Back contact heterojunction solar cell and preparation method thereof, and battery assembly

By preparing the oxide layer and the second intrinsic polysilicon layer in the back-contact heterojunction solar cell and performing carbon and phosphorus doping treatment, the parasitic absorption and structural stability of the polysilicon is solved, and the short-circuit current and current density of the battery are improved , achieving more efficient photoelectric conversion.

CN118825103BActive Publication Date: 2024-11-19GOLDEN SOLAR (QUANZHOU) NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411297183.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-19
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

The existing back contact heterojunction solar cells have severely affected the battery short-circuit current due to parasitic absorption of polycrystalline silicon. In the prior art, there are dielectric barriers to deposit polycrystalline silicon stacks with different refractive indices, and thin-layer polycrystalline silicon is difficult to withstand high-energy hydrogen bombardment, resulting in structural damage.

Method used

The oxide layer and the second intrinsic polysilicon layer are prepared in sequence on the front of the silicon wafer, and carbon and phosphorus doping are performed to form a doped structural film layer with gradient concentration. The gradient doping of carbon and phosphorus is achieved through tube PECVD to reduce the Optical loss and carrier recombination improve the passivation level and protect the polysilicon layer from hydrogen treatment by a highly carbon doped layer.

Benefits of technology

The parasitic absorption of polysilicon is reduced, the short-circuit current and current density of the battery is improved, the photoelectric conversion efficiency is improved, and the stability of the polysilicon layer and the oxide layer is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825103B_ABST
    Figure CN118825103B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of solar cells, and specifically provides a back-contact heterojunction solar cell and a preparation method thereof, and a cell assembly. An oxide layer and a second intrinsic polysilicon layer are sequentially prepared on the front side of a silicon wafer, and the second intrinsic polysilicon layer is subjected to carbon-doping and phosphorus-doping treatments, so as to prepare a concentration-gradient doping structure film layer, wherein the doping concentration decreases exponentially from the surface layer to the bottom layer, the linear gradient carbon doping can help reduce optical loss, the linear gradient phosphorus doping can help reduce carrier recombination, and improve the passivation level, and the presence of a high-concentration carbon-doped layer on the surface layer helps to resist the bombardment of subsequent hydrogen treatment, thereby reducing the parasitic absorption of polysilicon, and is beneficial to increasing the short-circuit current of the battery, thereby improving the current density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solar cells, and in particular relates to a back-contact heterojunction solar cell and a preparation method and a cell assembly thereof. Background Art

[0002] When the existing back-contact heterojunction solar cell uses a tunneling oxide layer + N-type polysilicon structure on the front, the short-circuit current of the battery is seriously affected due to the serious parasitic absorption of polysilicon. In the prior art, in order to reduce the parasitic absorption of polysilicon, the prior art mainly achieves this by depositing polysilicon stacks with different refractive indices and thinning the thickness of polysilicon. The deposition of polysilicon stacks with different refractive indices usually uses in-situ doping of carbon or oxygen. The polysilicon stacks prepared by this method have dielectric barriers in different film layers, which will affect the propagation of light; because the tunneling polysilicon structure needs to be hydrogen treated to improve the passivation level, the thinner polysilicon cannot withstand the bombardment of high-energy hydrogen, which can easily damage the polysilicon layer and the oxide layer.

[0003] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0004] The purpose of the present invention is to overcome the technical problem that the short-circuit current of the existing back-contact heterojunction solar cell is seriously affected by the parasitic absorption of polycrystalline silicon.

[0005] In order to achieve the above-mentioned object, in a first aspect, a back-contact heterojunction solar cell is provided, comprising: a silicon wafer having a front side and a back side, a first semiconductor layer, a second semiconductor layer and a third semiconductor layer;

[0006] A first semiconductor layer is arranged on the back side of the silicon wafer, the first semiconductor layer comprises a tunneling silicon oxide layer and an N-type doped polysilicon layer sequentially formed on the silicon wafer, the N-type doped polysilicon layer comprises a first intrinsic polysilicon layer and a phosphorus-doped polysilicon layer;

[0007] The first semiconductor layer is separated by a plurality of second semiconductor opening regions, the second semiconductor opening regions and the surface of the first semiconductor layer around the second semiconductor opening regions are covered with a second semiconductor layer, the second semiconductor layer is composed of an intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer or a P-type doped microcrystalline silicon layer; a first semiconductor opening region is provided between adjacent second semiconductor opening regions, and the first semiconductor opening region separates the second semiconductor layer;

[0008] The third semiconductor layer includes an oxide layer and a second intrinsic polysilicon layer stacked in sequence on the front side of the silicon wafer; the side of the second intrinsic polysilicon layer close to the oxide layer is the bottom layer, and the side away from the oxide layer is the surface layer; wherein the total phosphorus doping concentration of the second intrinsic polysilicon layer is 1e19cm -3 ~5e19cm -3 The total carbon doping concentration of the second intrinsic polysilicon layer is 1e20cm -3 ~8e20cm -3 The surface phosphorus doping concentration of the second intrinsic polysilicon layer is 2e21cm -3 ~8e21cm -3 , the surface carbon doping concentration is 3e22cm -3 ~8e22cm -3 The bottom phosphorus doping concentration of the second intrinsic polysilicon layer is 3e17cm -3 ~6e17cm -3 , bottom carbon doping concentration 2e18cm -3 ~5e18cm -3 , and the phosphorus doping concentration and carbon doping concentration change linearly from the surface to the bottom layer.

[0009] Optionally, the phosphorus doping concentration of the second intrinsic polysilicon layer changes linearly from the surface layer to the bottom layer with a gradient slope of 1.3e19-8e20, and the carbon doping concentration changes linearly from the surface layer to the bottom layer with a gradient slope of 2e21-8e21.

[0010] Optionally, the oxide layer has a thickness of 2-4 nm, the second intrinsic polysilicon layer has a thickness of 10-15 nm, the surface layer of the second intrinsic polysilicon layer has a thickness of 2-4 nm, and the bottom layer of the second intrinsic polysilicon has a thickness of 1-2 nm.

[0011] Optionally, the back-contact heterojunction solar cell further includes: an anti-reflection layer; the anti-reflection layer is arranged on a side of the second intrinsic polysilicon layer away from the silicon wafer; and the thickness of the anti-reflection layer is 80 nm to 100 nm.

[0012] Optionally, the anti-reflection layer is composed of a first silicon nitride anti-reflection layer, a second silicon nitride anti-reflection layer, a first silicon oxynitride anti-reflection layer, a second silicon oxynitride anti-reflection layer and a silicon oxide layer in sequence; wherein the thickness of the first silicon nitride anti-reflection layer is 20nm~30nm, the thickness of the second silicon nitride anti-reflection layer is 15nm~25nm; the thickness of the first silicon oxynitride anti-reflection layer is 10nm~20nm; the thickness of the second silicon oxynitride anti-reflection layer is 10nm~20nm; the thickness of the silicon oxide layer is 25nm~40nm.

