Method for forming interconnection structure

By using a boron-containing compound to form a barrier layer and selectively depositing the barrier layer in microelectronic components, the problem of insufficient selectivity of metal deposition on the dielectric surface in the existing technology is solved, the effect of reducing via hole resistance is achieved, and the quality of microelectronics is improved. component performance.

CN118824944APending Publication Date: 2024-10-22APPLIED MATERIALS INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410478054.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-19
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing technology makes it difficult to selectively deposit metal on the dielectric surface in microelectronic components, especially when the growth of tantalum nitride on the aluminum oxide surface is inhibited, resulting in reduced electrical performance.

Method used

By exposing the features to a boron-containing compound, a barrier layer is formed, and a barrier layer is selectively deposited on the barrier layer, followed by removal of the barrier layer to reduce via resistance, using an atomic layer deposition (ALD) process and plasma treatment to increase deposition density.

Benefits of technology

It effectively reduces the via resistance on the dielectric surface and alumina surface by at least 20%, and improves the interconnect structure performance of microelectronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118824944A_ABST
    Figure CN118824944A_ABST
Patent Text Reader

Abstract

Methods of forming semiconductor elements by enhanced selective deposition are described. In some embodiments, a barrier layer is deposited on a metal surface prior to depositing the barrier layer. The methods include exposing a substrate having a metal surface, a dielectric surface, and an alumina or aluminum nitride surface to a barrier molecule, such as a boron-containing compound, to selectively form a barrier layer on one of the alumina or aluminum nitride surface and the metal surface over the dielectric surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present disclosure generally relate to methods of forming interconnect structures in microelectronic components. More particularly, embodiments of the present disclosure relate to methods of improving selective deposition of metal on dielectric surfaces during formation of interconnect structures in microelectronic components. Background Art

[0002] The semiconductor industry faces many challenges in the pursuit of device miniaturization, which involves the rapid scaling of nanoscale features. Such issues include the introduction of complex manufacturing steps, such as multiple photolithography steps, and the integration of high-performance materials. Selective deposition holds promise for device miniaturization because it has the potential to remove expensive photolithography steps by simplifying integration schemes.

[0003] Selective deposition of materials can be achieved in a variety of ways. Chemical precursors can selectively react with one surface relative to another surface (metal or dielectric). Process parameters such as pressure, substrate temperature, precursor partial pressure and / or gas flow can be adjusted to adjust the chemical kinetics of a specific surface reaction. Another possible approach involves surface pretreatment, which can be used to activate or passivate the target surface of the incoming film deposition precursor. For example, a self-assembled monolayer (SAM) can be formed on the surface to prevent subsequent deposition on the surface.

[0004] The self-assembled monolayers of the prior art do not inhibit the growth of a tantalum nitride barrier layer on a tungsten surface. The growth of tantalum nitride on metallic tungsten can be slowed down using bifunctional SAMs based on oxygen and nitrogen. However, bifunctional SAMs also inhibit the growth of tantalum nitride on aluminum oxide surfaces, which are often used as etch stop layers in electronic components. Inhibition of the tantalum nitride barrier layer on the aluminum oxide layer / surface results in reduced electrical performance of the electronic component.

[0005]

[0006] Therefore, there is a growing need in the art for methods of improving the selective deposition of metals on dielectric surfaces during the formation of interconnect structures in microelectronic components. Summary of the invention

[0006] One or more embodiments of the present disclosure are directed to a method of forming a microelectronic component. The method includes exposing a feature structure extending into a semiconductor substrate to a substrate having a general formula R (3-n) BX nor a boron-containing compound of H3B-BH3, wherein n is 0 to 3, X is hydrogen or methyl, and each R is independently selected from alkyl, aryl, olefin, and alkyne groups having 1 to 22 carbon atoms to form a barrier layer. The feature structure defines a gap including a metal surface, a dielectric surface, and an aluminum oxide surface or an aluminum nitride surface, and the barrier layer is selectively formed on the metal surface above one of the aluminum oxide surface or the aluminum nitride surface and the dielectric surface. The method further includes selectively depositing a barrier layer on one of the aluminum oxide surface or the aluminum nitride surface and the dielectric surface above the barrier layer; and removing the barrier layer.

[0007] In one aspect, wherein the boron-containing compound may include

[0008]

[0009] wherein each R is independently selected from alkyl, aryl, alkene and alkyne groups having 1 to 22 carbon atoms.

[0010] In another aspect, wherein the boron-containing compound may include

[0011]

[0012] wherein R is selected from alkyl, aryl, alkene and alkyne groups having 1 to 22 carbon atoms.

[0013] In yet another aspect, wherein the boron-containing compound may include 9-borabicyclo[3.3.1]nonane

[0014]

[0015] In another aspect, the boron-containing compound is carried in an inert gas selected from the group consisting of helium (He), neon (Ne), argon (Ar) and krypton (Kr).

[0016] In another aspect, the metal surface may include one or more of tungsten (W), molybdenum (Mo), or cobalt (Co).

[0017] In yet another aspect, the dielectric surface may include a low-k dielectric material.

[0018] In another aspect, wherein selectively depositing the barrier layer may include an atomic layer deposition (ALD) process.

[0019] In another aspect, the barrier layer may include tantalum nitride (TaN).

[0020] In yet another aspect, the method can further include selectively depositing a metal liner on the barrier layer.

[0021] In another aspect, the metal liner may include one or more of ruthenium (Ru), cobalt (Co), molybdenum (Mo), or tantalum (Ta).

[0022] In yet another aspect, the removing the barrier layer may include exposing the barrier layer to plasma.

[0023] In another aspect, the plasma can be an inductively coupled plasma (ICP).

[0024] In yet another aspect, the plasma may be a capacitively coupled plasma (CCP).

[0025] In another aspect, exposing the barrier layer to a plasma increases the density of the barrier layer.

[0026] In yet another aspect, the method may further include performing a gap-fill process to deposit a gap-fill material within the gap.

[0027] In another aspect, the gap-fill material may include copper (Cu) or cobalt (Co).

[0028] In another aspect, the method can reduce the resistance of the via by at least 20% compared to a method that does not include forming a barrier layer, the barrier layer being selectively formed on the metal surface relative to the dielectric surface and the aluminum oxide surface or the aluminum nitride surface.

