the silicon carbide whisker to the silane coupling agent is 1:0.1 to 0.5.

[0015] Since nano silicon carbide is used to improve the cutting resistance of polypropylene composite fibers, but nano silicon carbide is easy to agglomerate during the mixing and heating process with polypropylene, resulting in poor dispersibility, the present invention uses silicon carbide whiskers modified by a silane coupling agent; and since the surface of nano silicon carbide is easy to react with water in the air and has hydroxyl groups, it participates in the hydrolysis of the silane coupling agent during the above reaction process and is combined together through chemical bonds to obtain a modified silicon carbide material. On the one hand, after modification, the force between silicon carbide whiskers can be weakened to avoid whisker agglomeration, thereby improving the dispersibility of silicon carbide in polypropylene; on the other hand, the silicon carbide whiskers dispersed in polypropylene can absorb energy transmitted from the outside, increase the tensile strength and tensile modulus, and improve the strength, cutting resistance and safety performance of polypropylene fibers; During the preparation of the polypropylene composition, by regulating the silicon carbide whiskers, when the diameter of the silicon carbide whiskers is 100-600nm and the length is 3-20µm, the strength and cut resistance of the polypropylene composition fiber can be further improved. The study found that under the premise of good dispersibility, nano-silicon carbide of a certain diameter and length is easier to form uniform and regular fibrous crystal nuclei during the stretching and heat setting of the polypropylene composition fiber, and the fibrous crystal nucleus can effectively promote the chain segments along its orientation and grow into an orderly arranged crystal structure on its surface, so that the polypropylene composition can not only improve the tensile strength and tensile modulus of the fiber, but also help to improve the wear resistance and cut resistance of the fiber.

[0016] The polypropylene composite fiber of the present invention is prepared by dispersing the silicon carbide whiskers modified by the silane coupling agent prepared above on the surface of homopolypropylene by means of heating and blending to obtain a blended spinning material, and then spinning the blended spinning material by means of melt spinning at 230-270° C., heat drawing and heat setting to obtain a composite fiber (i.e., a polypropylene composite fiber); The manufacturing methods of polypropylene composite fibers can be divided into two categories according to the physical state of the raw materials used: chip spinning (indirect spinning) and direct spinning; according to the spinning speed, it can be divided into conventional spinning and high-speed spinning; according to the fiber type, it can be divided into filament spinning and short fiber spinning; The production of polypropylene composite fibers goes through three processes: preparation of spinning solution - spinning - post-processing, wherein the preparation of spinning solution is to heat polypropylene above the melting point to melt it into a relatively stable viscous fluid; spinning is to eject the molten polypropylene viscous fluid from the fine holes of the spinneret and cool and solidify into filaments in the surrounding air (or water); post-processing is the stretching, shaping or fibrillation process to give the fiber specific physical properties. Embodiment 1:

[0017] This embodiment provides a cut-resistant and abrasion-resistant polypropylene composition fiber, which is prepared from a polypropylene composition; The polypropylene composition includes modified silicon carbide whiskers with a content of 0.5wt% homopolypropylene and homopolypropylene with a viscosity average molecular weight of 200,000 (the homopolypropylene purchased is a product produced by Hengli Petrochemical), the content of the modified silicon carbide whiskers is 0.5wt% of homopolypropylene, and the modified silicon carbide whiskers are silicon carbide whiskers modified by a silane coupling agent; The preparation method of silicon carbide whiskers modified by silane coupling agent comprises: firstly dispersing silicon carbide whiskers in deionized water by ultrasonic method for 30 minutes, then adding silane coupling agent, controlling the temperature at 70°C, stirring for 5 hours, and drying to obtain silicon carbide whiskers modified by silane coupling agent; The weight ratio of silicon carbide whiskers to silane coupling agent in the silicon carbide whiskers modified by silane coupling agent is 1:0.1; the silane coupling agent is a mixture of dodecylsilane coupling agent and 3-aminopropyltrimethoxysilane, and the weight ratio of dodecylsilane coupling agent (the dodecylsilane coupling agent is UP-312 produced by Nanjing Youpu Chemical Co., Ltd.) and 3-aminopropyltrimethoxysilane (the 3-aminopropyltrimethoxysilane is KH-540 produced by Qingdao Hengda Zhongcheng Technology Co., Ltd.) is 2:3; the diameter of silicon carbide whiskers (the silicon carbide whiskers are SiCW-80 produced by Qinhuangdao Yinuo High-tech Materials Development Co., Ltd.) is 200-500nm, the length is 3-20μm, and it is β-type; The silicon carbide whiskers modified by the silane coupling agent prepared above are dispersed on the surface of homopolypropylene by means of heating and blending to obtain a blended spinning material; the blended spinning material is then melt-spinned at 230° C., heat-drawn and heat-set to obtain a composite fiber (i.e., a polypropylene composite fiber); The polypropylene composition fiber prepared as above is woven into a cut-resistant fabric through a textile process. The fabric includes gloves, clothing, cloth, etc. The fabric is tested according to EN388-2016, and its cut-resistant grade is A and the abrasion resistance is 3000 turns. Embodiment 2:

[0018] This embodiment provides a cut-resistant and abrasion-resistant polypropylene composition fiber, which is prepared from a polypropylene composition; The polypropylene composition includes modified silicon carbide whiskers with a content of 5wt% homopolypropylene and homopolypropylene with a viscosity average molecular weight of 250,000 (the homopolypropylene purchased is a product produced by Hengli Petrochemical), the content of the modified silicon carbide whiskers is 5wt% of the homopolypropylene, and the modified silicon carbide whiskers are silicon carbide whiskers modified by a silane coupling agent; The preparation method of silicon carbide whiskers modified by silane coupling agent comprises: firstly dispersing silicon carbide whiskers in deionized water by ultrasonic method for 30 minutes, then adding silane coupling agent, controlling the temperature at 70°C, stirring for 5 hours, and drying to obtain silicon carbide whiskers modified by silane coupling agent; The weight ratio of silicon carbide whiskers to silane coupling agents in the silicon carbide whiskers modified by silane coupling agents is 1:0.5; the silane coupling agent is a mixture of dodecylsilane coupling agent and 3-aminopropyltrimethoxysilane, and the weight ratio of dodecylsilane coupling agent (the dodecylsilane coupling agent is UP-313 produced by Nanjing Youpu Chemical Co., Ltd.) and 3-aminopropyltrimethoxysilane (the 3-aminopropyltrimethoxysilane is KH-540 produced by Qingdao Hengda Zhongcheng Technology Co., Ltd.) is 3:2; the diameter of silicon carbide whiskers (the silicon carbide whiskers are SiCW-80 produced by Qinhuangdao Yinuo High-tech Materials Development Co., Ltd.) is 200-500nm, the length is 3-20μm, and it is β-type; The silicon carbide whiskers modified by the silane coupling agent prepared above are dispersed on the surface of homopolypropylene by heating and blending to obtain a blended spinning material; the blended spinning material is then melt-spinned at 260° C., heat-drawn and heat-set to obtain a composite fiber (i.e., a polypropylene composite fiber); The polypropylene composition fiber prepared as above is woven into a cut-resistant fabric through a textile process. The fabric includes gloves, clothing, cloth, etc. The fabric is tested according to EN388-2016, and its cut-resistant grade is B and the abrasion resistance is 8000 revolutions. Embodiment 3:

[0019] This embodiment provides a cut-resistant and abrasion-resistant polypropylene composition fiber, which is prepared from a polypropylene composition; The polypropylene composition includes modified silicon carbide whiskers with a content of 3wt% homopolypropylene and homopolypropylene with a viscosity average molecular weight of 300,000 (the homopolypropylene purchased is a product produced by Hengli Petrochemical), the content of the modified silicon carbide whiskers is 3wt% of the homopolypropylene, and the modified silicon carbide whiskers are silicon carbide whiskers modified by a silane coupling agent; The preparation method of silicon carbide whiskers modified by silane coupling agent comprises: firstly dispersing silicon carbide whiskers in deionized water by ultrasonic method for 30 minutes, then adding silane coupling agent, controlling the temperature at 70°C, stirring for 5 hours, and drying to obtain silicon carbide whiskers modified by silane coupling agent; The weight ratio of silicon carbide whiskers to silane coupling agents in the silicon carbide whiskers modified by silane coupling agents is 1:0.2; the silane coupling agent is a mixture of dodecylsilane coupling agent and 3-aminopropyltrimethoxysilane, and the weight ratio of dodecylsilane coupling agent (the dodecylsilane coupling agent is UP-312 produced by Nanjing Youpu Chemical Co., Ltd.) and 3-aminopropyltrimethoxysilane (the 3-aminopropyltrimethoxysilane is KH-540 produced by Qingdao Hengda Zhongcheng Technology Co., Ltd.) is 1:1; the diameter of silicon carbide whiskers (the silicon carbide whiskers are SiCW-90 produced by Qinhuangdao Yinuo High-tech Materials Development Co., Ltd.) is 100-600nm, the length is 3-20μm, and it is β-type; The silicon carbide whiskers modified by the silane coupling agent prepared above are dispersed on the surface of homopolypropylene by heating and blending to obtain a blended spinning material; the blended spinning material is then melt-spinned at 270° C., heat-drawn and heat-set to obtain a composite fiber (i.e., a polypropylene composite fiber); The polypropylene composition fiber prepared as above is woven into a cut-resistant fabric through a textile process. The fabric includes gloves, clothing, cloth, etc. The fabric is tested according to EN388-2016, and its cut-resistant grade is B and the abrasion resistance is 6000 revolutions. Embodiment 4:

[0020] This embodiment provides a cut-resistant and abrasion-resistant polypropylene composition fiber, which is prepared from a polypropylene composition; The polypropylene composition includes modified silicon carbide whiskers with a content of 4wt% homopolypropylene and homopolypropylene with a viscosity average molecular weight of 250,000 (the homopolypropylene purchased is a product produced by Hengli Petrochemical), the content of the modified silicon carbide whiskers is 4wt% of the homopolypropylene, and the modified silicon carbide whiskers are silicon carbide whiskers modified by a silane coupling agent; The preparation method of silicon carbide whiskers modified by silane coupling agent comprises: firstly dispersing silicon carbide whiskers in deionized water by ultrasonic method for 30 minutes, then adding silane coupling agent, controlling the temperature at 70°C, stirring for 5 hours, and drying to obtain silicon carbide whiskers modified by silane coupling agent; Among them, the weight ratio of silicon carbide whiskers and silane coupling agent in the silicon carbide whiskers modified by silane coupling agent is 1:0.4; the silane coupling agent is a mixture of dodecylsilane coupling agent and 3-aminopropyltrimethoxysilane, and the weight ratio of dodecylsilane coupling agent (the dodecylsilane coupling agent purchased is UP-312 product produced by Nanjing Youpu Chemical Co., Ltd.) and 3-aminopropyltrimethoxysilane (3-aminopropyltrimethoxysilane purchased is KH-540 product produced by Qingdao Hengda Zhongcheng Technology Co., Ltd.) is 1:1.2; the diameter of silicon carbide whiskers (the silicon carbide whiskers purchased are SiCW-90 products produced by Qinhuangdao Yinuo High-tech Materials Development Co., Ltd.) is 100-600nm, the length is 3-20μm, and it is β-type; The silicon carbide whiskers modified by the silane coupling agent prepared above are dispersed on the surface of homopolypropylene by heating and blending to obtain a blended spinning material; the blended spinning material is then melt-spinned at 270° C., heat-drawn and heat-set to obtain a composite fiber (i.e., a polypropylene composite fiber); The polypropylene composition fiber prepared as above is woven into a cut-resistant fabric through a textile process. The fabric includes gloves, clothing, cloth, etc. The fabric is tested according to EN388-2016, and its cut-resistant grade is B and the abrasion resistance is 6500 revolutions. Embodiment 5:

[0021] This embodiment provides a cut-resistant and abrasion-resistant polypropylene composition fiber, which is prepared from a polypropylene composition; The polypropylene composition includes modified silicon carbide whiskers with a content of 2wt% homopolypropylene and homopolypropylene with a viscosity average molecular weight of 250,000 (the homopolypropylene purchased is a product produced by Hengli Petrochemical), the content of the modified silicon carbide whiskers is 2wt% of the homopolypropylene, and the modified silicon carbide whiskers are silicon carbide whiskers modified by a silane coupling agent; The preparation method of silicon carbide whiskers modified by silane coupling agent comprises: firstly dispersing silicon carbide whiskers in deionized water by ultrasonic method for 30 minutes, then adding silane coupling agent, controlling the temperature at 70°C, stirring for 5 hours, and drying to obtain silicon carbide whiskers modified by silane coupling agent; Among them, the weight ratio of silicon carbide whiskers and silane coupling agent in the silicon carbide whiskers modified by silane coupling agent is 1:0.3; the silane coupling agent is a mixture of dodecylsilane coupling agent and 3-aminopropyltrimethoxysilane, and the weight ratio of dodecylsilane coupling agent (the dodecylsilane coupling agent purchased is UP-312 product produced by Nanjing Youpu Chemical Co., Ltd.) and 3-aminopropyltrimethoxysilane (3-aminopropyltrimethoxysilane purchased is KH-540 product produced by Qingdao Hengda Zhongcheng Technology Co., Ltd.) is 1:1.6; the diameter of silicon carbide whiskers (the silicon carbide whiskers purchased are SiCW-80 products produced by Qinhuangdao Yinuo High-tech Materials Development Co., Ltd.) is 200-500nm, the length is 3-20μm, and it is β-type; The silicon carbide whiskers modified by the silane coupling agent prepared above are dispersed on the surface of homopolypropylene by heating and blending to obtain a blended spinning material; the blended spinning material is then melt-spinned at 270° C., heat-drawn and heat-set to obtain a composite fiber (i.e., a polypropylene composite fiber); The polypropylene composition fiber prepared as above is woven into a cut-resistant fabric through a textile process. The fabric includes gloves, clothing, cloth, etc. The fabric is tested according to EN388-2016, and its cut-resistant grade is A and the abrasion resistance is 4000 revolutions.