[0013] Optionally, a textured surface is formed on the front side of the silicon wafer and the surface of the silicon wafer located in the second semiconductor opening area, and the second semiconductor layer and the third semiconductor layer fill the textured surfaces in corresponding areas respectively.

[0014] Optionally, the thickness of the intrinsic amorphous silicon layer is 5nm-15nm, the thickness of the P-type doped amorphous silicon layer or the P-type doped microcrystalline silicon layer is 10nm-35nm, and the boron doping concentration in the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer is 1e19cm -3 ~4e20cm -3 .

[0015] Optionally, the back-contact heterojunction solar cell further includes: an isolation groove; the isolation groove is located between the adjacent first semiconductor opening region and the second semiconductor opening region; the first semiconductor opening region and the second semiconductor layer are both covered with a transparent conductive film layer, and the isolation groove separates the transparent conductive film layer located in the first semiconductor opening region from the transparent conductive film layer located on the second semiconductor layer.

[0016] Optionally, the width of the first semiconductor opening region is 0.1 mm to 0.3 mm; the width of the second semiconductor opening region is 0.3 mm to 0.6 mm; and / or the width of the isolation trench is 30 um to 200 um.

[0017] In a second aspect, an embodiment of the present invention further provides a method for preparing a back-contact heterojunction solar cell, which is used to prepare the back-contact heterojunction solar cell as described in the first aspect, and the method for preparing the back-contact heterojunction solar cell comprises the following steps:

[0018] S01, providing a silicon wafer;

[0019] S02, sequentially preparing a tunneling silicon oxide layer and an N-type doped polysilicon layer on the back side of the silicon wafer to obtain a first semiconductor layer; the N-type doped polysilicon layer is composed of a first intrinsic polysilicon layer and a phosphorus-doped polysilicon layer;

[0020] S03, preparing a mask layer on the surface of the first semiconductor layer;

[0021] S04, removing a portion of the mask layer and a corresponding portion of the first semiconductor layer to form alternately arranged second semiconductor opening regions;

[0022] S05, removing the remaining mask layer, N-type doped polycrystalline layer and tunneling silicon oxide layer in the second semiconductor opening region by texturing and cleaning, and forming a texture surface on the front side of the silicon wafer and the surface of the silicon wafer located in the second semiconductor opening region, and then removing the mask layer on the back side of the silicon wafer outside the second semiconductor opening region;

[0023] S06, sequentially preparing an oxide layer and a second intrinsic polysilicon layer on the front side of the silicon wafer;

[0024] S07, doping the second intrinsic polysilicon layer with carbon and phosphorus to obtain a third semiconductor layer, and performing hydrogen treatment and depositing an anti-reflection layer; wherein the total doping concentration of phosphorus in the second intrinsic polysilicon layer is 1e19cm -3 ~5e19cm -3 The total carbon doping concentration of the second intrinsic polysilicon layer is 1e20cm -3 ~8e20cm -3 The surface phosphorus doping concentration of the second intrinsic polysilicon layer is 2e21cm -3 ~8e21cm -3 , the surface carbon doping concentration is 3e22cm -3 ~8e22cm -3 The bottom phosphorus doping concentration of the second intrinsic polysilicon layer is 3e17cm -3 ~6e17cm -3 , bottom carbon doping concentration 2e18cm -3 ~5e18cm -3 , and the phosphorus doping concentration and carbon doping concentration change linearly from the surface to the bottom layer;

[0025] S08, depositing a second semiconductor layer on the back side of the silicon wafer obtained in step S07, wherein the second semiconductor layer is composed of an intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer or a P-type doped microcrystalline silicon layer;

[0026] S09, etching an opening on the back side of the silicon wafer obtained in step S08 to form a first semiconductor opening region spaced apart from the second semiconductor opening region.

[0027] Optionally, after step S09, the method further includes:

[0028] S10, cleaning and removing the second semiconductor layer remaining in the first semiconductor opening region, and then depositing a transparent conductive film layer on the back side of the obtained silicon wafer;

[0029] S11, making an opening on the transparent conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove;

[0030] S12, forming a first electrode on the transparent conductive film layer in the first semiconductor opening region, and correspondingly forming a second electrode on the transparent conductive film layer in the second semiconductor opening region.

[0031] In a third aspect, an embodiment of the present invention further provides a battery assembly, which includes the back-contact heterojunction solar cell as described in the first aspect.

[0032] The present invention has at least the following beneficial effects:

[0033] The present invention prepares an oxide layer and a second intrinsic polysilicon layer on the front side of a silicon wafer in sequence, and performs carbon doping and phosphorus doping treatment on the second intrinsic polysilicon layer, thereby preparing a doped structure film layer with a concentration gradient, wherein the doping concentration decreases exponentially from the surface layer to the bottom layer, wherein the total doping concentration of phosphorus is 1e19~5e19cm -3 , the total carbon doping concentration is 1e20~8e20cm -3 , the bottom phosphorus doping concentration is 3e17~6e17cm -3 , bottom carbon doping concentration 2e18~5e18cm -3 , the surface phosphorus doping concentration is 2e21~8e21cm -3 , surface carbon doping concentration 3e22~8e22cm -3 Linear gradient carbon doping can help reduce optical losses, linear gradient phosphorus doping can help reduce carrier recombination and improve the passivation level, and the presence of a high-concentration carbon-doped layer on the surface can help resist the bombardment of subsequent hydrogen treatment, thereby reducing the parasitic absorption of polysilicon and increasing the short-circuit current of the battery, thereby increasing the current density.

[0034] Furthermore, unlike the prior art which in-situ doped and deposited polysilicon film layers with different refractive indices, the present invention uses tubular PECVD to treat intrinsic polysilicon with methane and phosphine to achieve gradual doping of carbon and phosphorus, and ultimately achieve the effect of a polysilicon film layer with a gradual refractive index, thereby improving the dielectric barrier existing between film layers with different refractive indices in the prior art and reducing optical losses. On the other hand, through the doping method used in the present invention, a highly doped area of ​​carbon can be formed on the surface of the polysilicon film, which can protect the polysilicon layer and the oxide layer from damage caused by PECVD bombardment, and is more conducive to improving the passivation level. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0036] Figure 1 It is a schematic diagram of the internal structure of a back-contact heterojunction solar cell provided in an embodiment of the present invention.