[0029] Another embodiment of the present disclosure is directed to a method of forming a microelectronic element. The method includes exposing a feature structure extending into a semiconductor substrate to a barrier molecule including the general formula (I) or (II):

[0030]

[0031] wherein each R is independently selected from alkyl, aryl, olefin and alkyne groups having 1 to 22 carbon atoms to form a barrier layer. The feature structure defines a gap including a metal surface, a dielectric surface and an aluminum oxide surface or an aluminum nitride surface, and selectively forms a barrier layer on the metal surface above one of the aluminum oxide surface or the aluminum nitride surface and the dielectric surface. The method further includes selectively depositing a barrier layer on one of the aluminum oxide surface or the aluminum nitride surface and the dielectric surface above the barrier layer; and removing the barrier layer.

[0032] In one aspect, the method may further include performing a gap filling process after removing the barrier layer, the gap filling process including filling the gap with one or more of copper (Cu) or cobalt (Co). BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to be able to understand in detail the manner in which the above-mentioned features of the present disclosure are achieved, the present disclosure briefly summarized above may be described in more detail by reference to embodiments, some of which are shown in the accompanying drawings. However, it should be noted that the accompanying drawings illustrate only typical embodiments of the present disclosure and therefore should not be considered as limiting the scope of the present disclosure, as the present disclosure may admit of other equally effective embodiments.

[0034] Figure 1 A process flow diagram illustrating a method of forming a microelectronic element according to one or more embodiments of the present disclosure;

[0035] Figure 2 shows a schematic cross-sectional view of a microelectronic element prior to a selective deposition process according to one or more embodiments of the present disclosure;

[0036] Figure 3 FIG. 2 shows a structure after forming a barrier layer according to one or more embodiments of the present disclosure. Figure 2 A schematic cross-sectional view of a microelectronic component;

[0037] Figure 4 FIG. 2 shows a structure after forming a barrier layer according to one or more embodiments of the present disclosure. Figure 3 A schematic cross-sectional view of a microelectronic component;

[0038] Figure 5 FIG. 2 shows a structure after removing the barrier layer according to one or more embodiments of the present disclosure. Figure 4 A schematic cross-sectional view of a microelectronic component;

[0039] Figure 6 FIG. 1 shows a structure after forming a metal liner according to one or more embodiments of the present disclosure. Figure 5 A schematic cross-sectional view of a microelectronic component; and

[0040] Figure 7 FIG. 2 shows a structure after forming a second metal layer according to one or more embodiments of the present disclosure. Figure 6 Schematic cross-sectional view of a microelectronic component. DETAILED DESCRIPTION

[0041] Before describing several exemplary embodiments of the present disclosure, it should be understood that the present disclosure is not limited to the details of construction or processing steps set forth in the following description. The present disclosure is capable of other embodiments and can be practiced or carried out in various ways.

[0042] As used in this specification and the appended claims, the terms "substrate" and "wafer" are used interchangeably, and both refer to a surface or portion of a surface on which a process acts. Those skilled in the art will also understand that reference to a substrate may also refer to only a portion of a substrate, unless the context clearly indicates otherwise. In addition, reference to depositing on a substrate may mean both a bare substrate and a substrate having one or more films or features deposited or formed thereon.

[0043] As used herein, "substrate surface" refers to any portion of a substrate or a portion of a material surface formed on a substrate on which film processing is performed. For example, depending on the application, the substrate surface that can be processed on it includes materials such as silicon, silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, and other conductive materials. The substrate includes, but is not limited to, a semiconductor wafer. The substrate can be exposed to a pretreatment process to polish, etch, reduce, oxidize, hydroxylate, anneal, UV cure, electron beam cure, and / or bake the substrate surface. In addition to performing film processing directly on the surface of the substrate itself, in the present disclosure, as disclosed in more detail below, any disclosed film processing steps can also be performed on the bottom layer formed on the substrate, and the term "substrate surface" is intended to include such a bottom layer indicated by the context. Therefore, for example, in the case where a film / layer or a portion of a film / layer has been deposited on the substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface. The substrate can have various dimensions, such as a 200mm or 300mm diameter wafer, and a rectangular or square window glass. In some embodiments, the substrate includes a rigid discrete material. What a given substrate surface comprises will depend on what film is to be deposited, as well as the specific chemistry used.

[0044] As used herein, "atomic layer deposition" or "cyclic deposition" refers to a process that includes sequential exposure to two or more reactive compounds to deposit a layer of material on a substrate surface. As used in this specification and the appended claims, the terms "reactive compound", "reactive gas", "reactive substance", "precursor", "process gas", etc. are used interchangeably to refer to a substance that can react with the surface of the substrate or the material on the substrate surface (e.g., chemical adsorption, oxidation, reduction, cycloaddition). The substrate or portion of the substrate is sequentially exposed to two or more reactive compounds introduced into a reaction zone of the processing chamber.

[0045] Embodiments of the present disclosure provide methods for depositing a barrier layer on a metal surface. Embodiments of the present disclosure identify methods for depositing a barrier layer, which methods may be used alone or in combination with one another.

[0046] Embodiments of the present disclosure advantageously provide methods of depositing a barrier material, such as tantalum nitride (TaN), on a dielectric surface by preventing the barrier material from being deposited on the metal surface via a barrier layer deposited on the metal surface.

[0047] Embodiments of the present disclosure provide methods for forming interconnect structures when manufacturing microelectronic components. In one or more embodiments, the microelectronic components described herein include at least one top interconnect structure interconnected to at least one bottom interconnect structure. Embodiments of the present disclosure provide microelectronic components and methods for manufacturing microelectronic components, which improve the performance of the interconnect, such as reducing the via resistance.

[0048] refer to Figures 1 to 7 , describes a general process flow for a method 10 of forming a microelectronic component according to one or more embodiments of the present disclosure. The methods described herein (e.g., method 10) can be used to form semiconductor components or interconnects for semiconductor components. An interconnect used in this manner is a conductive portion of an electronic component that allows electrical connection between different layers of the electronic component.

