Inorganic-organic hybrid nano-film photoelectric device for simulating nerve synapse and preparation method of inorganic-organic hybrid nano-film photoelectric device

Inorganic-organic hybrid nano-thin film optoelectronic devices are prepared through molecular layer/atomic layer deposition technology, which solves the shortcomings of inorganic-organic hybrid materials in the existing technology in simulating the function of synapses and realizes the function of multiple synapses. Simulation provides new materials and preparation methods for artificial neural networks and flexible optoelectronic devices.

CN118829239APending Publication Date: 2024-10-22NANJING UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410760368.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the existing technology, optoelectronic devices that simulate neural synapses mainly rely on inorganic or organic materials. There is a lack of research on inorganic-organic hybrid materials, which limits the tunability and flexibility of the materials, making it difficult to achieve efficient functional simulation of neural synapses. .

Method used

Inorganic-organic hybrid nano-film optoelectronic devices are prepared at low temperature using molecular layer/atomic layer deposition technology. Through the double-layer stack structure of inorganic-organic hybrid films and metal oxide films, vertical or planar structures that simulate neural synapses are constructed to achieve Functional simulation.

Benefits of technology

It has realized the important functions of simulating neural synapses, such as long-term potentiation, long-term inhibition, short-term plasticity transition, double-pulse facilitation, learning, forgetting and re-learning, and conditioned reflection, broadening the material selection for the photoelectric functional layer, and providing Artificial neural network computing and flexible bionic optoelectronic devices provide new material ideas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118829239A_ABST
    Figure CN118829239A_ABST
Patent Text Reader

Abstract

The invention discloses an inorganic-organic hybrid nano-film photoelectric device for simulating nerve synapse and a preparation method thereof. The photoelectric device structure comprises a vertical structure which is composed of a substrate, a bottom electrode, a photoelectric material layer and a top electrode in sequence; the planar structure sequentially comprises a substrate, a photoelectric material layer and an interdigital electrode. The photoelectric material layer is of a double-layer nano stack structure composed of an inorganic-organic hybrid thin film and a metal oxide thin film, the inorganic-organic hybrid thin film is metal-based hydroquinone, metal-based p-aminophenol or metal-based maleic acid, and the metal oxide thin film is ZnO, TiO2, HfO2, ZrO2, MoO3, Ta2O5, GeO2, WO3, SnO2 or IGZO. The inorganic-organic hybrid / metal oxide thin film is prepared by adopting a molecular layer / atomic layer deposition technology, the inorganic-organic hybrid / metal oxide thin film can be compatible with a microelectronic process and is suitable for large-scale integration, and the constructed photoelectric device has several important functions of neural synapse-like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the intersection of semiconductor optoelectronic devices, neuroscience and artificial intelligence, and specifically relates to an inorganic-organic hybrid nano-thin film optoelectronic device that simulates neural synapses and a preparation method thereof. Background Art

[0002] As the core structure in the nervous system, synapses are responsible for information transmission and processing between neurons. Their complex and sophisticated functions have always been an important area of ​​neuroscience research. Optoelectronic devices, with their excellent photoelectric conversion characteristics, provide new possibilities for simulating and replicating biological functions. In recent years, with the continuous development of optoelectronic device technology, more and more researchers have begun to explore the use of optoelectronic devices to simulate the functions of synapses. By carefully designing and optimizing the structure and performance of optoelectronic devices, optoelectronic signals can be used to simulate the information transmission, processing and learning capabilities of synapses. This interdisciplinary integration not only helps to deepen our understanding of the working principles of the nervous system, but also provides new ideas for the development of more advanced and intelligent artificial neural networks.

[0003] In previous studies, inorganic materials, organic materials or halide perovskite materials were mostly used as optoelectronic materials, and a small amount involved quantum dot optoelectronic materials. However, reports on the use of inorganic-organic hybrid material systems in optoelectronic synapses are relatively rare. Inorganic-organic hybrid material systems are different from traditional composite materials. Inorganic-organic elements can achieve molecular-level composites, contain rich and colorful physical and chemical properties, and have the advantages of both inorganic and organic compounds. They show great tunability and flexibility in material structure and performance, so they are particularly suitable for the development of flexible optoelectronic devices. At present, the preparation methods of inorganic-organic hybrid materials mainly include sol-gel method, hydrothermal synthesis method, blending method, intercalation composite method, LB film method, etc. Most of them are solution-based preparation technologies. The preparation technology of inorganic-organic hybrid thin film materials compatible with microelectronic processes is in urgent need of development. Atomic layer deposition (ALD) and its sub-category molecular layer deposition (MLD) are a new type of material preparation technology, which is unique in the controllable deposition of inorganics, polymers and inorganic-organic hybrid thin film materials. Its unique sequential self-limiting reaction mechanism makes it particularly suitable for the "bottom-up" design and preparation of inorganic-organic functional unit hybrid optoelectronic materials. Therefore, the present invention uses molecular layer / atomic layer deposition technology to prepare inorganic-organic / inorganic hybrid double-layer nanofilm optoelectronic devices that simulate neural synapses, and obtains a series of synaptic bionic functions. The present invention provides new material ideas and preparation methods for the development of artificial neural networks, and promotes research progress in the intersection of optoelectronic devices and neuroscience. Summary of the invention

[0004] Purpose of the invention: To provide an inorganic-organic hybrid nano-thin film optoelectronic device that simulates neural synapses and a preparation method thereof, and to use molecular layer deposition and atomic layer deposition techniques to prepare inorganic-organic hybrid nano-thin film optoelectronic devices with good bionic functions of simulating neural synapses at low temperature.

