Impermeability test method and device for concrete crack self-repairing coating
Through the combination of hard sheet prefabricated concrete cracks and a water penetration device, the problem in the existing technology of being unable to effectively test the impermeability performance of concrete crack self-healing coatings is solved, and the sealing performance evaluation of concrete crack self-healing coatings is realized, providing a Technical support in structural engineering.
Patent Information
- Application Number
- CN202410840557.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing technology cannot effectively test the anti-permeability performance of self-healing concrete crack coatings in actual engineering projects. Traditional methods cannot quantitatively analyze the internal cracks in concrete and cannot accurately evaluate the sealing performance of self-healing concrete crack coatings.
Use hard thin sheets to precast concrete cracks, and use a water penetration device to conduct tests. The impermeability strength and repairable crack width of the self-healing coating are measured through pressure. Combined with water level control, pressurization and measurement devices, the performance of the self-healing coating for concrete cracks is evaluated. Blocking ability.
It realizes the evaluation of the anti-permeability performance of concrete crack self-healing coatings under different crack widths and coating thicknesses, provides technical support for crack repair in actual structural engineering, and can quickly evaluate the sealing performance of concrete crack self-healing coatings.
Smart Images

Figure CN118817554A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cement-based material testing, and specifically relates to a method and a device for testing the anti-seepage strength of a concrete crack self-repairing coating under crack conditions. Background Art
[0002] Under the conditions of actual structural engineering with cracks, the anti-seepage performance of concrete crack self-repairing coatings is an important parameter that needs to be considered to achieve effective crack sealing. Being able to accurately obtain the anti-seepage performance of concrete crack self-repairing coatings when sealing cracks is crucial to better understanding the waterproof performance of concrete crack self-repairing coatings and guiding their application in waterproofing projects.
[0003] At present, the anti-seepage test of concrete crack self-repairing coating itself is generally carried out directly, and the research on the anti-seepage performance of concrete crack self-repairing coating is generally carried out under the condition of no cracks. However, in actual engineering, the service conditions of building structures are complicated, especially after concrete cracks, concrete crack self-repairing coating is needed to seal the cracks. Therefore, the current research on concrete crack self-repairing coating to repair cracks cannot meet the application of concrete crack self-repairing coating in the actual engineering field.
[0004] Chinese patent CN 117468570 A discloses a method for preventing cracks and leakage in reinforced concrete roofs, in which water is filled in roofs, bathrooms, balconies and other places to check for leaks. This method consumes a lot of manpower and material resources, and cannot fundamentally test the anti-seepage performance of waterproof materials. Chinese patent CN114235593A discloses a hydraulic pressure bond failure test device for polymer waterproof coatings of hydraulic structures, which can directly observe the bond failure strength of the coating under reverse water pressure and the anti-seepage strength under forward water pressure. However, the prefabricated holes in the concrete matrix of the device are mainly used to simulate water blocking parts such as structural joints and anchor cables of hydraulic structures, rather than for concrete cracks formed due to various factors. Chinese patent CN218036302U discloses a device for detecting the anti-seepage effect of the front / back water surface of concrete after leakage repair, which can be used to guide the material selection when repairing leakage on the front / back water surface of concrete and comprehensively evaluate the waterproof and anti-seepage effect after repair. However, the device uses a press to prefabricate concrete cracks, and is unable to quantitatively analyze the crack conditions inside the concrete, and is thus unable to effectively evaluate the crack sealing performance of the concrete crack self-repairing coating. Summary of the invention
[0005] In order to overcome the shortcomings of traditional methods in testing the crack sealing performance of self-repairing coatings for concrete cracks, the present invention provides a method and a device for testing the anti-seepage strength of self-repairing coatings for concrete cracks under crack conditions, uses hard thin slices to prefabricate concrete cracks, and uses a water penetration device to test and evaluate the anti-seepage performance and repairable crack width of the self-repairing coating for concrete cracks, thereby determining the crack sealing ability of the self-repairing coating for concrete cracks.