[0049] Figure 1 The method 10 in the embodiment of the present invention includes exposing a feature structure extending into a semiconductor substrate to a barrier molecule, such as a boron-containing compound, to form a barrier layer, the feature structure defining a gap including a metal surface, a dielectric surface, and an aluminum oxide surface or an aluminum nitride surface, selectively forming the barrier layer on one of the aluminum oxide surface or the aluminum nitride surface and the metal surface above the dielectric surface (operation 12); selectively depositing a barrier layer on one of the aluminum oxide surface or the aluminum nitride surface and the dielectric surface above the barrier layer (operation 14); removing the barrier layer (operation 16); optionally, selectively depositing a metal liner on the barrier layer (operation 18); and performing a gap filling process (operation 20).

[0050] Embodiments of the present disclosure advantageously provide methods for reducing via resistance. It has been advantageously found that the methods described herein, such as method 10, can reduce the total effective resistance of a circuit, and identify barrier chemistries and strategies to weaken the adsorption of molecules on metals with more van der Waals bonding forces so that the molecules are more easily desorbed after deposition of a barrier layer (e.g., TaN) and cleaning, thereby maintaining the overall resistance benefit. Advantageously, the methods described herein, such as method 10, reduce the resistance of the via by at least 20% compared to methods that do not include forming a barrier layer, and selectively form a barrier layer on a metal surface relative to a dielectric surface and an aluminum oxide surface or an aluminum nitride surface.

[0051] Figure 2An exemplary embodiment of an electronic component 100 is shown. Those skilled in the art will recognize that the illustrated embodiment is merely one exemplary possible configuration, and that the scope of the present disclosure is not limited to the illustrated electronic component structure.

[0052] Figure 2 The electronic component 100 shown has a substrate 105 with a first layer 110 formed thereon. The substrate 105 can be any suitable substrate material for electronic components. In some embodiments, the substrate 105 is a semiconductor substrate. In some embodiments, the substrate 105 can include additional layers of dielectrics, metals, etch stop layers, and semiconductor layers including underlying circuits (e.g., transistors, capacitors) formed in existing processes.

[0053] Those skilled in the art will appreciate that the use of ordinal numbers such as "first" and "second" to describe different layers or films does not imply a specific position or number within an electronic component, or specify an order of formation. A "second" layer of material may be formed without the presence of a "first" layer. When referring to the drawings, the ordinal numbers are used for descriptive purposes.

[0054] The first layer 110 is an optional layer. In some embodiments, the first layer 110 is omitted. In some embodiments, the first layer 110 is composed of a stack of more than one layer. The first layer 110 can have any suitable function, including but not limited to being used as an etch stop layer for previous or future microelectronic component manufacturing operations.

[0055] A first dielectric layer 140 is formed on a portion of the first layer 110. The first dielectric layer 140 has inner sidewalls 142 that define the boundaries of the first dielectric layer 140 and leave an opening. The opening may be, for example, a trench for a first metallization layer of the electronic component 100.

[0056] The first dielectric layer 140 may be any suitable material formed by any suitable technique known to those skilled in the art. In some embodiments, the first dielectric layer 140 comprises one or more of an oxide or a nitride. In some embodiments, the first dielectric layer 140 comprises silicon oxide. The first dielectric layer 140 of some embodiments is deposited by one or more of chemical vapor deposition (CVD), atomic layer deposition (ALD), plasma enhanced chemical vapor deposition (PECVD), plasma enhanced atomic layer deposition (PEALD), physical vapor deposition (PVD), or spin coating techniques.

[0057] The dielectric surface of the first dielectric layer 140 on the substrate 105 may include any suitable dielectric material. Suitable dielectric materials include, but are not limited to, oxides (e.g., silicon oxide), low-k dielectric materials, and high-k dielectric materials. In some embodiments, the dielectric surface consists essentially of silicon oxide. When used in this manner, the term "consisting essentially of" means that the surface is greater than or equal to about 95%, 98%, or 99% of the material based on area. In some embodiments, the first dielectric layer 140 includes one or more of silicon oxide (SiO2), silicon nitride (SiN), silicon oxynitride carbon (SiCON), silicon oxycarbide (SiOC), aluminum oxide (AlOx), or aluminum nitride (AlNx).

[0058] In some embodiments, the liner 120 is formed on the top surface of the first layer 110 and abuts the inner sidewall 142 of the first dielectric layer 140. The liner 120 of some embodiments serves as one or more of an adhesion layer, a barrier layer, or a liner. The liner 120 may be any suitable material, including but not limited to oxides and nitrides. The liner 120 may be formed by any suitable technique known to those skilled in the art. In some embodiments, the liner 120 is formed as a conformal film by atomic layer deposition (ALD).

[0059] In some embodiments, the first metal layer 130 is formed on the pad 120 and forms a first metallization layer. The first metal layer 130 can be any suitable material deposited by any suitable technique known to those skilled in the art. Suitable metal materials include, but are not limited to, metals, metal nitrides, metal alloys, and other conductive materials. In some embodiments, the first metal layer 130 includes one or more of copper (Cu), cobalt (Co), tungsten (W), molybdenum (Mo), ruthenium (Ru), or titanium nitride (TiN). In some embodiments, the first metal layer 130 is substantially composed of cobalt (Co). In some embodiments, the first metal layer 130 is substantially composed of tungsten (W). In some embodiments, the first metal layer 130 is substantially composed of titanium nitride (TiN).

[0060] In some embodiments, an etch stop layer 150 is formed on the first metal layer 130. The etch stop layer 150 may be any suitable material formed by any suitable technique known to those skilled in the art.

[0061] In some embodiments, the etch stop layer 150 includes one or more of aluminum oxide (AlOx), such as Al2O3, or aluminum nitride (AlNx). In some embodiments, the etch stop layer 150 consists essentially of one or more of aluminum oxide (AlOx) or aluminum nitride (AlNx). In some embodiments, the etch stop layer 150 includes aluminum oxide (AlOx). In some embodiments, the etch stop layer 150 consists essentially of aluminum oxide (AlOx). In some embodiments, the etch stop layer 150 includes aluminum nitride (AlNx). In some embodiments, the etch stop layer 150 consists essentially of aluminum nitride (AlNx).