[0037] Figure 2 A process flow chart of a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0038] Figure 3A process flow chart of another method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0039] Figure 4 A process structure diagram corresponding to step S01 in a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0040] Figure 5 A process structure diagram corresponding to steps S02 to S04 in a method for preparing a back-contact heterojunction solar cell provided in an embodiment of the present invention;

[0041] Figure 6 A process structure diagram corresponding to steps S05 and S06 in a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0042] Figure 7 A process structure diagram corresponding to step S07 in a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0043] Figure 8 A process structure diagram corresponding to steps S08 and S09 in a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0044] Fig. 9 A process structure diagram corresponding to step S10 in a method for preparing a back-contact heterojunction solar cell provided by an embodiment of the present invention;

[0045] Fig.10 A process structure diagram corresponding to steps S11 and S12 in a method for preparing a back-contact heterojunction solar cell provided in an embodiment of the present invention.

[0046] Description of Reference Numerals

[0047] 1. Silicon wafer, 2. Tunneling silicon oxide layer, 3. N-type doped polysilicon layer, 4. Mask layer, 5. Oxide layer, 6. Second intrinsic polysilicon layer, 7. Anti-reflection layer, 8. Intrinsic amorphous silicon layer, 9. P-type doped amorphous silicon layer or P-type doped microcrystalline silicon layer; 10. Transparent conductive film layer. DETAILED DESCRIPTION

[0048] In the present invention, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0049] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0050] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0051] First, as Figure 1 As shown, an embodiment of the present invention provides a back-contact heterojunction solar cell, comprising: a silicon wafer 1 having a front side and a back side, a first semiconductor layer, a second semiconductor layer and a third semiconductor layer; wherein the front side refers to the light-receiving surface of the silicon wafer 1, and the back side is the opposite back side of the light-receiving surface. In the embodiment of the present invention, the area close to the silicon wafer 1 is usually considered as the inside, and the area far from the silicon wafer 1 is considered as the outside.

[0052] Specifically, the first semiconductor layer is arranged on the back side of the silicon wafer 1, and the first semiconductor layer includes a tunneling silicon oxide layer 2 and an N-type doped polysilicon layer 3, wherein the tunneling silicon oxide layer 2 is closer to the back side of the silicon wafer 1 than the N-type doped polysilicon layer 3. The N-type doped polysilicon layer 3 is composed of a first intrinsic polysilicon layer and a phosphorus-doped polysilicon layer, and the first intrinsic polysilicon layer is closer to the back side of the silicon wafer 1 than the phosphorus-doped polysilicon layer.

[0053] In the embodiment of the present invention, a plurality of openings are formed on the first semiconductor layer by an etching process, thereby obtaining a second semiconductor opening region W2, that is, the first semiconductor layer is separated by a plurality of second semiconductor opening regions W2. The second semiconductor layer covers the second semiconductor opening region W2 (including the sidewalls of the second semiconductor opening region W2) and the surface of the first semiconductor layer around the second semiconductor opening region W2. A first semiconductor opening region W1 is provided between adjacent second semiconductor opening regions W2, and the first semiconductor opening region W1 separates the second semiconductor layer. Optionally, the second semiconductor layer is composed of an intrinsic amorphous silicon layer 8 and a P-type doped amorphous silicon layer or a P-type doped microcrystalline silicon layer 9, and the intrinsic amorphous silicon layer 8 is closer to the back side of the silicon wafer 1 than the P-type doped amorphous silicon layer or the P-type doped microcrystalline silicon layer 9. Optionally, the thickness of the intrinsic amorphous silicon layer 8 is 5nm~15nm, the thickness of the P-type doped amorphous silicon layer or the P-type doped microcrystalline silicon layer is 10nm~35nm, and the boron doping concentration in the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer is 1e19 cm -3 ~4e20 cm -3 .

[0054] The third semiconductor layer is arranged on the front side of the silicon wafer 1. The third semiconductor layer includes an oxide layer 5 and a second intrinsic polysilicon layer 6 stacked on the front side of the silicon wafer 1; the second intrinsic polysilicon layer is formed on the oxide layer 5. For the convenience of description, the side of the second intrinsic polysilicon layer 6 close to the oxide layer 5 is defined as the bottom layer, and the side of the second intrinsic polysilicon layer 6 away from the oxide layer 5 is defined as the surface layer. Since the doping concentration is gradually distributed, the surface layer and the bottom layer described in this embodiment are only to show the highest doping and the lowest doping gradient of the gradually doped, and there is no obvious boundary distinction between the surface layer and the bottom layer. Among them, the total phosphorus doping concentration of the second intrinsic polysilicon layer is 1e19cm -3 ~5e19 cm -3 The total carbon doping concentration of the second intrinsic polysilicon layer is 1e20cm -3 ~8e20cm -3 The surface phosphorus doping concentration of the second intrinsic polysilicon layer is 2e21cm -3 ~8e21cm -3 , the surface carbon doping concentration is 3e22cm -3 ~8e22cm -3 The bottom phosphorus doping concentration of the second intrinsic polysilicon layer is 3e17cm -3 ~6e17cm -3 , bottom carbon doping concentration 2e18cm -3 ~5e18cm -3 , and the phosphorus doping concentration and carbon doping concentration change linearly from the surface to the bottom layer.

[0055] Optionally, the phosphorus doping concentration of the second intrinsic polysilicon layer changes linearly from the surface layer to the bottom layer with a gradient slope of 1.3e18-8e19. The carbon doping concentration changes linearly from the surface layer to the bottom layer with a gradient slope of 2e20-8e20. Such a gradient slope setting can effectively reduce optical loss and minimize the impact of PECVD hydrogen ion bombardment.

[0056] Optionally, the surface thickness of the second intrinsic polysilicon layer is 10-15 nm, and the bottom thickness of the second intrinsic polysilicon layer is 5-10 nm. Such thickness setting can effectively reduce optical loss.

[0057] Optionally, the width of the first semiconductor opening region W1 is 0.1 mm to 0.3 mm; the width of the second semiconductor opening region W2 is 0.3 mm to 0.6 mm.

[0058] In the embodiment of the present invention, an oxide layer and a second intrinsic polysilicon layer are sequentially prepared on the front side of the silicon wafer, and the second intrinsic polysilicon layer is subjected to carbon doping and phosphorus doping treatment, so as to prepare a doping structure film layer with a gradient concentration, wherein the doping concentration decreases exponentially from the surface layer to the bottom layer, wherein the total doping concentration of phosphorus is 1e19cm -3 ~5e19cm -3 , the total carbon doping concentration is 1e20cm -3 ~8e20 cm -3 , the bottom phosphorus doping concentration is 3e17cm -3 ~6e17cm -3 , bottom carbon doping concentration 2e18cm -3 ~5e18cm -3 , the surface phosphorus doping concentration is 2e21cm -3 ~8e21cm -3 , surface carbon doping concentration 3e22cm -3 ~8e22cm -3 Linear gradient carbon doping can help reduce optical losses, linear gradient phosphorus doping can help reduce carrier recombination and improve the passivation level, and the presence of a high-concentration carbon-doped layer on the surface can help resist the bombardment of subsequent hydrogen treatment, thereby reducing the parasitic absorption of polysilicon and increasing the short-circuit current of the battery, thereby increasing the current density.