[0006] The technical solution adopted by the present invention is:
[0007] A method for testing the impermeability of a concrete crack self-repairing coating comprises the following steps:
[0008] 1) Determine the thickness and crack width of the concrete matrix and prepare corresponding specimens, and cure them to the specified age;
[0009] 2) Determine the thickness of the self-repairing coating and seal the cracks, and assemble the device after curing to a specified age; fill the water storage container with water, and pressurize the water through a pressurizing device, and measure the anti-seepage strength of the self-repairing coating through the pressurized strength when the self-repairing coating is damaged;
[0010] 3) Finally, the width of the cracks that can be repaired by the self-repairing coating is determined by a measuring device, and the sealing capacity of the concrete crack self-repairing coating is calculated.
[0011] Furthermore, in the step 1), the strength grade of the concrete substrate should be ≥C20, the diameter should be 50-100 mm, the thickness should be 50-100 mm, the crack width should be 0.1 mm-0.5 mm, and the thickness of the concrete crack self-repairing coating should be 0.5 mm-10 mm.
[0012] In the step 1), the method for prefabricating concrete cracks is to use a hard sheet with a lubricant to penetrate the fresh concrete and insert and remove it regularly before final setting and hardening; the length of the hard sheet should be at least 20 mm less than the diameter of the test piece; the width of the cracks on the water-facing and water-receiving sides of the concrete cracks is observed under a microscope, and the nominal crack width D is equal to the average value of the measured values of the crack widths.
[0013] In the step 1), after the freshly mixed concrete with prefabricated cracks is hardened and cured, a waterproof coating is used to seal the cracks on the water-facing side or the water-receiving side, and the coating is cured to a specified age after hardening.
[0014] In the step 2), the initial pressure intensity is 0.1-0.5 MPa, and increases by 0.1 MPa every 1-3 hours.
[0015] In the step 3), when the impermeability of the self-repairing coating is not less than the impermeability of the concrete matrix, the width of the crack that can be repaired by the self-repairing coating is equal to the width of the prefabricated crack; when the impermeability of the self-repairing coating is less than the impermeability of the concrete matrix, the width of the crack that can be repaired by the self-repairing coating is:
[0016]
[0017] Where: d is the width of cracks that can be repaired by self-repairing coating, mm;
[0018] V——Total water seepage flow after self-repairing coating is damaged, mm 3 ;
[0019] T——water seepage time, s;
[0020] K——permeability coefficient of self-repairing coating, mm / s;
[0021] l——Length of crack in precast concrete, mm.
[0022] In the step 3), the sealing performance of the concrete crack self-repairing coating is evaluated by analyzing the anti-permeability strength and the repairable crack width of the self-repairing coating under conditions of different crack widths and different coating thicknesses.
[0023] A water-resistance testing device for concrete crack self-repairing coating, comprising a water level control device, a pressurizing device, a water seepage device and a measuring device, wherein the upper end of the water level control device is connected to the pressurizing device, and the lower end is connected to the water seepage device, and a measuring device is placed at the bottom of the water seepage device; the water level control device comprises a water storage container, a silicone sleeve and two stainless steel water-stopping hoops, and the connection between the water storage container and the water seepage device is wrapped with a silicone sleeve and fixed with two stainless steel water-stopping hoops; the pressurizing device comprises a pressurizing pipe, a pressurizing pump and a pressure gauge, and the two ends of the pressurizing pipe are respectively connected to the water storage container and the pressurizing pump, and a pressure gauge is installed on the pressurizing pipe; the water seepage device comprises a flange fixing device and a bracket, and the flange fixing device is placed on the bracket; the measuring device comprises a beaker, a load sensor, a data acquisition system and a computer, the beaker is placed on the load sensor, and the load sensor, the data acquisition system and the computer are connected in sequence using a data acquisition line. Further, the water storage container has a scale, and the water storage capacity should be ≥1L.
[0024] Furthermore, the flange fixing device includes two split flanges and four bolts, and the surface where the flange contacts the test piece is padded with a circular silicone gasket; the circular silicone gasket and the contact surface between the flange and the test piece are sealed using a sealing material.
[0025] Furthermore, a silicone sleeve and two stainless steel water-stop rings are used to seal the water level pipe and flange connection.