[0062] In some embodiments, a second dielectric layer 160 is formed on the etch stop layer 150. The second dielectric layer 160 can be any suitable material formed by any suitable technique known to those skilled in the art. In some embodiments, the second dielectric layer 160 includes one or more of an oxide or a nitride. In some embodiments, the second dielectric layer 160 includes a low-k dielectric material. In some embodiments, the second dielectric layer 160 includes silicon oxide. The second dielectric layer 160 of some embodiments is deposited by one or more of chemical vapor deposition (CVD), atomic layer deposition (ALD), plasma enhanced chemical vapor deposition (PECVD), plasma enhanced atomic layer deposition (PEALD), physical vapor deposition (PVD), or spin coating techniques.

[0063] The second dielectric layer 160 includes a material different from the etch stop layer 150. The dielectric surface of the second dielectric layer 160 may include any suitable dielectric material. Suitable dielectric materials include, but are not limited to, oxides (e.g., silicon oxide), low-k dielectric materials, and high-k dielectric materials. In some embodiments, the dielectric surface is substantially composed of silicon oxide. In some embodiments, the second dielectric layer 160 includes one or more of silicon oxide (SiO2), silicon nitride (SiN), silicon oxynitride carbon (SiCON), silicon oxycarbide (SiOC), aluminum oxide (AlOx), or aluminum nitride (AlNx). In some embodiments, the second dielectric layer 160 includes the same material as the first dielectric layer 140. In some embodiments, the second dielectric layer 160 includes a material different from the first dielectric layer 140.

[0064] The substrate 105 including the second dielectric layer 160, the etch stop layer 150 and the first metal layer 130 has a feature structure 170 formed therein. The feature structure 170 is formed in the second dielectric layer 160 and the etch stop layer 150, thereby exposing the top surface 132 of the first metal layer 130. The feature structure 170 shown has a via portion 172 and a trench portion 174.

[0065] The via portion 172 extends through the second dielectric layer 160 and the etch stop layer 150 to the first metal layer 130. The via portion 172 exposes the top surface 132 of the first metal layer 130. The top surface 132 of the first metal layer 130 forms a bottom surface 164 of the via portion 172. One side of the via portion 172 is defined by the sidewall 162 of the second dielectric layer 160 and the sidewall 163 of the etch stop layer 150. The other side of the via portion 172 is defined by the lower sidewall 167 of the second dielectric layer 160 and the sidewall 163 of the etch stop layer 150. Those skilled in the art will recognize that the via portion 172 can have a circular cross-section, and recognize that the use of a first side and a second side (e.g., one side and the other side) to describe the via portion 172 is for the purpose of description based on the cross-sectional view in the drawings. When via portion 172 is a cylindrical hole, the sidewalls of the dielectric layer and the etch stop layer are continuous so that there is actually a single sidewall rather than first and second sides (eg, one side and the other side) appearing in cross section.

[0066] Trench portion 174 has a bottom surface 168 formed by second dielectric layer 160 and one side of trench portion 174 is defined by upper sidewall 169 including second dielectric layer 160. Trench portion 174 has an open side in which via portion 172 passes through second dielectric layer 160 and etch stop layer 150.

[0067] Portions of feature 170 not defined by via portion 172 and trench portion 174 may be collectively referred to as gaps.

[0068] Embodiments of the present disclosure advantageously provide methods for surface pretreatment, such as selective barrier of metal surfaces, including but not limited to copper, cobalt, tungsten, tantalum, tantalum nitride, tantalum oxide, titanium, titanium oxide, titanium nitride, ruthenium, ruthenium oxide, and iridium, etc. Some embodiments advantageously provide methods for selectively growing dielectric materials on dielectric surfaces, such as SiO2, SiN, SiCON, SiOC, etc.

[0069] Figure 1 The embodiment shown is a substrate 105 for further deposition processes. In the embodiment shown, the etch stop layer 150 is one or more of aluminum oxide or aluminum nitride, and the surface (sidewall 163) of the etch stop layer 150 is one or more of an aluminum oxide surface or an aluminum nitride surface. For the avoidance of doubt, unless the context otherwise provides, the identification of materials disclosed herein does not imply a stoichiometric ratio. For example, an aluminum oxide (AlOx) material contains aluminum and oxygen, and an aluminum nitride (AlNx) material contains aluminum and nitrogen. The ratio of these elements is not necessarily 1:1.

[0070] The substrate 105 has one or more of a metal surface (bottom surface 164 of the via portion 172), a dielectric surface (side wall 162, lower side wall 167, bottom surface 168, upper side wall 169 and top surface 161), and an aluminum oxide surface or an aluminum nitride surface (side wall 163 of the etch stop layer 150).

[0071] Figure 3 shows the selective deposition of barrier layer 180 after Figure 2 The electronic component 100 of FIG. 1 is a substrate 105 including one or more of a metal surface (bottom surface 164 of via portion 172), a dielectric surface (sidewall 162, lower sidewall 167, bottom surface 168, upper sidewall 169, and top surface 161), and an aluminum oxide surface or an aluminum nitride surface (sidewall 163 of etch stop layer 150) is exposed to barrier molecules, such as a boron-containing compound, to form a barrier layer 180. The barrier layer 180 is selectively formed on the dielectric surface (sidewall 162, lower sidewall 167, bottom surface 168, upper sidewall 169, and top surface 161) and the metal surface (bottom surface 164 of via portion 172) above the aluminum oxide surface or the aluminum nitride surface.

[0072] In some embodiments, the barrier molecule used to deposit the barrier layer 180 comprises a boron-containing compound. In some embodiments, the boron-containing compound has a general formula R (3-n) BX n or H3B-BH3, wherein n is 0 to 3, X is hydrogen or methyl, and each R is independently selected from alkyl, aryl, alkene, and alkyne groups having 1 to 22 carbon atoms. In one or more embodiments, the boron-containing compound includes BH3. In one or more embodiments, the boron-containing compound includes H3B-BH3.

[0073] In some embodiments, the boron-containing compound comprises

[0074]

[0075] wherein each R is independently selected from alkyl, aryl, alkene and alkyne groups having 1 to 22 carbon atoms.

[0076] In some embodiments, the boron-containing compound comprises

[0077]

[0078] wherein R is selected from alkyl, aryl, alkene and alkyne groups having 1 to 22 carbon atoms.