[0059] In some embodiments, continue to refer to Figure 1 The back contact heterojunction solar cell further includes an anti-reflection layer 7, which is arranged on the side of the third semiconductor layer away from the silicon wafer 1, specifically on the side of the second intrinsic polysilicon layer away from the silicon wafer. The anti-reflection layer 7 is mainly used to reduce the reflection of light, thereby improving the photoelectric conversion efficiency. The thickness of the anti-reflection layer is generally 80mm~100mm. If it is too thick, it is not conducive to the penetration of light, and if it is too thin, the reflection effect of the incident light is not good.

[0060] Specifically, the anti-reflection layer 7 is composed of a first silicon nitride anti-reflection layer, a second silicon nitride anti-reflection layer, a first silicon oxynitride anti-reflection layer, a second silicon oxynitride anti-reflection layer and a silicon oxide layer in sequence; wherein the thickness of the first silicon nitride anti-reflection layer is 20nm~30nm, the thickness of the second silicon nitride anti-reflection layer is 15nm~25nm; the thickness of the first silicon oxynitride anti-reflection layer is 10nm~20nm; the thickness of the second silicon oxynitride anti-reflection layer is 10nm~20nm; the thickness of the silicon oxide layer is 25nm~40nm.

[0061] In some embodiments, a textured surface is formed on the front side of the silicon wafer 1 and on the surface of the silicon wafer 1 located in the second semiconductor opening area. The second semiconductor layer and the third semiconductor layer respectively fill the textured surfaces in corresponding areas. The textured surface is formed by an acid cleaning process, which can not only remove excess film layer material, but also help to increase the bonding strength between the film layers.

[0062] In some embodiments, continue to refer to Figure 1 The back-contact heterojunction solar cell also includes: an isolation groove; the isolation groove is located between the adjacent first semiconductor opening area and the second semiconductor opening area; the first semiconductor opening area and the second semiconductor layer are both covered with a transparent conductive film layer 10, and the isolation groove separates the transparent conductive film layer 10 located in the first semiconductor opening area from the transparent conductive film layer 10 located on the second semiconductor layer.

[0063] Optionally, the width of the isolation groove is 30um~200um.

[0064] In a second aspect, an embodiment of the present invention further provides a method for preparing a back-contact heterojunction solar cell, which is used to prepare a back-contact heterojunction solar cell as in the above embodiment, such as Figure 2 As shown, the method for preparing a back contact heterojunction solar cell comprises the following steps:

[0065] S01. Provide a silicon wafer.

[0066] Alternatively, if Figure 4 As shown, step S01 may also include other conventional operations, such as double-sided polishing and optional cleaning of the silicon wafer 1. The silicon wafer 1 is preferably an N-type single crystal silicon wafer 1. The silicon wafer 1 may be a Czochralski single crystal silicon wafer 1 or a cast single crystal silicon wafer 1.

[0067] S02. A tunneling silicon oxide layer and an N-type doped polysilicon layer are sequentially prepared on the back side of the silicon wafer to obtain a first semiconductor layer; the N-type doped polysilicon layer is composed of a first intrinsic polysilicon layer and a phosphorus-doped polysilicon layer.

[0068] Optionally, the N-type doped polysilicon layer 3 is composed of a first intrinsic polysilicon layer and a phosphorus-doped polysilicon layer. Figure 5As shown, the first semiconductor layer can be formed by tubular PECVD, LPCVD or PVD in-situ doping deposition annealing, preferably tubular PECVD in-situ doping, in the first stage, laughing gas is introduced, the glow is turned on, and the tunneling silicon oxide layer 2 is formed by chemical reaction, the reaction temperature of the first stage is 400~450℃, the reaction pressure is 100~2000mtorr (mitorr), the time is 10~60 seconds, and the thickness of the tunneling silicon oxide layer 2 is 1~2nm; then enter the second stage, the second stage firstly introduces silane and hydrogen, turns on the glow, and forms a tunneling silicon oxide layer 2 by chemical reaction. The first intrinsic polysilicon layer is formed by chemical reaction. The reaction temperature of the second stage is 400~450℃, the reaction time is 300~900 seconds, the reaction pressure is 100~2000mtorr, and the thickness of the intrinsic polysilicon layer is 30~50nm. In the third stage, silane, phosphine and hydrogen are introduced, the glow is turned on, and a phosphorus-doped polysilicon layer is formed by chemical reaction. The reaction temperature of the third stage is 400~450℃, the reaction time is 200~600 seconds, the reaction pressure is 100~2000mtorr, and the thickness of the phosphorus-doped polysilicon layer is 80~100nm.

[0069] S03. Form a mask layer on the surface of the first semiconductor layer.

[0070] Optionally, continue to Figure 5 A mask layer 4 is grown on the surface of the cleaned first semiconductor layer. The mask layer 4 can be silicon nitride, silicon oxide and silicon oxynitride. Preferably, silicon nitride is deposited as the mask layer 4 using tubular PECVD with a thickness of 50 to 200 nm, and hydrofluoric acid is used to remove the silicon nitride coated on the front side.

[0071] S04, removing a portion of the mask layer and a corresponding portion of the first semiconductor layer to form alternately arranged second semiconductor opening regions.

[0072] Optionally, see Figure 6 , an opening is etched on the back of the silicon wafer 1 by laser or mask etching to form a second semiconductor opening area W2. The width of the second semiconductor opening area W2 is 0.3-0.6 mm, and the mask layer 4, the N-type doped polycrystalline layer 3 and the tunneling silicon oxide layer 2 in the second semiconductor opening area W2 are etched away. Optionally, the laser can be an ultraviolet or green laser with a pulse width of less than 100 ns.

[0073] S05. Remove the remaining mask layer, N-type doped polycrystalline layer and tunneling silicon oxide layer in the second semiconductor opening area through texturing and cleaning, and at the same time form a texturing surface on the front side of the silicon wafer and the surface of the silicon wafer located in the second semiconductor opening area, and then remove the mask layer on the back side of the silicon wafer outside the second semiconductor opening area.

[0074] Optionally, continue to Figure 6The mask layer 4 outside the second semiconductor opening region W2 on the back side of the silicon wafer 1 is removed by cleaning with hydrofluoric acid.

[0075] S06. Sequentially prepare an oxide layer and a second intrinsic polysilicon layer on the front side of the silicon wafer.