[0026] Compared with the prior art, the technical effects of the present invention are embodied in:
[0027] 1. The present invention can use different hard slices to accurately preform crack widths, overcoming the shortcoming that traditional methods cannot quantitatively preform cracks;
[0028] 2. The equipment of the present invention is simple and quick to install, and there is no need to use sealing materials such as epoxy resin to seal the concrete matrix, and it can be used in multiple scenarios;
[0029] 3. The present invention fully considers the sealing performance of concrete crack self-repairing coating under crack conditions, and can quickly evaluate the anti-seepage performance of concrete crack self-repairing coating under different crack widths, different coating thicknesses, and on the water-facing and water-retaining surfaces, providing theoretical guarantee and technical support for concrete crack self-repairing coating to repair cracks in actual structural engineering;
[0030] 4. The present invention can effectively evaluate the crack repair width of concrete crack self-repairing coatings under water pressure, and provide technical guarantee for the application scope of crack repair of concrete self-repairing coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a structural schematic diagram of the anti-seepage strength device of the concrete crack self-repairing coating under crack conditions of the present invention;
[0032] Figure 2 Schematic diagram of prefabrication of cracks in fresh concrete in the mold.
[0033] Figure 3 for Figure 1 Top view of the center flange fixture. DETAILED DESCRIPTION
[0034] The specific implementation of the embodiment of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the embodiment of the present invention, and is not used to limit the embodiment of the present invention.
[0035] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0036] Reference Figure 1 to Figure 3 , a method for testing the impermeability of a concrete crack self-repairing coating, comprising the following steps:
[0037] 1) Determine the thickness and crack width of the concrete matrix and prepare corresponding specimens, and cure them to the specified age;
[0038] In the step 1), the strength grade of the concrete substrate should be ≥C20, the diameter should be 50-100 mm, the thickness should be 50-100 mm, the crack width should be 0.1 mm-0.5 mm, and the thickness of the concrete crack self-repairing coating should be 0.5 mm-10 mm.
[0039] In the step 1), the method for prefabricating concrete cracks is to use a hard sheet with a lubricant to penetrate the fresh concrete and insert and remove it regularly before final setting and hardening; the length of the hard sheet should be at least 20 mm less than the diameter of the test piece; the width of the cracks on the water-facing and water-receiving sides of the concrete cracks is observed under a microscope, and the nominal crack width D is equal to the average value of the measured values of the crack widths.
[0040] In the step 1), after the freshly mixed concrete with prefabricated cracks is hardened and cured, a waterproof coating is used to seal the cracks on the water-facing side or the water-receiving side, and the coating is cured to a specified age after hardening.
[0041] 2) Determine the thickness of the self-repairing coating and seal the cracks, and assemble the device after curing to a specified age; fill the water storage container with water, and pressurize the water through a pressurizing device, and measure the anti-seepage strength of the self-repairing coating through the pressurized strength when the self-repairing coating is damaged;
[0042] In the step 2), the initial pressure strength is 0.1-0.5 MPa, and should be increased by 0.1 MPa every 1-3 hours;
[0043] 3) Finally, the width of the cracks that can be repaired by the self-repairing coating is determined by a measuring device, and the sealing capacity of the concrete crack self-repairing coating is calculated.
[0044] In the step 3), when the impermeability of the self-repairing coating is not less than the impermeability of the concrete matrix, the width of the crack that can be repaired by the self-repairing coating is equal to the width of the prefabricated crack; when the impermeability of the self-repairing coating is less than the impermeability of the concrete matrix, the width of the crack that can be repaired by the self-repairing coating is:
[0045]
[0046] Where: d is the width of cracks that can be repaired by self-repairing coating, mm;
[0047] V——Total water seepage flow after self-repairing coating is damaged, mm 3 ;
[0048] T——water seepage time, s;
[0049] K——permeability coefficient of self-repairing coating, mm / s;
[0050] l——Length of crack in precast concrete, mm.
[0051] In the step 3), the sealing performance of the concrete crack self-repairing coating is evaluated by analyzing the anti-permeability strength and the repairable crack width of the self-repairing coating under conditions of different crack widths and different coating thicknesses.
[0052] A device for testing the anti-seepage of a self-repairing coating for concrete cracks comprises a water level control device, a pressurizing device, a water seepage device and a measuring device, wherein the upper end of the water level control device is connected to the pressurizing device, and the lower end is connected to the water seepage device, and a measuring device is placed under the water seepage device; the water level control device comprises a water storage container 1, a silicone sleeve 2 and two stainless steel water-stopping hoops 3, the connection between the water storage container and the water seepage device is wrapped with a silicone sleeve and fixed with two stainless steel water-stopping hoops; the pressurizing device comprises a pressurizing pipe 4, a pressurizing pump and a pressure gauge 5, the two ends of the pressurizing pipe are respectively connected to the water storage container and the pressurizing pump, and a pressure gauge is installed on the pressurizing pipe; the water seepage device comprises a flange fixing device and a bracket 6, and the flange fixing device is placed on the bracket; the measuring device comprises a beaker 7, a load sensor 8, a data acquisition system and a computer, the beaker is placed on the load sensor, and the load sensor, the data acquisition system and the computer are sequentially connected using a data acquisition line.