[0079] In some embodiments, the alkyl group includes a straight chain group (e.g., n-butyl), a branched group (e.g., tert-butyl), or a cyclic group (e.g., cyclohexyl). When used in this manner, the letter "C" followed by a number (e.g., "C4") means that the substituent includes a specified number of carbon atoms (e.g., C4 includes four carbon atoms). In one or more embodiments, each R is independently selected from alkyl, aryl, alkene, and alkyne groups having 1 to 22 carbon atoms, and R includes substituted alkyl. In one or more embodiments, the substituted alkyl includes one or more cyclic substituents or aryl substituents.

[0080] In some embodiments, the boron-containing compound includes 9-borabicyclo[3.3.1]nonane

[0081]

[0082] In some embodiments, the boron-containing compound includes one or more of the following:

[0083]

[0084] (4-(Diphenylamino)phenylboronic acid),

[0085]

[0086] (borane pyridine),

[0087]

[0088] (tri-tert-butyl borate),

[0089]

[0090] (4-(Diethylamino)phenylboronic acid),

[0091]

[0092] (3-(N,N-dimethylamino)phenylboronic acid),

[0093]

[0094] (p-Toluenethiolboric acid),

[0095]

[0096] (p-Tolueneboric acid),

[0097]

[0098] (4-methoxyphenylboronic acid),

[0099]

[0100] (4-(tert-butyldimethylsilyloxy)phenylboronic acid), or

[0101]

[0102] (4-Formylphenylboronic acid).

[0103] In some embodiments, the barrier molecule used to deposit the barrier layer 180 includes a barrier molecule having the general formula (I) or (II):

[0104]

[0105] wherein each R is independently selected from alkyl, aryl, alkene and alkyne groups having 1 to 22 carbon atoms.

[0106] In some embodiments, the boron-containing compound is carried in a suitable inert gas known to those skilled in the art. In some embodiments, the inert gas is selected from the group consisting of: helium (He), neon (Ne), argon (Ar), and krypton (Kr).

[0107] Barrier layer 180 is a metal boride selectively formed on a metal surface. In some embodiments, the metal boride is selectively formed on a metal surface (bottom surface 164 of via portion 172) above one or more of an aluminum oxide surface or an aluminum nitride surface (sidewall 163 of etch stop layer 150) and a dielectric surface (sidewall 162, lower sidewall 167, bottom surface 168, upper sidewall 169, and top surface 161). As used in this specification and the appended claims, the phrase "selectively above..." or the like means that the subject material is deposited on the surface to a greater extent than on another surface. In some embodiments, "selectively" means that the subject material is formed on the selective surface at a rate greater than or equal to 10 times, 15 times, 20 times, 25 times, 30 times, 35 times, 40 times, 45 times, or 50 times the formation rate on the unselected surface.

[0108] In some embodiments, the barrier molecule reacts with a metal surface (including but not limited to Cu, Co, W and TiN) in solution or gas phase. In some embodiments, the metal surface is cleaned before reacting with the barrier molecule. The organoborane selectively reacts with the metal surface through the boron head group on one or more of the aluminum oxide surface or the aluminum nitride surface (sidewall 163 of the etch stop layer 150) and the dielectric surface (e.g., SiO2). The organic portion of the boron-containing compound acts as a hydrophobic protective layer that prevents the growth of subsequent dielectric layers (e.g., BN) on the metal, enabling the dielectric to be selectively deposited on the dielectric surface.

[0109] The dielectric surface of the substrate may include any suitable dielectric material. Suitable dielectric materials include, but are not limited to, oxides (e.g., silicon oxide), low-k dielectric materials, and high-k dielectric materials. In some embodiments, the dielectric surface consists essentially of silicon oxide. When used in this manner, the term "consisting essentially of" means that the surface is greater than or equal to about 95%, 98%, or 99% of the material, based on area.

[0110] The metal surface of the substrate may include any suitable metal material. Suitable metal materials include, but are not limited to, metals, metal nitrides, metal alloys, and other conductive materials. In some embodiments, the metal surface includes one or more of cobalt, tungsten, or titanium nitride. In some embodiments, the metal surface consists essentially of cobalt. In some embodiments, the metal surface consists essentially of tungsten. In some embodiments, the metal surface consists essentially of titanium nitride.

[0111] In some embodiments, forming the barrier layer 180 comprises exposing the substrate to a soaking bath of barrier molecules. In some embodiments, forming the barrier layer 180 comprises exposing the substrate to pulses of barrier chemistry. The pulses of barrier chemistry may be of any suitable duration and occur any suitable number of times. In some embodiments, during the formation of the barrier layer 180, the pulses of barrier chemistry are greater than 1, 10, 100, 250, 500, or 1000. In some embodiments, the total exposure time to the barrier chemistry is greater than 1 second, 10 seconds, 100 seconds, 500 seconds, or 1000 seconds.

[0112] In some embodiments, the boron groups are cross-linked to each other after deposition. In some embodiments, the barrier layer contains substantially no cross-links between the boron groups. The term "substantially no cross-links" used in this manner means that there are less than or equal to about 5%, 2%, or 1% cross-links based on the surface area.

[0113] Some embodiments of the present disclosure provide methods for improving the performance of interconnects. The interconnects include metal lines that transmit current within the same component layer and metal vias that transmit current between layers. These lines and vias are formed with conductive metals such as copper or cobalt in gaps formed within the components. In one or more embodiments, the dielectric layer includes at least one feature structure that defines a gap including sidewalls and a bottom. In one or more embodiments, the gap includes metal lines and metal vias. In one or more embodiments, the metal lines have sidewalls and a bottom. In one or more embodiments, the metal vias have sidewalls and a bottom. As used in this specification and the appended claims, unless otherwise stated, reference to the "bottom of the gap" is intended to mean the bottom of the metal via closest to the substrate.

[0114] As technology nodes advance, for example, when shrinking microelectronic components and interconnects to the 3nm node and beyond the back end of line (BEOL), new interfaces such as tungsten (W), molybdenum (Mo), and ruthenium (Ru) are included. Improving the self-assembled monolayer (SAM) selectivity of metals to low-k surfaces becomes more challenging, especially when these interfaces contain different types of impurities such as oxygen, carbon, nitrogen, fluorine, chlorine, etc. It has been determined that pre-cleaning before the SAM process further improves SAM selectivity. Pre-cleaning helps control damage to low-k dielectric materials.

