Back contact battery and preparation method thereof, photovoltaic module

By setting a first insulating layer with a relatively low solvent mass and a higher second insulating layer on the fine gate electrode of the back contact battery, and using ultrasonic treatment and curing technology, the resistivity caused by excessive solvent in the insulating layer is solved and The leakage problem improves the battery's conductivity and efficiency.

CN118825098BActive Publication Date: 2024-12-03GOLDEN SOLAR (QUANZHOU) NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411297169.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-03
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

Excessive solvent content of existing back contact batteries in the insulating layer slurry results in an increase in the resistivity of the fine gate electrode and the contact resistivity, affecting the battery efficiency and increasing the possibility of leakage.

Method used

The first insulating layer and the second insulating layer are arranged in sequence on the fine gate electrode. The solvent mass percentage of the first insulating layer is smaller than that of the second insulating layer. The structure and performance of the insulating layer are optimized through ultrasonic processing and curing techniques, reducing resistivity and avoiding Quality defects.

Benefits of technology

Effectively reduce the resistivity and contact resistivity of the fine gate electrode, improve conductivity, ensure insulation effect, prevent leakage, and improve battery efficiency and product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825098B_ABST
    Figure CN118825098B_ABST
Patent Text Reader

Abstract

The present invention discloses a back contact battery and a preparation method thereof, and a photovoltaic module, and relates to the technical field of back contact batteries. The back contact battery can effectively reduce the resistivity of the fine grid electrode and the contact resistivity between the fine grid electrode and the conductive film layer, improve the conductive performance of the fine grid electrode, ensure the battery efficiency, avoid quality defects, ensure the insulation effect, prevent leakage, further ensure the battery efficiency, and improve the product yield, by sequentially providing a first insulating layer and a second insulating layer on the fine grid electrode, and the solvent mass percentage of the first insulating layer is less than the solvent mass percentage of the second insulating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of back contact batteries, and in particular relates to a back contact battery and a preparation method thereof, and a photovoltaic module. Background Art

[0002] At present, in the process of making electrodes for back-contact batteries, generally, a low-temperature silver paste fine grid electrode is first set on the conductive film layer, then an insulating ink is printed on the low-temperature silver paste to form an insulating layer, and finally a main grid electrode is set on the insulating layer. Since the low-temperature silver paste achieves conductivity by bonding the conductive particles with a binder, there are a large number of pores in the low-temperature silver paste. In order to improve the printing effect of the insulating layer slurry, a large amount of solvents (such as defoamers, leveling agents, thickeners, diluents, curing agents, etc.) are often added to the insulating layer. However, these solvents will significantly increase the resistivity of the fine grid electrode and the contact resistivity between the fine grid electrode and the conductive film layer, directly affecting the conductive properties of the fine grid electrode, thereby affecting the battery efficiency; and if the solvent content in the insulating layer is directly reduced, the insulating layer will have a large number of quality defects (such as bubbles, pinholes, uneven surface, uneven thickness, etc.), which will directly affect the insulation effect and increase the possibility of leakage, thereby affecting the battery efficiency and product yield.

[0003] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art that the resistivity of the fine gate electrode and the contact resistivity between the fine gate electrode and the conductive film layer are high, the conductive performance of the fine gate electrode is poor, and the battery efficiency is low. A back-contact battery and its preparation method, a photovoltaic module are provided. The back-contact battery effectively reduces the resistivity of the fine gate electrode and the contact resistivity between the fine gate electrode and the conductive film layer, improves the conductive performance of the fine gate electrode, ensures the battery efficiency, avoids quality defects, ensures the insulation effect, prevents leakage, further ensures the battery efficiency, and improves the product yield.

[0005] In order to achieve the above objectives, in a first aspect, the present invention provides a back contact battery, comprising:

[0006] substrate;

[0007] A transparent conductive film layer, wherein the transparent conductive film layer is disposed on the substrate, the transparent conductive film layer comprises a first sub-conductive film layer and a second sub-conductive film layer, and an isolation groove is disposed between the first sub-conductive film layer and the second sub-conductive film layer;

[0008] A fine gate electrode, the fine gate electrode comprising a first sub-electrode and a second sub-electrode, the first sub-electrode being arranged on the first sub-conductive film layer, and the second sub-electrode being arranged on the second sub-conductive film layer;

[0009] A first insulating layer, which is disposed on the first sub-conductive film layer and covers the outside of the first sub-electrode;

[0010] A second insulating layer is disposed on the substrate and covers the first insulating layer and the first sub-conductive film layer and fills the isolation groove, wherein the mass percentage of the solvent in the first insulating layer is less than the mass percentage of the solvent in the second insulating layer;

[0011] The main gate electrode is arranged on the second insulating layer and the second sub-conductive film layer, and covers the outside of the second sub-electrode.