[0022] Comparative Example 1: The cut-resistant and wear-resistant polypropylene composition fiber provided in this comparative example is prepared from a homopolymer polypropylene composition, which includes modified silicon carbide whiskers and homopolymer polypropylene; The difference between this comparative example and Example 5 is that the content of the modified silicon carbide whisker is 0.1 wt % of the homopolypropylene.

[0023] Comparative Example 2: The cut-resistant and abrasion-resistant polypropylene composition fiber provided in this comparative example is prepared from a homopolymer polypropylene composition, which comprises modified silicon carbide whiskers and homopolymer polypropylene; The difference between this comparative example and Example 5 is that the content of the modified silicon carbide whisker is 10 wt % of the homopolypropylene.

[0024] Comparative Example 3: The cut-resistant and abrasion-resistant polypropylene composition fiber provided in this comparative example is prepared from a homopolymer polypropylene composition, which comprises modified silicon carbide whiskers and homopolymer polypropylene; The difference between this comparative example and Example 5 is that the viscosity average molecular weight of the homopolypropylene is 100,000.

[0025] Comparative Example 4: The cut-resistant and abrasion-resistant polypropylene composition fiber provided in this comparative example is prepared from a homopolymer polypropylene composition, which comprises modified silicon carbide whiskers and homopolymer polypropylene; The difference between this comparative example and Example 5 is that the viscosity average molecular weight of the homopolypropylene is 500,000, and the product purchased is produced by Sinopec Zhenhai Refining and Chemical Company.

[0026] Comparative Example 5: The cut-resistant and abrasion-resistant polypropylene composition fiber provided in this comparative example is prepared from a homopolymer polypropylene composition, which comprises modified silicon carbide whiskers and homopolymer polypropylene; The difference between this comparative example and Example 5 is that the weight ratio of the silicon carbide whiskers to the silane coupling agent in the silicon carbide whiskers modified with the silane coupling agent is 1:0.03.

[0027] Comparative Example 6: The cut-resistant and abrasion-resistant polypropylene composition fiber provided in this comparative example is prepared from a homopolymer polypropylene composition, which comprises modified silicon carbide whiskers and homopolymer polypropylene; The difference between this comparative example and Example 5 is that the weight ratio of the silicon carbide whiskers to the silane coupling agent in the silicon carbide whiskers modified with the silane coupling agent is 1:3.

[0028] Comparative Example 7: The cut-resistant and abrasion-resistant polypropylene composition fiber provided in this comparative example is prepared from a homopolymer polypropylene composition, which comprises modified silicon carbide whiskers and homopolymer polypropylene; The difference between this comparative example and Example 5 is that the weight ratio of dodecylsilane coupling agent to 3-aminopropyltrimethoxysilane is 1:6.

[0029] Comparative Example 8: The cut-resistant and abrasion-resistant polypropylene composition fiber provided in this comparative example is prepared from a homopolymer polypropylene composition, which comprises modified silicon carbide whiskers and homopolymer polypropylene; The difference between this comparative example and Example 5 is that the weight ratio of dodecylsilane coupling agent to 3-aminopropyltrimethoxysilane is 6:1.

[0030] Comparative Example 9: The cut-resistant and abrasion-resistant polypropylene composition fiber provided in this comparative example is prepared from a homopolymer polypropylene composition, which comprises modified silicon carbide whiskers and homopolymer polypropylene; The difference between this comparative example and Example 5 is that the diameter of the silicon carbide whiskers in the silicon carbide whiskers modified by the silane coupling agent is 100-600nm, the length is 50μm, and the β type, and the SiCW-98 product purchased is produced by Qinhuangdao Yinuo High-tech Materials Development Co., Ltd.