[0115] In some embodiments, the substrate 105 is cleaned before exposing the substrate 105 to the barrier molecules. In some embodiments, only the metal surface of the substrate is cleaned before exposing the substrate to the barrier molecules. In some embodiments, the substrate or the metal surface of the substrate is cleaned with a hydrogen plasma. In some embodiments, the hydrogen plasma is a capacitively coupled plasma (CCP). In some embodiments, the hydrogen plasma is an inductively coupled plasma (ICP). In some embodiments, the hydrogen plasma comprises a plasma of H2. In some embodiments, the hydrogen plasma comprises or consists essentially of a combination of argon (Ar) and hydrogen (H2). In some embodiments, the hydrogen plasma comprises or consists essentially of a combination of helium (He) and hydrogen (H2).

[0116] The barrier layer 180 is formed at a temperature that is favorable for close packing of a self-assembled monolayer of the barrier chemical. In some embodiments, the substrate 105 is maintained at a temperature in the range of 100° C. to 500° C., or in the range of 150° C. to 450° C., or in the range of 200° C. to 400° C., or in the range of 225° C. to 350° C., or in the range of 250° C. to 350° C., or in the range of 250° C. to 300° C.

[0117] Some embodiments of the present disclosure relate to selectively depositing a barrier layer on a dielectric surface relative to a metal surface. A selective barrier layer (e.g., tantalum nitride) can reduce RC delay by >50%. Current processes selectively deposit TaN on copper using known SAMs for the N3 technology node. For next generation components, it is desirable to selectively deposit tantalum nitride on a dielectric surface relative to tungsten metal.

[0118] Embodiments of the present disclosure advantageously provide methods for surface pretreatment, such as selective barrier treatment of metal surfaces (including but not limited to copper, cobalt, tungsten, tantalum, tantalum nitride, tantalum oxide, titanium, titanium oxide, titanium nitride, ruthenium, ruthenium oxide, and iridium, etc.). Some embodiments advantageously provide methods for surface pretreatment of metal surfaces such as silicon oxide (SiO x ), silicon nitride (SiN), silicon oxynitride carbon (SiCON), silicon carbide (SiCO), etc., and a method of selectively growing a barrier material on a dielectric surface.

[0119] Pre-cleaning of the substrate may be performed at any suitable temperature depending on, for example, the cleaning technique. In some embodiments, pre-cleaning of the substrate is performed at a temperature in the range of 200°C to 500°C or in the range of 300°C to 400°C.

[0120] Figure 4 FIG. 1 shows a block layer 190 formed on the surface of the second dielectric layer 160 and the etch stop layer 150. Figure 3 An electronic component 100.

[0121] In some embodiments, barrier layer 190 is a dielectric layer selectively deposited on the dielectric surface after barrier layer 180 is deposited. In some embodiments, barrier layer 190 includes silicon nitride. Silicon nitride can be deposited by any suitable process. In one or more embodiments, barrier layer 190 is formed by an atomic layer deposition (ALD) process. A suitable process may include exposing the substrate to a silicon halide and ammonia. Suitable silicon halides include, but are not limited to, dichlorosilane (DCS), trichlorosilane (TCS), tetrachlorosilane (SiCl4), silicon tetrabromide (SiBr4), tetraiodosilane (SiI4), and hexachlorodisilane (HCDS).

[0122] In some embodiments, barrier layer 190 includes or consists essentially of tantalum nitride (TaN). In some embodiments, tantalum nitride (TaN) is deposited by a thermal atomic layer deposition (ALD) process. When used in this manner, the thermal process does not include a plasma. In some embodiments, penta(dimethylamino)tantalum (PDMAT) and ammonia are used in a thermal ALD process to deposit tantalum nitride.

[0123] In some embodiments, the substrate is repeatedly exposed to barrier molecules after the barrier layer 190 is deposited to regenerate the barrier layer. In some embodiments, the barrier layer 190 is deposited again after the barrier layer is regenerated. In some embodiments, the substrate is repeatedly exposed to barrier molecules and the barrier layer is deposited until the barrier layer reaches a predetermined thickness.

[0124] One or more exposures to surface barrier chemistry or barrier layer regeneration may be performed after a number of deposition cycles or after a predetermined film thickness is formed. In some embodiments, prior to barrier layer 180 regeneration, the barrier layer 180 is exposed to a surface barrier chemistry or barrier layer regeneration at about to about within the range of, or about to about within the range of, or about to about The barrier layer 190 is deposited to a thickness within a range of .

[0125] Some embodiments of barrier layer 190 include or consist essentially of tantalum nitride. In some embodiments, first metal layer 130 includes tungsten, etch stop layer 150 includes one or more of aluminum oxide or aluminum nitride, second dielectric layer 160 includes silicon oxide, and barrier layer 190 includes tantalum nitride.

[0126] In some embodiments, the metal surfaces (first metal layer 130 and bottom surface 164) include tungsten. In some embodiments, the metal surfaces (first metal layer 130 and bottom surface 164) consist essentially of tungsten. In some embodiments, the metal surfaces (first metal layer 130 and bottom surface 164) include cobalt. In some embodiments, the metal surfaces (first metal layer 130 and bottom surface 164) consist essentially of cobalt.

[0127] In some embodiments, after barrier layer 180 is formed on the underlying metal surface (bottom surface 164 of via portion 172), barrier layer 190 is selectively deposited on top surface 161, sidewall 162, lower sidewall 167, bottom surface 168, upper sidewall 169 of second dielectric layer 160 in feature 170, and the surface (sidewall 163) of etch stop layer 150. In other words, barrier layer 190 is deposited on sidewall 162, sidewall 163, and bottom surface 168 of via portion 172 of feature 170, and upper sidewall 169 of trench portion 174. In some embodiments, barrier layer 190 is formed on the sidewall to barrier layer 180 on the metal surface. In some embodiments, due to the presence of barrier layer 180, a small gap is formed between bottom surface 164 of via portion 172 and the bottom edge of barrier layer 190.

[0128] In some embodiments, barrier layer 190 includes tantalum nitride. In some embodiments, barrier layer 190 consists essentially of tantalum nitride. Tantalum nitride can be deposited by any suitable process known to those skilled in the art. In some embodiments, barrier layer 190 includes one or more of tantalum nitride (TaN), titanium nitride (TiN), silicon nitride (SiN), titanium silicon nitride (TiSiN), tantalum silicon nitride (TaSiN), or silicon oxynitride (SiON).