[0012] Preferably, the mass percentage of the solvent in the first insulating layer is less than 8%;

[0013] And / or, the mass percentage of the solvent in the first insulating layer is less than half of the mass percentage of the solvent in the second insulating layer.

[0014] Preferably, the ratio of the width of the first insulating layer to the width of the second insulating layer is 0.1-0.8.

[0015] Preferably, the maximum thickness of the first insulating layer is greater than the thickness of the first sub-electrode.

[0016] Preferably, the ratio of the maximum thickness of the first insulating layer to the thickness of the first sub-electrode is 1.2-2;

[0017] And / or, the thickness of the first sub-electrode is 2 μm-30 μm.

[0018] Preferably, the thickness of the second insulating layer is in the range of 2.4 μm-30 μm.

[0019] In a second aspect, the present invention provides a method for preparing a back-contact battery, which is used to prepare the above-mentioned back-contact battery. The method for preparing the back-contact battery comprises:

[0020] S1. Providing a substrate;

[0021] S2. Depositing a transparent conductive film layer on the back side of the substrate, and then opening an isolation groove on the transparent conductive film layer to form a first sub-conductive film layer and a second sub-conductive film layer;

[0022] S3. forming a first sub-electrode on the first sub-conductive film layer, and forming a second sub-electrode on the second sub-conductive film layer;

[0023] S4. forming a first insulating layer on the first sub-conductive film layer so that the first insulating layer covers the outside of the first sub-electrode;

[0024] S5. forming a second insulating layer on the back side of the substrate so that the second insulating layer covers the first insulating layer and the first sub-conductive film layer and fills the isolation groove, wherein the mass percentage of the solvent in the first insulating layer is less than the mass percentage of the solvent in the second insulating layer;

[0025] S6. Form a main gate electrode on the second insulating layer and the second sub-conductive film layer so that the main gate electrode covers the outside of the second sub-electrode.

[0026] Preferably, S4 includes:

[0027] Printing insulating ink on the first sub-conductive film layer by screen printing to form a first insulating layer;

[0028] The first insulating layer is subjected to ultrasonic treatment to eliminate bubbles generated by printing, wherein the ultrasonic frequency is 10kHz-500kHz;

[0029] The first insulating layer is ultraviolet-cured and / or thermally cured in a curing oven.

[0030] Preferably, the ultrasonic treatment satisfies the following relationship:

[0031] A∝P a ·f b ·t c ·η -d ;

[0032] Wherein, A is the defoaming effect, η is the viscosity of the first insulating layer, P is the processing power, f is the processing frequency, t is the processing time, and a, b, c, and d are the empirical coefficients of the corresponding parameters, respectively.

[0033] Preferably, the viscosity of the first insulating layer is 100 mPa·s-550 mPa·s;

[0034] and / or, processing power of 10W-50000W;

[0035] And / or, the processing time is 0.5s-360s.

[0036] Preferably, S5 includes:

[0037] Printing insulating ink on the substrate by screen printing to form a second insulating layer;

[0038] The second insulating layer is ultraviolet-cured and / or thermally cured in a curing oven.

[0039] Preferably, the second insulating layer is printed with transparent insulating ink;

[0040] And / or, the viscosity of the second insulating layer is 10 mPa·s-150 mPa·s.

[0041] In a third aspect, the present invention provides a photovoltaic module comprising the above-mentioned back contact cell.

[0042] Beneficial effects:

[0043] Through research, it is found that in the process of making electrodes, the solvents in the insulating layer (such as defoamers, leveling agents, thickeners, diluents, curing agents, etc.) will significantly increase the resistivity of the fine grid electrode and the contact resistivity between the fine grid electrode and the conductive film layer, directly affecting the conductive performance of the fine grid electrode, thereby affecting the battery efficiency; and if the solvent content in the insulating layer is directly reduced, the insulating layer will have a large number of quality defects (such as bubbles, pinholes, uneven surface, uneven thickness, etc.), directly affecting the insulation effect, resulting in an increased possibility of leakage, thereby affecting the battery efficiency and product yield. Based on this, further research has been conducted to propose the present invention.