[0076] Optionally, see Figure 7 , formed by tubular PECVD, LPCVD or PVD deposition annealing, preferably using tubular PECVD, in the first stage, nitrous oxide is introduced, the glow is turned on, and an oxide layer 5 is formed by chemical reaction. The reaction temperature in the first stage is 400-450°C, the nitrous oxide flow rate is 5000-8000sccm; the reaction pressure is 100-2000mtorr, the time is 120-240 seconds, and the oxide layer thickness is 2-4nm; then enter the second stage, in the second stage, silane and hydrogen are introduced Gas is turned on, and the glow is turned on to form a second intrinsic polysilicon layer 6 through chemical reaction. The reaction temperature of the second stage is 400~450℃, the reaction time is 50~150 seconds, and the reaction pressure is 100~2000mtorr. The thickness of the second intrinsic polysilicon layer 6 is 10~150nm, and high-temperature annealing is performed. The annealing pressure is 300mbar~800mbar, the annealing temperature is 900~950℃, and the annealing time is 60~120M. After annealing, HF is used to remove the surface oxide layer.

[0077] S07, doping the second intrinsic polysilicon layer with carbon and phosphorus to obtain a third semiconductor layer, and performing hydrogen treatment and depositing an anti-reflection layer.

[0078] Specifically, in the first stage, a mixture of phosphine and methane is introduced, the glow is turned on, the reaction temperature is 400-450°C, the PH3 flow rate is 300-500sccm, the CH4 flow rate is 1000-1500sccm, the reaction pressure is 300-500mtorr, the time is 240-360 seconds, the power is 3-5KW, and the total phosphorus doping concentration is 1e19-5e19cm -3 , the total carbon doping concentration is 1e20~8e20cm -3 , the bottom phosphorus doping concentration is 3e17~6e17cm -3 , bottom carbon doping concentration 2e18~5e18 cm -3 , the surface phosphorus doping concentration is 2e21~8e21cm -3 , surface carbon doping concentration 3e22~8e22 cm -3, thereby obtaining the third semiconductor layer; in the second stage, hydrogen is introduced, the H2 flow rate is 3000~5000sccm, the reaction temperature is 400~450℃, and the power is 5~7KW; in the third stage, silane and ammonia are introduced, the glow is turned on, and a silicon nitride anti-reflection layer is formed through chemical reaction. The reaction temperature of the third stage is 400~450℃, the silane flow rate is 1200~1600sccm, the NH3 flow rate is 5000~8000sccm, the reaction time is 700~1000 seconds, the reaction pressure is 500~3000mtorr, the power is 4000~6000W, and the thickness of the silicon nitride anti-reflection layer is 80~110nm.

[0079] S08. Depositing a second semiconductor layer on the back side of the silicon wafer obtained in step S07. The second semiconductor layer is composed of an intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer or a P-type doped microcrystalline silicon layer.

[0080] Optionally, see Figure 8 , a second semiconductor layer is deposited on the back of the silicon wafer 1 by plasma enhanced chemical vapor deposition (PECVD) technology, and the second semiconductor layer includes an intrinsic amorphous silicon layer 8 and a P-type doped amorphous layer or a P-type doped microcrystalline silicon layer. The thickness of the intrinsic amorphous silicon layer 8 is 5nm~15nm, the thickness of the P-type doped amorphous layer or the P-type doped microcrystalline silicon layer is 10nm~35nm, and the boron doping concentration in the P-type doped amorphous layer or the P-type doped microcrystalline silicon layer is 1e19~4e20 cm -3 .

[0081] S09, etching an opening on the back side of the silicon wafer 1 obtained in step S08 to form a first semiconductor opening region spaced apart from the second semiconductor opening region.

[0082] Optionally, continue to Figure 8 , using laser or mask etching, an opening is etched on the back of the silicon wafer 1 to form a first semiconductor opening area W1 spaced apart from the second semiconductor opening area W2, and then cleaned. The width of the first semiconductor opening area W1 is 0.1mm~0.3mm, and the second semiconductor layer on the upper surface of the first semiconductor opening area W1 is cleaned after etching. Optionally, the laser is an ultraviolet or green laser, and the pulse width is less than 50ns.

[0083] In some optional implementations, see Figure 3 , after step S09, further comprising:

[0084] S10 , cleaning and removing the remaining second semiconductor layer in the first semiconductor opening region, and then depositing a transparent conductive film layer 10 on the back side of the obtained silicon wafer 1 .

[0085] Alternatively, if Fig. 9As shown, a transparent conductive film layer 10 is deposited on the back of the silicon wafer 1 by physical vapor deposition technology (PVD) or activated plasma deposition technology (RPD). The thickness of the transparent conductive film layer 10 is 40nm~80nm. The material of the transparent conductive film layer 10 can be an indium oxide film doped with tin oxide, titanium oxide, zinc oxide or gallium oxide, or a zinc oxide film doped with aluminum oxide, gallium oxide or boron oxide.

[0086] S11 , opening is performed on the transparent conductive film layer 10 between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove.

[0087] Alternatively, if Fig.10 As shown, an isolation groove is formed between the first semiconductor opening region and the second semiconductor region by laser or etching, and the width of the isolation groove is 30um-200um.

[0088] S12, forming a first electrode on the transparent conductive film layer 10 in the first semiconductor opening region, and correspondingly forming a second electrode on the transparent conductive film layer 10 in the second semiconductor opening region.

[0089] Continue reading Fig.10 A first electrode is formed on the conductive film layer of the first semiconductor region, and a second electrode is correspondingly formed on the conductive film layer of the second semiconductor region. A silver gate electrode can be formed by a screen printing process and low-temperature sintering, or the electrode can be formed by electroplating. Preferably, the gate line electrode is formed by electroplating.

[0090] The method for preparing a back-contact heterojunction solar cell in the embodiment of the present invention may further include other conventionally required steps, which may be selected according to actual needs and will not be described in detail here.

[0091] In a third aspect, an embodiment of the present invention further provides a battery assembly, which includes a back-contact heterojunction solar cell as described in the aforementioned embodiment.

[0092] The battery assembly provided in this embodiment includes the back-contact heterojunction solar cell in the aforementioned embodiment. The back-contact heterojunction solar cell has an N-type polysilicon layer with a multi-film layer structure with a specific refractive index, and the refractive index of each film layer is changed by doping carbon and oxygen elements in different proportions. At the same time, each film layer matches the corresponding thickness to achieve a combination of high and low refractive index film layers, which is beneficial to increase the short-circuit current, thereby realizing a back-contact solar cell structure with a high current density.

[0093] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0094] Example 1

[0095] A back contact heterojunction solar cell with a specific front laminate structure, the structure of which is as follows Figure 1 As shown, its preparation method is as follows Figure 3 As shown, including:

[0096] S01. Provide a silicon wafer.