[0031] Comparative Example 10: The cut-resistant and abrasion-resistant polypropylene composition fiber provided in this comparative example is prepared from a homopolymer polypropylene composition, which comprises modified silicon carbide whiskers and homopolymer polypropylene; The difference between this comparative example and Example 5 is that the silane coupling agent in the silane coupling agent-modified silicon carbide whiskers is a mixture of octadecylsilane coupling agent and 3-aminopropyltrimethoxysilane, and the octadecylsilane coupling agent purchased is UP-318 product produced by Nanjing Youpu Chemical Co., Ltd.

[0032] Comparative Example 11: The cut-resistant and abrasion-resistant polypropylene composition fiber provided in this comparative example is prepared from a homopolymer polypropylene composition, which comprises modified silicon carbide whiskers and homopolymer polypropylene; The difference between this comparative example and Example 5 is that the silane coupling agent in the silane coupling agent-modified silicon carbide whiskers is a mixture of methyl silane coupling agent and 3-aminopropyltrimethoxysilane, and the methyl silane coupling agent purchased is UP-302 product produced by Nanjing Youpu Chemical Co., Ltd.

[0033] The following is a table of cut resistance grades and abrasion resistance data of cut-resistant fabrics woven from Examples 1-5 and Comparative Examples 1-11, where the cut resistance grades and abrasion resistance are tested in accordance with EN388-2016: ; As can be seen from the above table, the anti-cutting grade and wear resistance of the anti-cutting fabric woven from the polypropylene composition fiber through a textile process are related to the content of modified silicon carbide whiskers, the viscosity-average molecular weight of homopolypropylene and the selected manufacturer, the weight ratio of silicon carbide whiskers to silane coupling agent, the weight ratio of dodecylsilane coupling agent to 3-aminopropyltrimethoxysilane, the diameter of silicon carbide whiskers and the selected product, the selectivity of the silane coupling agent and the selected manufacturer. Therefore, the polypropylene composition fiber prepared by the present invention has excellent wear resistance and cut resistance, effectively prolongs the service life of the fiber, thereby making the fiber easier to be used in the field of labor protection products, and ensuring the application scope of the fiber in the field of labor protection products.

Claims

1. A polypropylene composition fiber, wherein the fiber is prepared from a polypropylene composition, characterized in that: The raw material components of the polypropylene composition include homopolypropylene and modified silicon carbide whiskers with a content of 0.5-5wt% of homopolypropylene. The modified silicon carbide whiskers are silicon carbide whiskers modified by a silane coupling agent, and the silicon carbide whiskers modified by a silane coupling agent are prepared from silicon carbide whiskers and a silane coupling agent.

2. A polypropylene composite fiber according to claim 1, characterized in that: The viscosity average molecular weight of the homopolypropylene is 100,000 to 300,000.

3. A polypropylene composite fiber according to claim 1, characterized in that: The specific preparation steps of the silane coupling agent modified silicon carbide whisker are: ultrasonically dispersing the silicon carbide whisker in a solvent for 20 to 40 minutes, adding a silane coupling agent, stirring at 60 to 80° C. for 2 to 6 hours, and drying to obtain the silane coupling agent modified silicon carbide whisker.

4. A polypropylene composite fiber according to claim 3, characterized in that: The solvent is one of water, methanol, ethyl acetate, acetone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, tetrahydrofuran, and dimethyl sulfoxide, or a mixture of several of them.

5. A polypropylene composite fiber according to claim 3, characterized in that: The weight ratio of the silicon carbide whisker to the silane coupling agent is 1:0.1-0.

5.

6. A polypropylene composite fiber according to claim 5, characterized in that: The silicon carbide whisker is of β-crystal type and its diameter and length are 100-600nm and 3-20µm respectively.

7. A polypropylene composite fiber according to claim 5, characterized in that: The silane coupling agent is one of an alkyl silane coupling agent and an amino silane coupling agent or a mixture of both.

8. A polypropylene composite fiber according to claim 7, characterized in that: The weight ratio of the alkylsilane coupling agent to the aminosilane coupling agent is 2:3 to 3:

2.

9. The polypropylene composite fiber according to claim 1, characterized in that: The specific preparation steps of the fiber are: firstly, the polypropylene composition is heated in a mixer to obtain a blended spinning material, and then the blended spinning material is spun, heat-drawn and shaped to obtain the polypropylene composition fiber.

10. A cut-resistant fabric, characterized in that: The fiber is prepared by using a polypropylene composition fiber as described in any one of claims 1 to 9.