[0044] The back-contact battery provided by the present invention adopts the above-mentioned technical scheme, especially the first insulating layer and the second insulating layer are sequentially arranged on the fine gate electrode, and the solvent mass percentage of the first insulating layer is less than the solvent mass percentage of the second insulating layer, which effectively reduces the resistivity of the fine gate electrode and the contact resistivity between the fine gate electrode and the conductive film layer, improves the conductive performance of the fine gate electrode, ensures the battery efficiency, avoids quality defects, ensures the insulation effect, prevents leakage, further ensures the battery efficiency, and improves the product yield.

[0045] The method for preparing a back-contact battery provided by the present invention is used to prepare the above-mentioned back-contact battery, which can effectively improve the conductive performance, avoid quality defects, and ensure battery efficiency and product yield.

[0046] The photovoltaic module provided by the present invention, including the above-mentioned back contact cell, has relatively good photoelectric conversion efficiency and high photovoltaic power generation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0048] Figure 1 This is a schematic structural diagram of the back contact battery provided by the present invention.

[0049] Description of reference numerals:

[0050] 100 - back contact battery; 110 - substrate; 120 - first sub-conductive film layer; 130 - second sub-conductive film layer; 140 - first sub-electrode; 150 - second sub-electrode; 160 - first insulating layer; 170 - second insulating layer; 180 - main gate electrode; 190 - isolation groove. DETAILED DESCRIPTION

[0051] In the present invention, unless otherwise specified, directional words such as "upper, lower, left, right" are generally understood in conjunction with the directions shown in the drawings and actual applications.

[0052] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0053] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0054] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).

[0055] Please refer to Figure 1In the first aspect, the present invention provides a back-contact battery 100, which effectively reduces the resistivity of the fine gate electrode and the contact resistivity between the fine gate electrode and the conductive film layer, improves the conductive performance of the fine gate electrode, ensures battery efficiency, avoids quality defects, ensures insulation effect, prevents leakage, further ensures battery efficiency, and improves product yield by sequentially arranging a first insulating layer 160 and a second insulating layer 170 on the fine gate electrode, and the solvent mass percentage of the first insulating layer 160 is less than the solvent mass percentage of the second insulating layer 170.

[0056] The back contact cell 100 includes a substrate 110, a transparent conductive film layer, a fine gate electrode, a first insulating layer 160, a second insulating layer 170 and a main gate electrode 180. The transparent conductive film layer includes a first sub-conductive film layer 120 and a second sub-conductive film layer 130, and an isolation groove 190 is provided between the first sub-conductive film layer 120 and the second sub-conductive film layer 130, that is, the first sub-conductive film layer 120 and the second sub-conductive film layer 130 are disconnected. The fine gate electrode includes a first sub-electrode 140 and a second sub-electrode 150, the first sub-electrode 140 is provided on the first sub-conductive film layer 120, and the second sub-electrode 150 is provided on the second sub-conductive film layer 130. The first insulating layer 160 is provided on the first sub-conductive film layer 120 and covers the first sub-electrode 140, and the first insulating layer 160 is used to perform preliminary insulation on the first sub-electrode 140. The second insulating layer 170 is disposed on the substrate 110 and covers the first insulating layer 160 and the first sub-conductive film layer 120, and fills the isolation groove 190. The area of ​​the second insulating layer 170 is larger than the area of ​​the first insulating layer 160. The second insulating layer 170 is used to perform secondary insulation on the first sub-electrode 140 to ensure the insulation effect. The main gate electrode 180 is disposed on the second insulating layer 170 and the second sub-conductive film layer 130, and covers the second sub-electrode 150. The main gate electrode 180 is used to conduct with the second sub-electrode 150. The first insulating layer 160 and the second insulating layer 170 are both used to isolate the main gate electrode 180 from the first sub-electrode 140 to prevent the first sub-electrode 140 from being connected to the second sub-electrode 150 and causing a short circuit.