[0097] Alternatively, if Figure 4 As shown, step S01 may also include other conventional operations, such as double-sided polishing and optional cleaning of the silicon wafer 1. The silicon wafer 1 is preferably an N-type single crystal silicon wafer 1. The silicon wafer 1 may be a Czochralski single crystal silicon wafer 1 or a cast single crystal silicon wafer 1.

[0098] S02. A tunneling silicon oxide layer and an N-type doped polysilicon layer are sequentially prepared on the back side of the silicon wafer to obtain a first semiconductor layer; wherein the N-type doped polysilicon layer 3 is composed of a first intrinsic polysilicon layer and a phosphorus-doped polysilicon layer. The tunneling oxide layer 2 has a thickness of 1.5 nm, the intrinsic polysilicon layer has a thickness of 50 nm, and the phosphorus-doped polysilicon layer has a thickness of 100 nm.

[0099] S03, forming a mask layer on the surface of the first semiconductor layer.

[0100] Optionally, continue to Figure 5 A mask layer 4 is grown on the surface of the cleaned first semiconductor layer. The mask layer 4 can be silicon nitride, silicon oxide and silicon oxynitride. Preferably, silicon nitride is deposited as the mask layer 4 using tubular PECVD with a thickness of 50 to 200 nm, and hydrofluoric acid is used to remove the silicon nitride coated on the front side.

[0101] S04, removing a portion of the mask layer and a corresponding portion of the first semiconductor layer to form alternately arranged second semiconductor opening regions.

[0102] Optionally, see Figure 6 , an opening is etched on the back of the silicon wafer 1 by laser or mask etching to form a second semiconductor opening area W2. The width of the second semiconductor opening area W2 is 0.3 mm, and the mask layer 4, the N-type doped polycrystalline layer 3 and the tunneling silicon oxide layer 2 in the second semiconductor opening area W2 are etched away.

[0103] S05. Remove the remaining mask layer, N-type doped polycrystalline layer and tunneling silicon oxide layer in the second semiconductor opening area through texturing and cleaning, and at the same time form a texturing surface on the front side of the silicon wafer and the surface of the silicon wafer located in the second semiconductor opening area, and then remove the mask layer on the back side of the silicon wafer outside the second semiconductor opening area.

[0104] S06. Forming an oxide layer and a second intrinsic polysilicon layer in sequence on the front side of the silicon wafer.

[0105] Optionally, see Figure 7, the oxide layer thickness is 2nm; the second intrinsic polysilicon layer thickness is 15nm.

[0106] S07, doping the second intrinsic polysilicon layer with carbon and phosphorus, performing hydrogen treatment, and depositing an anti-reflection layer.

[0107] Specifically, a mixed gas of phosphine and methane is introduced, the glow is turned on, the reaction temperature is 400-450°C, the PH3 flow rate is 300-500sccm, the CH4 flow rate is 1000-1500sccm, the reaction pressure is 300-500mtorr, the time is 240-360 seconds, the power is 3-5KW, and the total phosphorus doping concentration is 1e19 cm -3 , the total carbon doping concentration is 1e20 cm -3 , the bottom phosphorus doping concentration is 3e17 cm -3 , bottom carbon doping concentration 2e18 cm -3 The surface phosphorus doping concentration is 2e21 cm -3 , surface carbon doping concentration 3e22cm -3 The phosphorus doping concentration and carbon doping concentration of the second intrinsic polysilicon layer change linearly from the surface layer to the bottom layer with gradient slopes of 1.3e20 and 2e21 respectively, and the thickness of the anti-reflection layer is 100nm.

[0108] S08. Depositing a second semiconductor layer on the back side of the silicon wafer obtained in step S07. The second semiconductor layer is composed of an intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer or a P-type doped microcrystalline silicon layer.

[0109] Optionally, see Figure 8 , an intrinsic amorphous silicon layer 8 and a P-type doped amorphous layer or a P-type doped microcrystalline silicon layer are sequentially deposited on the back of the silicon wafer 1 by plasma enhanced chemical vapor deposition (PECVD) technology. The thickness of the intrinsic amorphous silicon layer 8 is 10nm, the thickness of the P-type doped amorphous layer or the P-type doped microcrystalline silicon layer is 25nm, and the boron doping concentration in the P-type doped amorphous layer or the P-type doped microcrystalline silicon layer is 2e20cm -3 .

[0110] S09, etching an opening on the back side of the silicon wafer 1 obtained in step S08 to form a first semiconductor opening region spaced apart from the second semiconductor opening region.

[0111] Optionally, continue to Figure 8 , using laser or mask etching, an opening is etched on the back of the silicon wafer 1 to form a first semiconductor opening area W1 spaced apart from the second semiconductor opening area W2, and then cleaned. The width of the first semiconductor opening area W1 is 0.2 mm, and the second semiconductor layer on the upper surface of the first semiconductor opening area W1 is cleaned after etching.

[0112] S10 , cleaning and removing the remaining second semiconductor layer in the first semiconductor opening region, and then depositing a transparent conductive film layer 10 on the back side of the obtained silicon wafer 1 .

[0113] Alternatively, if Fig. 9 As shown, a transparent conductive film layer 10 is deposited on the back of the silicon wafer 1 by physical vapor deposition technology (PVD) or activated plasma deposition technology (RPD). The thickness of the transparent conductive film layer 10 is 50 nm. The material of the transparent conductive film layer 10 can be an indium oxide film doped with tin oxide, titanium oxide, zinc oxide or gallium oxide, or a zinc oxide film doped with aluminum oxide, gallium oxide or boron oxide.

[0114] S11 , opening is performed on the transparent conductive film layer 10 between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove.

[0115] Alternatively, if Fig.10 As shown, an isolation groove is formed between the first semiconductor opening region and the second semiconductor region by laser or etching, and the width of the isolation groove is 100 um.

[0116] S12, forming a first electrode on the transparent conductive film layer 10 in the first semiconductor opening region, and correspondingly forming a second electrode on the transparent conductive film layer 10 in the second semiconductor opening region.

[0117] Continue reading Fig.10 A first electrode is formed on the conductive film layer of the first semiconductor region, and a second electrode is correspondingly formed on the conductive film layer of the second semiconductor region. A silver gate electrode can be formed by a screen printing process and low-temperature sintering, or the electrode can be formed by electroplating. Preferably, the gate line electrode is formed by electroplating.

[0118] Example 2

[0119] The method of Example 1 is followed, except that in step S07, the total phosphorus doping concentration of the second intrinsic polysilicon layer is 3e19 cm -3 , the total carbon doping concentration is 3e20cm -3 , the bottom phosphorus doping concentration is 4e17cm -3 , bottom carbon doping concentration 3e18cm -3 The surface phosphorus doping concentration is 4e21cm -3 , surface carbon doping concentration 5e22cm -3 The phosphorus doping concentration and carbon doping concentration of the second intrinsic polysilicon layer change linearly from the surface layer to the bottom layer, and the gradient slopes are 2.7e20 and 3.3e21 respectively.