[0129] In the embodiment shown in the figures, barrier layer 190 is formed on sidewalls 162 of via portion 172, lower sidewalls 167, bottom surface 168, and upper sidewalls 169 of trench portion 174 of feature 170. These figures do not show barrier layer 190 material on top surface 161 of second dielectric layer 160. In some embodiments, deposition of barrier layer 190 results in formation of barrier layer 190 on top surface 161 of second dielectric layer 160. Substrate 105 is then processed, such as by chemical mechanical polishing (CMP), to remove barrier layer 190 from top surface 161 of second dielectric layer 160.

[0130] The barrier layer 180 formed on clean substrates including W, Si, SiO2 and Al2O3 surfaces was subjected to a tantalum nitride deposition process at different temperatures. The tantalum nitride layer formed on each surface showed that less than 1000 tantalum nitride layers were formed on the W surface after 1000 deposition cycles. TaN, and formed on the surface of Al2O3, SiO2 and Si In some embodiments, the barrier layer 180 is reformed on the metal surface after less than or equal to 1000, 500, 400, 300, 200, or 100 cycles of TaN deposition.

[0131] In some embodiments, barrier layer 190 is formed as to In some embodiments, when the barrier layer 180 is formed on one or more of the aluminum oxide surface or the aluminum nitride surface and the dielectric surface When tantalum nitride is formed on the metal surface, less than or equal to of tantalum nitride.

[0132] Figure 5 1 shows the bottom surface 164 of the via portion 172 after the barrier layer 180 is removed to expose the via portion 172. Figure 4 In the electronic component 100, the bottom surface 164 of the via portion 172 is the top surface of the first metal layer 130. The barrier layer 180 can be removed by any suitable technique known to those skilled in the art. In some embodiments, removing the barrier layer 180 includes exposing the barrier layer 180 to a plasma. In some embodiments, the plasma is an inductively coupled plasma (ICP). In some embodiments, the plasma is a capacitively coupled plasma (CCP). It has been advantageously found that exposing the barrier layer 180 to a plasma increases the density of the barrier layer 190.

[0133] In some embodiments, removing the barrier layer 180 results in a small gap between the top surface of the first metal layer 130 (the bottom surface 164 of the via portion 172). The gap is negligible and does not affect subsequent processing. In some embodiments, removing the barrier layer 180 results in substantially no gap between the top surface of the first metal layer 130 and the bottom edge of the barrier layer 190.

[0134] Figure 6 The metal liner 192 is deposited on the barrier layer 190. Figure 5electronic components (optional operation 18). In some embodiments, metal liner 192 is selectively deposited on barrier layer 190 by any suitable deposition process described herein. In some embodiments, metal liner 192 includes one or more of ruthenium (Ru), cobalt (Co), molybdenum (Mo), or tantalum (Ta). Metal liner 192 of some embodiments includes or consists essentially of cobalt (Co). In some embodiments, metal liner 192 is formed as to Thickness within the range.

[0135] In some embodiments, metal liner 192 includes cobalt (Co), barrier layer 190 includes tantalum nitride, etch stop layer 150 includes one or more of aluminum oxide or aluminum nitride, second dielectric layer 160 includes silicon oxide, and first metal layer 130 includes tungsten.

[0136] Figure 7 The following diagram shows the structure of the feature 170 after the second metal layer 195 is deposited. Figure 6 In other words, Figure 7 The gap filling process of operation 20 is shown. In some embodiments, a second metal layer 195 is deposited to fill the gap, i.e., the portion of the feature structure 170 that is not defined by the via portion 172 and the groove portion 174. The second metal layer 195 is formed on the top surface of the first metal layer 130 (the bottom surface 164 of the via portion 172). In some embodiments, the second metal layer 195 is formed on the top surface of the metal liner 192. The second metal layer 195 may also be referred to as a "gap filling material". In some embodiments, the gap filling material includes copper (Cu) or cobalt (Co). In some embodiments, the gap filling material includes copper (Cu). In some embodiments, the gap filling material contains cobalt (Co). In some embodiments, the gap filling material consists essentially of copper (Cu). In some embodiments, the gap filling material consists essentially of cobalt (Co).

[0137] In some embodiments, the gap filling material includes copper (Cu), the metal liner 192 includes cobalt (Co), the barrier layer 190 includes tantalum nitride, the etch stop layer 150 includes one or more of aluminum oxide or aluminum nitride, the second dielectric layer 160 includes silicon oxide, the first metal layer 130 includes tungsten, and the second metal layer 195 is formed on the top surface of the first metal layer 130 and on the metal liner 192, and the top surface of the first metal layer 130 is exposed through the via portion 172 of the feature structure 170.

[0138] In an embodiment where the metal liner 192 is not present, a second metal layer 195 is formed on the top surface of the first metal layer 130 exposed by the via portion 172 of the feature structure 170, on the barrier layer 190 on the sidewall 162 of the via portion 172, and on the barrier layer 190 on the lower sidewall 167, bottom surface 168 and upper sidewall 169 of the groove portion 174.

[0139] In some embodiments, a blanket deposition process deposits second metal layer 195 into feature 170 and on top surface 161 of second dielectric layer 160. Second metal layer 195 formed on top surface 161 of second dielectric layer 160 may be removed by any suitable technique, including but not limited to etching and chemical mechanical planarization.

[0140] One or more embodiments of the present disclosure are directed to a non-transitory computer-readable medium including instructions that, when executed by a controller of a processing chamber, cause the processing chamber to perform the operations of method 10. In some embodiments, the non-transitory computer-readable medium includes instructions that, when executed by a controller of the processing chamber, cause the processing chamber to: expose a feature structure extending into a semiconductor substrate to a barrier molecule to form a barrier layer, the feature structure defining a gap including a metal surface, a dielectric surface, and an aluminum oxide surface or an aluminum nitride surface, selectively forming the barrier layer on one of the aluminum oxide surface or the aluminum nitride surface and a metal surface above the dielectric surface (operation 12); selectively depositing the barrier layer on one of the aluminum oxide surface or the aluminum nitride surface and the dielectric surface above the barrier layer (operation 14); removing the barrier layer (operation 16); optionally, selectively depositing a metal liner on the barrier layer (operation 18); and performing a gap filling process (operation 20).