[0057] Further, the mass percentage of the solvent in the first insulating layer 160 is smaller than the mass percentage of the solvent in the second insulating layer 170 , that is, the solvent content in the second insulating layer 170 is greater than the solvent content in the first insulating layer 160 . Since the first insulating layer 160 covers the outside of the first sub-electrode 140 and is in direct contact with the first sub-electrode 140, and the solvent content of the first insulating layer 160 is relatively low, the influence of the solvent on the resistivity of the first sub-electrode 140 can be effectively reduced, the resistivity of the first sub-electrode 140 is reduced, and the contact resistivity between the first sub-electrode 140 and the first sub-conductive film layer 120 is reduced, so as to ensure the conductivity of the first sub-electrode 140, thereby improving the battery efficiency; at the same time, since the second insulating layer 170 covers the outside of the first insulating layer 160 and is not in direct contact with the first sub-electrode 140, and the solvent content of the second insulating layer 170 is relatively high, the second insulating layer 170 will not have quality defects, has good insulation effect, can prevent leakage, ensure battery efficiency and product yield, and the second insulating layer 170 can make up for the quality defects of the first insulating layer 160 when covering the first insulating layer 160 (the solvent content of the first insulating layer 160 is relatively low, and quality defects are prone to occur), further improving the insulation effect, and ensuring battery efficiency and product yield.

[0058] Preferably, the mass percentage of the solvent in the first insulating layer 160 is less than 8%, more preferably less than 5%. A reasonable mass percentage of the solvent in the first insulating layer 160 can reduce the influence of the solvent on the resistivity and contact resistivity of the silver paste electrode, which is beneficial to reducing the battery Rs and thus improving efficiency.

[0059] Preferably, the mass percentage of the solvent in the first insulating layer 160 is less than half of the mass percentage of the solvent in the second insulating layer 170. A reasonable ratio of the mass percentages of the solvent in the second insulating layer 170 can improve the fluidity of the second insulating layer 170, help reduce printing defects, and ensure the insulation effect of areas outside the coverage area of ​​the first insulating layer 160.

[0060] It should be noted that the fine gate electrode is in a strip shape, that is, the first sub-electrode 140 and the second sub-electrode 150 are both in a strip shape, and their cross-sections are semicircular or semi-elliptical. The thickness of the first sub-electrode 140 is the maximum protruding height of the first sub-electrode 140 in a direction perpendicular to the first sub-conductive film layer 120, and the thickness of the second sub-electrode 150 is the maximum protruding height of the second sub-electrode 150 in a direction perpendicular to the second sub-conductive film layer 130. The first insulating layer 160 is disposed on the first sub-conductive film layer 120 and covers the outside of the first sub-electrode 140. The width direction of the first insulating layer 160 is perpendicular to the length direction of the first sub-electrode 140. The thickness of the first insulating layer 160 is uneven, and the thickness of the first insulating layer 160 first decreases and then increases in its width direction, that is, the thickness of the first insulating layer 160 reaches the minimum in the middle of the first sub-electrode 140 (that is, the maximum protruding height position of the first sub-electrode 140). The second insulating layer 170 is arranged on the substrate 110 and covers the first insulating layer 160 and the first sub-conductive film layer 120. The width direction of the second insulating layer 170 is the same as the width direction of the first insulating layer 160. The thickness of the second insulating layer 170 is uneven. The thickness of the second insulating layer 170 reaches the minimum in the middle of the first sub-electrode 140 (that is, the maximum protruding height position of the first sub-electrode 140).

[0061] Preferably, the ratio of the width of the first insulating layer 160 to the width of the second insulating layer 170 is 0.1-0.8. A reasonable ratio of the width of the first insulating layer 160 to the width of the second insulating layer 170 can minimize the amount of ink used and the coverage area of ​​the first insulating layer 160, which is beneficial to improve defects such as bubbles and pinholes in the first insulating layer 160 through ultrasonic defoaming.

[0062] Preferably, the maximum thickness of the first insulating layer 160 is greater than the thickness of the first sub-electrode 140. Specifically, the ratio of the maximum thickness of the first insulating layer 160 to the thickness of the first sub-electrode 140 is 1.2-2. A reasonable ratio of the maximum thickness of the first insulating layer 160 to the thickness of the first sub-electrode 140 can ensure sufficient effective insulation thickness, which is beneficial to avoid the main gate electrode 180 and the fine gate electrode from generating a short circuit defect due to insufficient effective insulation thickness.

[0063] Preferably, the thickness of the first sub-electrode 140 is 2μm-30μm. A reasonable thickness of the first sub-electrode 140 can reduce the requirement for the thickness of the first insulating layer 160 , which is beneficial to reducing the thickness of the first insulating layer 160 to improve the ultrasonic defoaming effect of the insulating layer and reduce defects in the first insulating layer 160 .