[0120] Example 3

[0121] The method of Example 1 is followed, except that in step S07, the total phosphorus doping concentration of the second intrinsic polysilicon layer is 5e19cm -3 , the total carbon doping concentration is 8e20cm -3 , the bottom phosphorus doping concentration is 6e17cm -3 , bottom carbon doping concentration 5e18cm -3 The surface phosphorus doping concentration is 8e21cm -3 , surface carbon doping concentration 8e22cm -3 , the phosphorus doping concentration and carbon doping concentration of the second intrinsic polysilicon layer change linearly from the surface layer to the bottom layer, and the gradient slopes are 5.3e20 and 5.3e21;

[0122] The total thickness of the second intrinsic polysilicon layer is 15 nm, the surface thickness of the second intrinsic polysilicon layer is 4 nm, and the bottom thickness of the second intrinsic polysilicon layer is 2 nm.

[0123] Example 4

[0124] The method of Example 1 is referred to, except that the thickness of the anti-reflection layer is adjusted to 80 nm.

[0125] Example 5

[0126] The method of Example 1 is followed, except that the thickness and boron doping concentration of the P-type doped amorphous silicon layer or the P-type doped microcrystalline silicon layer 9 in the second semiconductor layer are adjusted. The thickness of the P-type doped amorphous silicon layer or the P-type doped microcrystalline silicon layer 9 is 35 nm, and the boron doping concentration in the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer is 4e20 cm -3 .

[0127] The process parameters that need to be adjusted to meet the thickness and boron doping concentration of the P-type doped amorphous silicon layer or the P-type doped microcrystalline silicon layer 9 are: prolonging the film deposition time and increasing the borane flow rate.

[0128] Example 6

[0129] The method of Example 1 is referred to, except that the size relationship between the first semiconductor opening region W1 and the second semiconductor opening region W2 is adjusted, the width W1 of the first semiconductor opening region W1 is 0.3 mm, and the width W2 of the second semiconductor opening region W2 is 0.6 mm.

[0130] Example 7

[0131] The method of Example 1 is referred to, except that the thicknesses of the tunneling silicon oxide layer 2, the intrinsic polysilicon layer and the phosphorus-doped polysilicon layer are adjusted, the thickness of the tunneling oxide layer 2 is 2 nm, the thickness of the intrinsic polysilicon layer is 30 nm, and the thickness of the phosphorus-doped polysilicon layer is 80 nm.

[0132] Comparative Example 1

[0133] The method of Example 1 is referred to, except that only the third semiconductor layer having the oxide layer 5 and the second intrinsic polysilicon layer 6 is formed, and the second intrinsic polysilicon layer 6 is not doped with carbon and phosphorus.

[0134] Comparative Example 2

[0135] The method of Example 1 is followed, except that in step S07, a third semiconductor layer having an oxide layer 5 and a second intrinsic polysilicon layer 6 is formed, and the second intrinsic polysilicon layer 6 is doped with carbon and phosphorus, but the total doping concentrations of carbon and phosphorus are 1e21cm -3 and 1e20 cm -3 .

[0136] Comparative Example 3

[0137] The method of Example 1 is followed, except that the carbon doping concentration and phosphorus doping concentration of the surface layer of the second intrinsic polysilicon layer 6 are 1e21 cm -3 and 1e20cm -3 The carbon doping concentration and phosphorus doping concentration of the bottom layer are 1e17cm -3 and 1e16cm -3 .

[0138] Comparative Example 4

[0139] The method of Example 1 is referred to, except that the gradient slopes of the carbon doping concentration and the phosphorus doping concentration from the surface layer to the bottom layer of the second intrinsic polysilicon layer 6 are 1e20 and 1e18.

[0140] Comparative Example 5

[0141] The method of Example 1 is referred to, except that in step S07, only the third semiconductor layer is formed, and no reflective layer is prepared.

[0142] Comparative Example 6

[0143] The method of Example 1 is referred to, except that the thickness of each film layer of the third semiconductor layer in step S07 is adjusted, specifically, the thickness of the oxide layer is 1 nm, the thickness of the second intrinsic polysilicon layer is 8 nm, the surface thickness of the second intrinsic polysilicon layer is 1.5 nm, and the bottom thickness of the second intrinsic polysilicon layer is 0.5 nm.

[0144] Test Case

[0145] The back-contact heterojunction solar cells obtained in the above embodiments and comparative examples were subjected to performance tests, and the results are shown in Table 1. The unit of short-circuit current Isc is A, the unit of open-circuit voltage Voc is V, the unit of fill factor FF is %, and the unit of cell conversion efficiency Eta is %.

[0146] Table 1 Performance tests of various embodiments and comparative examples

[0147]

[0148] From the above results, it can be seen that, compared with the comparative example, the embodiment scheme of the present invention can significantly improve the short-circuit current and open-circuit voltage, which is beneficial to improving the battery conversion efficiency. Further, according to Example 1 and Examples 2 to 7, and Comparative Examples 1 to 6, it can be seen that the preferred specific structure and specific doping concentration scheme of the present invention can keep both the voltage and short-circuit current at a high level, which is more conducive to improving the battery conversion efficiency.

[0149] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A back contact heterojunction solar cell, characterized in that: include: A silicon wafer having a front side and a back side; A first semiconductor layer is arranged on the back side of the silicon wafer, the first semiconductor layer comprises a tunneling silicon oxide layer and an N-type doped polysilicon layer sequentially formed on the silicon wafer, the N-type doped polysilicon layer comprises a first intrinsic polysilicon layer and a phosphorus-doped polysilicon layer; The first semiconductor layer is separated by a plurality of second semiconductor opening regions, the second semiconductor opening regions and the surface of the first semiconductor layer around the second semiconductor opening regions are covered with a second semiconductor layer, the second semiconductor layer is composed of an intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer or a P-type doped microcrystalline silicon layer; a first semiconductor opening region is provided between adjacent second semiconductor opening regions, and the first semiconductor opening region separates the second semiconductor layer; The third semiconductor layer includes an oxide layer and a second intrinsic polysilicon layer stacked in sequence on the front side of the silicon wafer; the side of the second intrinsic polysilicon layer close to the oxide layer is the bottom layer, and the side away from the oxide layer is the surface layer; wherein the total phosphorus doping concentration of the second intrinsic polysilicon layer is 1e19cm -3 ~5e19cm -3 The total carbon doping concentration of the second intrinsic polysilicon layer is 1e20cm -3 ~8e20cm -3 The surface phosphorus doping concentration of the second intrinsic polysilicon layer is 2e21cm -3 ~8e21cm -3 , the surface carbon doping concentration is 3e22cm -3 ~8e22cm -3 The bottom phosphorus doping concentration of the second intrinsic polysilicon layer is 3e17cm -3 ~6e17cm -3 , bottom carbon doping concentration 2e18cm -3 ~5e18cm -3 , and the phosphorus doping concentration and carbon doping concentration change linearly from the surface to the bottom layer. The intrinsic polysilicon is treated with methane and phosphine using tubular PECVD to achieve gradual doping of carbon and phosphorus.