[0141] Spatially relative terms such as "below", "below", "lower", "above", "on", etc. may be used herein to facilitate description of the relationship between an element or feature structure as shown in the figure and another or other elements or features. It should be understood that, in addition to the orientation shown in the figure, spatially relative terms are intended to cover different orientations of the device in use or operation. For example, if the device in the figure is turned over, the elements described as being "below" or "below" other elements or features will be oriented to be "above" other elements or features. Therefore, the exemplary term "below" can include the orientation above and below. The device can be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially relative descriptors used in this article are interpreted accordingly.

[0142] In the context of describing the materials and methods discussed herein (particularly in the context of the following claims), the use of the terms "a" and "an" and "the" and similar indicators should be interpreted as covering the singular and plural, unless otherwise specified herein or clearly contradicted by the context. Unless otherwise specified herein, the description of the numerical range herein is intended only to be used as a shorthand method for individually referring to each individual value falling within the range, and each individual value is incorporated into the specification as if it were individually described herein. All methods described herein can be performed in any suitable order, unless otherwise specified herein or clearly contradicted by the context. The use of any and all examples or exemplary language (e.g., "such as") provided herein is intended only to better illustrate the materials and methods, and is not intended to limit the scope, unless otherwise required. The language in the specification should not be interpreted as indicating that any unclaimed element is necessary for practicing the disclosed materials and methods.

[0143] References throughout the specification to "one embodiment," "certain embodiments," "one or more embodiments," or "an embodiment" mean that at least one embodiment of the present disclosure includes a particular feature, structure, material, or characteristic described in conjunction with the embodiment. Thus, phrases such as "in one or more embodiments," "certain embodiments," "in one embodiment," or "in an embodiment" that appear in various places throughout the specification do not necessarily refer to the same embodiment of the present disclosure. Furthermore, particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.

[0144] Although the disclosure herein has been described with reference to specific embodiments, it should be understood that these embodiments are merely illustrative of the principles and applications of the present disclosure. It will be apparent to those skilled in the art that various modifications and variations may be made to the methods and apparatus of the present disclosure without departing from the spirit and scope of the present disclosure. Therefore, the present disclosure is intended to include modifications and variations within the scope of the appended claims and their equivalents.

Claims

1. A method for forming a microelectronic component, the method include: A feature extending into the semiconductor substrate is exposed to a substrate having the general formula R (3-n) BX n or H 3 B–BH 3 a boron-containing compound, wherein n is 0 to 3, X is hydrogen or methyl, and each R is independently selected from alkyl, aryl, olefin, and alkyne groups having 1 to 22 carbon atoms, to form a barrier layer, wherein the feature structure defines a gap including a metal surface, a dielectric surface, and an aluminum oxide surface or an aluminum nitride surface, and the barrier layer is selectively formed on one of the aluminum oxide surface or the aluminum nitride surface and the metal surface above the dielectric surface; selectively depositing a barrier layer on one of the aluminum oxide surface or the aluminum nitride surface and the dielectric surface over the barrier layer; as well as The barrier layer is removed.

2. The method of claim 1, wherein the boron-containing compound comprises wherein each R is independently selected from alkyl, aryl, alkene and alkyne groups having 1 to 22 carbon atoms.

3. The method of claim 1, wherein the boron-containing compound comprises wherein R is selected from alkyl, aryl, alkene and alkyne groups having 1 to 22 carbon atoms.

4. The method of claim 1, wherein the boron-containing compound comprises 9-borabicyclo[3.3.1]nonane 5. The method of claim 1, wherein the boron-containing compound is carried in an inert gas selected from the group consisting of helium (He), neon (Ne), argon (Ar), and krypton (Kr).

6. The method of claim 1, wherein the metal surface comprises one or more of tungsten (W), molybdenum (Mo), or cobalt (Co).

7. The method of claim 1 wherein the dielectric surface comprises a low-k dielectric material.

8. The method of claim 1, wherein selectively depositing the barrier layer comprises an atomic layer deposition (ALD) process.

9. The method of claim 1, wherein the barrier layer comprises tantalum nitride (TaN).

10. The method of claim 1, further comprising selectively depositing a metal liner on the barrier layer.

11. The method of claim 10, wherein the metal liner comprises one or more of ruthenium (Ru), cobalt (Co), molybdenum (Mo), or tantalum (Ta).

12. The method of claim 1, wherein said removing said barrier layer comprises exposing said barrier layer to plasma.

13. The method of claim 12, wherein the plasma is an inductively coupled plasma (ICP).

14. The method of claim 12, wherein the plasma is a capacitively coupled plasma (CCP).

15. The method of claim 12, wherein exposing the barrier layer to a plasma increases the density of the barrier layer. 16 . The method of claim 1 , further comprising performing a gap-fill process to deposit a gap-fill material within the gap. 17 . The method of claim 16 , wherein the gap-fill material comprises copper (Cu) or cobalt (Co).

18. The method of claim 1, wherein the method reduces the resistance of the via by at least 20% compared to a method that does not include forming a barrier layer, the barrier layer being selectively formed on a metal surface relative to a dielectric surface and an aluminum oxide surface or an aluminum nitride surface.

19. A method of forming a microelectronic component, the method include: Exposing a feature extending into a semiconductor substrate to a barrier molecule comprising formula (I) or formula (II) wherein each R is independently selected from alkyl, aryl, olefin and alkyne groups having 1 to 22 carbon atoms to form a barrier layer, the feature structure defines a gap including a metal surface, a dielectric surface and an aluminum oxide surface or an aluminum nitride surface, and the barrier layer is selectively formed on one of the aluminum oxide surface or the aluminum nitride surface and the metal surface above the dielectric surface; selectively depositing a barrier layer on one of the aluminum oxide surface or the aluminum nitride surface and the dielectric surface over the barrier layer; as well as The barrier layer is removed. 20 . The method of claim 19 , further comprising performing a gap filling process after removing the barrier layer, the gap filling process comprising filling the gap with one or more of copper (Cu) or cobalt (Co).

Citation Information

Cited By

  • Semiconductor structure and manufacturing method thereof

    CN120824280A