[0064] Preferably, the thickness of the second insulating layer 170 is in the range of 2.4 μm-30 μm. A reasonable thickness of the second insulating layer 170 can ensure the insulation effect of the area not covered by the first insulating layer 160, which is beneficial to ensure the insulation effect of the battery and avoid short circuit.

[0065] It is worth noting that the superimposed combination of the first insulating layer 160 and the second insulating layer 170 is called a total insulating layer. When the total insulating layer covers the first sub-electrode 140, the first sub-electrode 140 is located in the middle of the total insulating layer, and the total insulating layer is high in the middle and low on both sides in the width direction. The thickness of the total insulating layer first increases and then decreases in the width direction, so that the position close to the first sub-electrode 140 (where the first insulating layer 160 and the second insulating layer 170 are simultaneously provided) has sufficient insulating thickness to ensure the insulation effect, and the position far away from the first sub-electrode 140 (where only the second insulating layer 170 is provided) has a thinner insulating thickness to reduce the impact on the subsequent printing of the main grid silver paste.

[0066] Specifically, the thickness of the total insulating layer at a position corresponding to the middle of the first sub-electrode 140 (i.e., the thickness of the middle position of the total insulating layer) is 1.5-2.5 times the thickness of the first sub-electrode 140. A reasonable ratio of the thickness of the middle position of the total insulating layer to the thickness of the first sub-electrode 140 can provide sufficient thickness to avoid the defect of insufficient effective insulation thickness caused by local protrusion of the first sub-electrode 140, which is beneficial to ensuring the insulation effect between the main gate electrode 180 and the fine gate electrode.

[0067] In one embodiment of the present invention, the first sub-electrode 140 is a positive electrode, the second sub-electrode 150 is a negative electrode, and the main gate electrode 180 is used to communicate with the negative electrode to achieve conduction of the negative electrode of the back contact battery 100. In another embodiment of the present invention, the first sub-electrode 140 is a negative electrode, the second sub-electrode 150 is a positive electrode, and the main gate electrode 180 is used to communicate with the positive electrode to achieve conduction of the positive electrode of the back contact battery 100.

[0068] In a second aspect, the present invention provides a method for preparing a back-contact battery 100, which is used to prepare the above-mentioned back-contact battery 100. The method for preparing the back-contact battery 100 comprises:

[0069] S1. Providing a substrate 110;

[0070] S2. A transparent conductive film layer is deposited on the back of the substrate 110, and then an isolation groove 190 is opened on the transparent conductive film layer to form a first sub-conductive film layer 120 and a second sub-conductive film layer 130;

[0071] S3. Forming a first sub-electrode 140 on the first sub-conductive film layer 120 and forming a second sub-electrode 150 on the second sub-conductive film layer 130;

[0072] S4. Forming a first insulating layer 160 on the first sub-conductive film layer 120 so that the first insulating layer 160 covers the outside of the first sub-electrode 140;

[0073] S5. forming a second insulating layer 170 on the back side of the substrate 110 so that the second insulating layer 170 covers the first insulating layer 160 and the first sub-conductive film layer 120 and fills the isolation groove 190, wherein the mass percentage of the solvent in the first insulating layer 160 is less than the mass percentage of the solvent in the second insulating layer 170;

[0074] S6. Forming a main gate electrode 180 on the second insulating layer 170 and the second sub-conductive film layer 130 , so that the main gate electrode 180 covers the outside of the second sub-electrode 150 .

[0075] It should be noted that in S1 , the substrate 110 is a silicon wafer after a semiconductor layer is deposited on the back side.

[0076] In S2, a transparent conductive film layer is first deposited on the back side of the substrate 110 by using physical vapor deposition technology (PVD) or activated plasma deposition technology (RPD), and then an isolation groove 190 is opened on the transparent conductive film layer by laser or etching to form a first sub-conductive film layer 120 and a second sub-conductive film layer 130 that are spaced apart.

[0077] In S3, the first sub-electrode 140 is formed on the first sub-conductive film layer 120 by screen printing, and the second sub-electrode 150 is formed on the second sub-conductive film layer 130 by printing. Since there is an isolation groove 190 between the first sub-conductive film layer 120 and the second sub-conductive film layer 130, the first sub-electrode 140 and the second sub-electrode 150 are in a separated state.

[0078] S4 consists of three stages:

[0079] Stage 1: Print insulating ink on the first sub-conductive film layer 120 by screen printing to form a first insulating layer 160. Preferably, in the first stage, the first insulating layer 160 is printed by UV insulating ink, and the first insulating layer 160 covers the first sub-electrode 140 to perform preliminary insulation on the first sub-electrode 140.