2. The back-contact heterojunction solar cell according to claim 1, characterized in that: The phosphorus doping concentration of the second intrinsic polysilicon layer changes linearly from the surface layer to the bottom layer, and the gradient slope thereof is 1.3e19-8e20, and the carbon doping concentration changes linearly from the surface layer to the bottom layer, and the gradient slope thereof is 2e21-8e21.

3. The back contact heterojunction solar cell according to claim 1, characterized in that: The thickness of the oxide layer is 2-4 nm, the thickness of the second intrinsic polysilicon layer is 10-15 nm, the surface thickness of the second intrinsic polysilicon layer is 2-4 nm, and the bottom thickness of the second intrinsic polysilicon layer is 1-2 nm.

4. The back contact heterojunction solar cell according to claim 1, characterized in that: Also includes: Anti-reflection layer; the anti-reflection layer is arranged on a side of the second intrinsic polysilicon layer away from the silicon wafer; the thickness of the anti-reflection layer is 80nm~100nm.

5. The back contact heterojunction solar cell according to claim 4, characterized in that: The anti-reflection layer is composed of a first silicon nitride anti-reflection layer, a second silicon nitride anti-reflection layer, a first silicon oxynitride anti-reflection layer, a second silicon oxynitride anti-reflection layer and a silicon oxide layer in sequence; Among them, the thickness of the first silicon nitride anti-reflection layer is 20nm~30nm, the thickness of the second silicon nitride anti-reflection layer is 15nm~25nm; the thickness of the first silicon oxynitride anti-reflection layer is 10nm~20nm; the thickness of the second silicon oxynitride anti-reflection layer is 10nm~20nm; the thickness of the silicon oxide layer is 25nm~40nm.

6. The back contact heterojunction solar cell according to claim 1, characterized in that: A textured surface is formed on the front side of the silicon wafer and the surface of the silicon wafer located in the second semiconductor opening area, and the second semiconductor layer and the third semiconductor layer fill the textured surfaces in corresponding areas respectively.

7. The back-contact heterojunction solar cell according to claim 1, characterized in that: The thickness of the intrinsic amorphous silicon layer is 5nm-15nm, the thickness of the P-type doped amorphous silicon layer or the P-type doped microcrystalline silicon layer is 10nm-35nm, and the boron doping concentration in the P-type doped amorphous silicon layer or the P-type microcrystalline silicon layer is 1e19 cm -3 ~4e20 cm -3 .

8. The back-contact heterojunction solar cell according to any one of claims 1 to 7, characterized in that: Also includes: Isolation tank; The isolation trench is located between the adjacent first semiconductor opening region and the second semiconductor opening region; The first semiconductor opening region and the second semiconductor layer are both covered with a transparent conductive film layer, and the isolation groove separates the transparent conductive film layer located in the first semiconductor opening region from the transparent conductive film layer located on the second semiconductor layer.

9. The back-contact heterojunction solar cell according to claim 8, characterized in that: The width of the first semiconductor opening region is 0.1 mm to 0.3 mm; the width of the second semiconductor opening region is 0.3 mm to 0.6 mm; and / or the width of the isolation trench is 30 um to 200 um.

10. A method for preparing a back-contact heterojunction solar cell, which is used to prepare the back-contact heterojunction solar cell according to any one of claims 1 to 9, the method for preparing the back-contact heterojunction solar cell comprising the following steps: S01, providing a silicon wafer; S02, sequentially preparing a tunneling silicon oxide layer and an N-type doped polysilicon layer on the back side of the silicon wafer to obtain a first semiconductor layer; the N-type doped polysilicon layer is composed of a first intrinsic polysilicon layer and a phosphorus-doped polysilicon layer; S03, preparing a mask layer on the surface of the first semiconductor layer; S04, removing a portion of the mask layer and a corresponding portion of the first semiconductor layer to form alternately arranged second semiconductor opening regions; S05, removing the remaining mask layer, N-type doped polycrystalline layer and tunneling silicon oxide layer in the second semiconductor opening region by texturing and cleaning, and forming a texture surface on the front side of the silicon wafer and the surface of the silicon wafer located in the second semiconductor opening region, and then removing the mask layer on the back side of the silicon wafer outside the second semiconductor opening region; S06, sequentially preparing an oxide layer and a second intrinsic polysilicon layer on the front side of the silicon wafer; S07, doping the second intrinsic polysilicon layer with carbon and phosphorus to obtain a third semiconductor layer, and performing hydrogen treatment and depositing an anti-reflection layer; wherein the total doping concentration of phosphorus in the second intrinsic polysilicon layer is 1e19cm -3 ~5e19cm -3 The total carbon doping concentration of the second intrinsic polysilicon layer is 1e20cm -3 ~8e20cm -3 The surface phosphorus doping concentration of the second intrinsic polysilicon layer is 2e21cm -3 ~8e21cm -3 , the surface carbon doping concentration is 3e22cm -3 ~8e22cm -3 The bottom phosphorus doping concentration of the second intrinsic polysilicon layer is 3e17cm -3 ~6e17cm -3 , bottom carbon doping concentration 2e18cm -3 ~5e18cm -3 , and the phosphorus doping concentration and carbon doping concentration change linearly from the surface to the bottom layer; S08, depositing a second semiconductor layer on the back side of the silicon wafer obtained in step S07, wherein the second semiconductor layer is composed of an intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer or a P-type doped microcrystalline silicon layer; S09, etching an opening on the back side of the silicon wafer obtained in step S08 to form a first semiconductor opening region spaced apart from the second semiconductor opening region.

11. The method for preparing a back-contact heterojunction solar cell according to claim 10, characterized in that: After step S09, the method further includes: S10, cleaning and removing the second semiconductor layer remaining in the first semiconductor opening region, and then depositing a transparent conductive film layer on the back side of the obtained silicon wafer; S11, making an opening on the transparent conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove; S12, forming a first electrode on the transparent conductive film layer in the first semiconductor opening region, and correspondingly forming a second electrode on the transparent conductive film layer in the second semiconductor opening region.

12. A battery assembly, characterized in that: It comprises the back-contact heterojunction solar cell according to any one of claims 1 to 9.