[0053] Furthermore, the water storage container has a scale, and the water storage capacity should be ≥1L.
[0054] Furthermore, the flange fixing device includes two split flanges 9 and four bolts 10, and the surface where the flange contacts the test piece 11 is padded with a circular silicone gasket 12; the circular silicone gasket and the contact surface between the flange and the test piece should be sealed with sealing materials such as silicone rubber.
[0055] Furthermore, a silicone sleeve and two stainless steel water-stop rings are used to seal the water storage container and the flange connection.
[0056] The following is a specific description through further embodiments:
[0057] Concrete mix ratio: water-binder ratio 0.4, cement 311kg / m 3 、Fly ash 104kg / m 3 、Slag 104kg / m 3 , water 207kg / m 3 、River sand 777kg / m 3 、Stone 864kg / m 3 , water reducing agent 5.2kg / m 3 .
[0058] First, use vaseline lubricant to lubricate the iron sheet with a thickness of 0.2 mm, a width of 80 mm, and a height of 50 mm. Then pour the prepared concrete into a mold with a diameter of 100 mm and a height of 50 mm, which is pre-installed with an iron sheet, and vibrate it to form a concrete. Figure 2 As shown, the iron sheets are inserted and pulled out every 0.5 h before the final setting time to form prefabricated cracks (13). After curing for 1 day, the molds are removed, the actual crack width is measured with a microscope, and the steel is cured in water until the age of 7 days.
[0059] The concrete material substrate is taken out of the water, and after the surface of the substrate is dried, the prepared concrete crack self-repairing coating (15) is applied to the water-facing surface of the cracks of the substrate (11) with a thickness of 10 mm. After curing for 1 day, the formwork is removed and the substrate is cured in water until the age of 7 days.
[0060] like Figure 3 As shown, after the surface of the cured specimen is dried, a circular silicone gasket (12) is placed on the coating surface, and the specimen is clamped in the center using two split flanges (9) and fixed using bolts (10).
[0061] Then insert the water level pipe into the round mouth of the flange and seal it with a silicone sleeve and two stainless steel water-stop hoops. Each hoop is 20 mm high and the hoops are tightened to make the connection between the water level pipe and the flange sealed. The circular silicone gasket is sealed with silicone rubber at the contact surface between the flange and the test piece.
[0062] The water storage container is filled with water and the water volume reaches 1L. Figure 1 As shown, the water storage container is then connected to the pressure pipe 4 and the pressure pump by means of a screw port, and the pressure strength is observed by means of a pressure gauge 5. The initial pressure strength is 0.1 MPa, and then increases by 0.1 MPa every 1 hour until penetration occurs at the bottom of the specimen. At this time, the pressure strength displayed by the pressure gauge is the anti-seepage strength of the concrete crack self-repairing coating. After the concrete crack self-repairing coating is damaged, the pressure remains unchanged, and the water flows into the beaker through the damaged cracks. The load sensor transmits the measured data to the computer through the data acquisition system, and the crack area that can be repaired by the self-repairing coating is obtained after data processing, which characterizes the sealing performance of the concrete crack self-repairing coating.
[0063] The above embodiments are only preferred embodiments of the present invention and are not limitations of the technical solutions of the present invention. Any technical solution that can be implemented on the basis of the above embodiments without creative work should be deemed to fall within the scope of protection of the patent of the present invention.
Claims
1. A method for testing the impermeability of a concrete crack self-repairing coating, characterized in that: The steps include: 1) Determine the thickness and crack width of the concrete matrix and prepare corresponding specimens, and cure them to the specified age; 2) Determine the thickness of the self-repairing coating and seal the cracks, and assemble the device after curing to a specified age; fill the water storage container with water, and pressurize the water through a pressurizing device, and measure the anti-seepage strength of the self-repairing coating through the pressurized strength when the self-repairing coating is damaged; 3) Finally, the width of the cracks that can be repaired by the self-repairing coating is determined by a measuring device, and the sealing capacity of the concrete crack self-repairing coating is calculated.