[0080] The second stage: ultrasonic treatment is performed on the first insulating layer 160 to eliminate bubbles generated by printing, wherein the ultrasonic frequency is 10kHz-500kHz. Specifically, in the second stage, the first insulating layer 160 before surface drying is ultrasonically treated. By ultrasonically treating the first insulating layer 160 with a low solvent content, it is possible to significantly reduce defects such as bubbles in the first insulating layer 160, reduce the contact probability between the second insulating layer 170 and the first sub-electrode 140, ensure the insulation effect, improve the battery efficiency, and reduce the influence of the solvent in the first insulating layer 160 on the resistivity of the first sub-electrode 140 and the contact resistivity between the first sub-electrode 140 and the first sub-conductive film layer 120, thereby improving the conductivity of the first sub-electrode 140.

[0081] Furthermore, ultrasonic treatment satisfies the following relationship: A∝P a ·f b ·t c ·η -d ;

[0082] Wherein, A is the defoaming effect, η is the viscosity of the first insulating layer 160, P is the processing power, f is the processing frequency, t is the processing time, and a, b, c, and d are respectively the empirical coefficients of the corresponding parameters.

[0083] Specifically, when the defoamer type is an acrylate-modified non-silicone defoamer and the content is 2%, the empirical coefficients are a=1.83, b=0.72, c=1.28, and d=3.52.

[0084] Preferably, the viscosity of the first insulating layer 160 is 100mPa·s-550mPa·s; and / or, the processing power is 10W-50000W; and / or, the processing time is 0.5s-360s. Reasonable viscosity, processing power and processing time of the first insulating layer 160 can control defects such as bubbles, pinholes, unevenness, uneven thickness, etc. of the first insulating layer 160, which is conducive to ensuring a good insulation effect between the fine gate electrode and the main gate electrode 180.

[0085] The third stage: UV curing and / or thermal curing of the first insulating layer 160 in a curing furnace. Furthermore, in the third stage, the first insulating layer 160 is cured by UV curing, thermal curing, or a combination of UV curing and thermal curing according to actual conditions to ensure the curing effect.

[0086] S5 consists of two stages:

[0087] Stage 1: Print insulating ink on the substrate 110 by screen printing to form a second insulating layer 170. Preferably, in the first stage, the second insulating layer 170 is printed with transparent insulating ink, and the second insulating layer 170 covers the first insulating layer 160 and the first sub-conductive film layer 120 and fills the isolation groove 190. The second insulating layer 170 is used to perform secondary insulation on the first sub-electrode 140.

[0088] Furthermore, when the thickness of the second insulating layer 170 is 15 μm, its transmittance is greater than or equal to 80%, which can increase the bifaciality of the back contact battery 100 to a certain extent, thereby improving the battery power generation efficiency. The viscosity of the second insulating layer 170 is 10 mPa·s-150 mPa·s. A reasonable viscosity of the second insulating layer 170 can optimize the thickness and defects of the second insulating layer 170, which is conducive to ensuring a good insulation effect between the transparent conductive layer and the main grid electrode 180.

[0089] Second stage: UV curing and / or thermal curing of the second insulating layer 170 in a curing furnace. Furthermore, in the second stage, the first insulating layer 160 is cured by UV curing, thermal curing, or a combination of UV curing and thermal curing according to actual conditions to ensure the curing effect.

[0090] In one embodiment of the present invention, only the first insulating layer 160 is subjected to ultrasonic treatment, and the second insulating layer 170 is not subjected to ultrasonic treatment. In another embodiment of the present invention, both the first insulating layer 160 and the second insulating layer 170 are subjected to ultrasonic treatment.

[0091] In S6 , a main gate electrode 180 is formed on the second insulating layer 170 and the second sub-conductive film layer 130 by screen printing, so that the main gate electrode 180 covers the second sub-electrode 150 , wherein the main gate electrode 180 has the same polarity as the second sub-electrode 150 .

[0092] In a third aspect, the present invention provides a photovoltaic module, which includes the above-mentioned back contact cell 100.

[0093] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0094] Example 1

[0095] A back contact battery 100 is prepared by the following steps:

[0096] S1. A substrate 110 is provided.

[0097] S2. A transparent conductive film layer is first deposited on the back of the substrate 110 by physical vapor deposition (PVD), and then an isolation groove 190 is opened on the transparent conductive film layer by etching to form a first sub-conductive film layer 120 and a second sub-conductive film layer 130 that are spaced apart.

[0098] S3. By screen printing, a first sub-electrode 140 is formed on the first sub-conductive film layer 120 , and a second sub-electrode 150 is formed on the second sub-conductive film layer 130 , wherein the thickness of the first sub-electrode 140 is 10 μm.

[0099] S4. First, the first insulating layer 160 is formed by screen printing; then, the first insulating layer 160 is subjected to ultrasonic treatment, during which the ultrasonic frequency is 30 kHz, the viscosity of the first insulating layer 160 is 220 mPa·s, the treatment power is 2700 W, and the treatment time is 30 seconds; then, the first insulating layer 160 is UV-cured by a curing furnace. The mass percentage of the solvent in the first insulating layer 160 is 2%.

[0100] S5. First, the second insulating layer 170 is formed by screen printing, and then the second insulating layer 170 is UV-cured in a curing furnace. The mass percentage of the solvent in the second insulating layer 170 is 8%, and the viscosity of the second insulating layer 170 is 80 mPa·s.

[0101] S6. Form a main gate electrode 180 on the second insulating layer 170 and the second sub-conductive film layer 130 by screen printing.

[0102] Example 2

[0103] The method of Example 1 is referred to, except that the mass percentage of the solvent in the first insulating layer 160 is adjusted to 5%, and the mass percentage of the solvent in the second insulating layer 170 is adjusted to 12%.

[0104] Example 3

[0105] The method of Example 1 is referred to, except that the mass percentage of the solvent in the first insulating layer 160 is adjusted to 7%, and the mass percentage of the solvent in the second insulating layer 170 is adjusted to 15%.

[0106] Example 4

[0107] The method of Example 1 is referred to, except that the ultrasonic treatment parameters are adjusted so that the ultrasonic frequency is 80 kHz, the viscosity of the first insulating layer 160 is 100 mPa·s, the treatment power is 1000 W, and the treatment time is 0.5 s.

[0108] Example 5

[0109] The method of Example 1 is referred to, except that the viscosity of the second insulating layer 170 is adjusted to 10 mPa·s.

[0110] Comparative Example 1

[0111] The method of Example 1 is referred to, except that the mass percentage of the solvent in the first insulating layer 160 is adjusted to 10%, and the mass percentage of the solvent in the second insulating layer 170 is adjusted to 6%.

[0112] Comparative Example 2

[0113] The method of Example 1 is referred to, except that the mass percentage of the solvent in the first insulating layer 160 is adjusted to 10%, and the mass percentage of the solvent in the second insulating layer 170 is adjusted to 22%.

[0114] Comparative Example 3

[0115] The method of Example 1 is referred to, except that the ultrasonic treatment parameters are adjusted so that the ultrasonic frequency is 40 kHz, the viscosity of the first insulating layer 160 is 500 mPa·s, the treatment power is 8000 W, and the treatment time is 100 s.

[0116] Comparative Example 4

[0117] The method of Example 1 is referred to, except that the viscosity of the second insulating layer 170 is adjusted to 300 mPa·s.

[0118] Test Case

[0119] The back contact cells 100 obtained in the above-mentioned embodiments and comparative examples were subjected to performance tests, and the results are shown in the following performance index comparison table.

[0120] Performance index comparison table:

[0121]

[0122] It can be seen from the above performance index comparison table that, relative to the comparative example, by adopting the embodiment scheme of the present invention, by sequentially arranging the first insulating layer 160 and the second insulating layer 170 on the fine gate electrode, and the solvent mass percentage of the first insulating layer 160 is less than the solvent mass percentage of the second insulating layer 170, the resistivity of the fine gate electrode and the contact resistivity of the fine gate electrode and the conductive film layer are effectively reduced, the conductive performance of the fine gate electrode is improved, the battery efficiency is guaranteed, and quality defects are avoided, the insulation effect is guaranteed, leakage is prevented, the battery efficiency is further guaranteed, and the product yield is improved.

[0123] Furthermore, according to Example 1 and Examples 2-5, it can be seen that the preferred battery structure of the present invention is more conducive to reducing resistivity, improving conductivity, and ensuring battery efficiency.