2. A method for testing the impermeability of a concrete crack self-repairing coating according to claim 1, characterized in that: In the step 1), the strength grade of the concrete substrate should be ≥C20, the diameter should be 50-100 mm, the thickness should be 50-100 mm, the crack width should be 0.1 mm-0.5 mm, and the thickness of the concrete crack self-repairing coating should be 0.5 mm-10 mm.
3. A method for testing the impermeability of a concrete crack self-repairing coating according to claim 1 or 2, characterized in that: In the step 1), the method for prefabricating concrete cracks is to use a hard sheet with a lubricant to penetrate the fresh concrete and insert and remove it regularly before final setting and hardening; the length of the hard sheet should be at least 20 mm less than the diameter of the test piece; the width of the cracks on the water-facing and water-receiving sides of the concrete cracks is observed under a microscope, and the nominal crack width D is equal to the average value of the measured values of the crack widths.
4. A method for testing the impermeability of a concrete crack self-repairing coating according to claim 1 or 2, characterized in that: In the step 1), after the freshly mixed concrete with prefabricated cracks is hardened and cured, a waterproof coating is used to seal the cracks on the water-facing side or the water-receiving side, and the coating is cured to a specified age after hardening.
5. A method for testing the impermeability of a concrete crack self-repairing coating according to claim 1 or 2, characterized in that: In the step 2), the initial pressure intensity is 0.1-0.5 MPa, and should be increased by 0.1 MPa every 1-3 hours.
6. A method for testing the impermeability of a concrete crack self-repairing coating according to claim 1 or 2, characterized in that: In the step 3), when the impermeability of the self-repairing coating is not less than the impermeability of the concrete matrix, the width of the crack that can be repaired by the self-repairing coating is equal to the width of the prefabricated crack; when the impermeability of the self-repairing coating is less than the impermeability of the concrete matrix, the width of the crack that can be repaired by the self-repairing coating is: Where: d is the width of cracks that can be repaired by self-repairing coating, mm; V——Total water seepage flow after self-repairing coating is damaged, mm 3 ; T——water seepage time, s; K——permeability coefficient of self-repairing coating, mm / s; l——Length of crack in precast concrete, mm.
7. A method for testing the impermeability of a concrete crack self-repairing coating according to claim 6, characterized in that: In the step 3), the sealing performance of the concrete crack self-repairing coating is evaluated by analyzing the anti-permeability strength and the repairable crack width of the self-repairing coating under conditions of different crack widths and different coating thicknesses.
8. A device for implementing the anti-permeability test method for concrete crack self-repairing coating according to claim 1, characterized in that: The device comprises a water level control device, a pressurizing device, a water seepage device and a measuring device. The upper end of the water level control device is connected to the pressurizing device, and the lower end is connected to the water seepage device. The measuring device is placed under the water seepage device. The water level control device comprises a water storage container (1), a silicone sleeve (2) and two stainless steel water stop rings (3). The connection between the water storage container and the water seepage device is wrapped with a silicone sleeve and fixed with two stainless steel water stop rings. The pressurizing device comprises a pressurizing pipe (4), a pressurizing pump and a pressure gauge (5). The two ends of the pressurizing pipe are respectively connected to the water storage container and the pressurizing pump. The pressure gauge is installed on the pressurizing pipe. The water seepage device comprises a flange fixing device and a bracket (6). The flange fixing device is placed on the bracket. The measuring device comprises a beaker (7), a load sensor (8), a data acquisition system and a computer. The beaker is placed on the load sensor. The load sensor, the data acquisition system and the computer are connected in sequence using a data acquisition line.
9. The device according to claim 8, characterized in that The water storage container has a scale and the water storage capacity should be ≥1L.
10. The device according to claim 8 or 9, characterized in that The flange fixing device comprises two split flanges (9) and four bolts (10); the surface where the flange contacts the test piece (11) is padded with a circular silicone gasket (12); the contact surface between the circular silicone gasket and the flange and the test piece should be sealed with a sealing material; the connection between the water storage container and the flange is sealed with a silicone sleeve and two stainless steel water-stop hoops.
Citation Information