[0124] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A back contact battery, characterized in that: include: substrate; A transparent conductive film layer, wherein the transparent conductive film layer is disposed on the substrate, the transparent conductive film layer comprises a first sub-conductive film layer and a second sub-conductive film layer, and an isolation groove is disposed between the first sub-conductive film layer and the second sub-conductive film layer; A fine gate electrode, the fine gate electrode comprising a first sub-electrode and a second sub-electrode, the first sub-electrode being disposed on the first sub-conductive film layer, and the second sub-electrode being disposed on the second sub-conductive film layer; A first insulating layer, wherein the first insulating layer is disposed on the first sub-conductive film layer and covers the outside of the first sub-electrode; a second insulating layer, the second insulating layer being disposed on the substrate and covering the first insulating layer and the first sub-conductive film layer and filling the isolation groove, wherein the mass percentage of the solvent in the first insulating layer is less than the mass percentage of the solvent in the second insulating layer, and the mass percentage of the solvent in the first insulating layer is less than 8%; A main gate electrode is arranged on the second insulating layer and the second sub-conductive film layer, and covers the outside of the second sub-electrode.

2. The back contact cell according to claim 1, characterized in that: The mass percentage of the solvent in the first insulating layer is less than half of the mass percentage of the solvent in the second insulating layer.

3. The back contact cell according to claim 1, characterized in that: The ratio of the width of the first insulating layer to the width of the second insulating layer is 0.1-0.

8.

4. The back contact cell according to claim 1, characterized in that: The maximum thickness of the first insulating layer is greater than the thickness of the first sub-electrode.

5. The back contact cell according to claim 4, characterized in that: The ratio of the maximum thickness of the first insulating layer to the thickness of the first sub-electrode is 1.2-2; And / or, the thickness of the first sub-electrode is 2 μm-30 μm.

6. The back contact cell according to claim 1, characterized in that: The thickness of the second insulating layer is in the range of 2.4 μm to 30 μm.

7. A method for preparing a back contact battery, characterized in that: Used to prepare a back contact battery as claimed in any one of claims 1 to 6, the preparation method of the back contact battery comprising: S1. Providing a substrate; S2. Depositing a transparent conductive film layer on the back side of the substrate, and then opening an isolation groove on the transparent conductive film layer to form a first sub-conductive film layer and a second sub-conductive film layer; S3. forming a first sub-electrode on the first sub-conductive film layer, and forming a second sub-electrode on the second sub-conductive film layer; S4. forming a first insulating layer on the first sub-conductive film layer so that the first insulating layer covers the outside of the first sub-electrode; S5. forming a second insulating layer on the back side of the substrate so that the second insulating layer covers the first insulating layer and the first sub-conductive film layer and fills the isolation groove, wherein the mass percentage of the solvent in the first insulating layer is less than the mass percentage of the solvent in the second insulating layer; S6. Form a main gate electrode on the second insulating layer and the second sub-conductive film layer so that the main gate electrode covers the outside of the second sub-electrode.

8. The method for preparing a back contact battery according to claim 7, characterized in that: S4 includes: Printing insulating ink on the first sub-conductive film layer by screen printing to form the first insulating layer; Performing ultrasonic treatment on the first insulating layer to eliminate bubbles generated by printing, wherein the ultrasonic frequency is 10kHz-500kHz; The first insulating layer is ultraviolet-cured and / or thermally cured in a curing oven.

9. The method for preparing a back contact battery according to claim 8, characterized in that: Ultrasonic treatment satisfies the following relationship: A∝P a ·f b ·t c ·or -d ; In the formula, A is the defoaming effect, η is the viscosity of the first insulating layer, P is the processing power, f is the processing frequency, t is the processing time, and a, b, c, and d are the empirical coefficients of the corresponding parameters, respectively.

10. The method for preparing a back contact battery according to claim 9, characterized in that: The viscosity of the first insulating layer is 100 mPa·s-550 mPa·s; and / or, processing power of 10W-50000W; And / or, the processing time is 0.5s-360s.

11. The method for preparing a back contact battery according to claim 7, characterized in that: S5 includes: Printing insulating ink on the substrate by screen printing to form the second insulating layer; The second insulating layer is ultraviolet-cured and / or thermally cured in a curing oven.

12. The method for preparing a back contact battery according to claim 11, characterized in that: The second insulating layer is printed by transparent insulating ink; And / or, the viscosity of the second insulating layer is 10 mPa·s-150 mPa·s.

13. A photovoltaic module, characterized in that: Comprising a back contact battery as described in any one of claims 1-6.

Citation Information

Patent Citations

  • Back-contact heterojunction solar cell adopting composite insulating film layer and manufacturing method of back-contact heterojunction solar cell