[0005] Technical solution: An inorganic-organic hybrid nano-thin film optoelectronic device that simulates neural synapses, the device structure includes: a vertical structure from bottom to top, a substrate, a bottom electrode, an optoelectronic material layer, and a top electrode; a planar structure from bottom to top, a substrate, an optoelectronic material layer, and interdigital electrodes. The optoelectronic material layer is composed of a double-layer nano-stack structure composed of an inorganic-organic hybrid film and a metal oxide film.

[0006] The inorganic-organic hybrid film is metal-based hydroquinone, metal-based p-aminophenol or metal-based maleic acid, and the metal oxide film is ZnO, TiO2, HfO2, ZrO2, MoO3, Ta2O5, GeO2, WO3, SnO2 or IGZO.

[0007] Furthermore, the thickness of the inorganic-organic hybrid film is 5 to 50 nm, and the thickness of the metal oxide film is 5 to 20 nm.

[0008] Furthermore, the metal matrix of the inorganic-organic hybrid thin film is one or more of Al, Ti, Zn, Sn, Hf, Zr, Ni, and Co.

[0009] Furthermore, the bottom electrode and the top electrode are made of one or more of Pt, Au, Ru, W, Ti, Cu, ITO, TiN, AZO, and Al alloy, and the substrate is a semiconductor substrate, an insulator substrate, or a flexible polymer substrate having an insulating layer on the surface.

[0010] The method for preparing the inorganic-organic hybrid nano-thin film optoelectronic device simulating neural synapses comprises the following steps:

[0011] Vertical structure devices:

[0012] Step 1: preparing a bottom electrode on a substrate by atomic layer deposition, magnetron sputtering or other thin film deposition processes;

[0013] Step 2: growing an inorganic-organic hybrid film at 80-350° C. on the prepared bottom electrode by using a molecular layer deposition technique, and then preparing a metal oxide film as an inorganic layer on the inorganic-organic hybrid film at 80-350° C. by using an atomic layer deposition technique to obtain an inorganic-organic / inorganic double-layer stacked structure of an optoelectronic material layer; or first atomically depositing a metal oxide film, and then molecularly depositing an inorganic-organic hybrid film, to obtain an inorganic / inorganic-organic double-layer stacked structure of an optoelectronic material layer;

[0014] Step three, preparing a top electrode on the optoelectronic material layer by magnetron sputtering and evaporative deposition to obtain an inorganic-organic hybrid nano-thin film optoelectronic device that simulates neural synapses.

[0015] Planar structure devices:

[0016] Step 1: grow an inorganic-organic hybrid film at 80-350°C on a substrate using molecular layer deposition technology, and then prepare a metal oxide film as an inorganic layer on the inorganic-organic hybrid film at 80-350°C using atomic layer deposition technology to obtain an inorganic-organic / inorganic double-layer stack structure of a photoelectric material layer; or first atomically layer deposit a metal oxide film, and then molecularly layer deposit an inorganic-organic hybrid film to obtain an inorganic / inorganic-organic double-layer stack structure of a photoelectric material layer.

[0017] Step 2: Prepare interdigitated electrodes (or parallel strip electrodes) on the optoelectronic material layer by using magnetron sputtering and evaporation deposition process to obtain a complete optoelectronic device structure.

[0018] Beneficial effects-The present invention has the following significant features:

[0019] 1. Molecular layer deposition is used to prepare inorganic-organic hybrid nanofilms. Inorganic-organic elements can achieve molecular-level composites, combining the advantages of both inorganic and organic compounds. Metal oxide nanofilms prepared by atomic layer deposition are composited with inorganic-organic hybrid nanofilms and have excellent photoelectric properties. The molecular layer deposition and atomic layer deposition technologies used have a lower process temperature (80-350°C), are compatible with microelectronic processes, and are suitable for large-scale integration.

[0020] 2. The inorganic-organic hybrid nanofilm optoelectronic device constructed by the present invention has achieved several important functions of synapses, such as long-term potentiation (LTP), long-term depression (LTD), the transition from short-term plasticity to long-term plasticity, double pulse facilitation (PPF), learning, forgetting, and relearning, as well as classical conditioned reflex functions, and can successfully simulate the learning and memory functions of synapses;

[0021] 4. The present invention broadens the material selection of the optoelectronic functional layer, laying a foundation for the application of inorganic-organic hybrid materials in large-scale artificial neural network calculations. In addition, the hybrid materials are easy to design and process, which also provides broad prospects for subsequent applications in flexible bionic neuromorphic optoelectronic devices and wearable devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a schematic diagram of a planar structure optoelectronic device of the present invention;

[0023] Figure 2These are atomic force microscope (AFM) images of zinc-based hydroquinone and zinc oxide in the photoelectric material layer 3 of Example 1 of the present invention: (a) is an AFM image of zinc-based hydroquinone, and (b) is an AFM image of a surface on which zinc oxide is deposited;

[0024] Figure 3 is a photoresponse current curve diagram of the optoelectronic device of Example 1 of the present invention under light of 375 nm wavelength with different light intensities;

[0025] Figure 4 is a graph showing the variation trend of the light response current of the optoelectronic device of Example 1 of the present invention as the number of light pulses increases;

[0026] Figure 5 is a trend diagram of the light response current of the optoelectronic device of Example 1 of the present invention changing with the light pulse time;

[0027] Figure 6 is a curve diagram of the transition from short-term plasticity (STP) to long-term plasticity (LTP) of the optoelectronic device in Example 1 of the present invention;

[0028] Figure 7 is a paired pulse facilitation (PPF) index diagram of the optoelectronic device of Example 1 of the present invention;

[0029] Figure 8 This is a diagram of a simulated learning-forgetting-relearning experiment of an optoelectronic device in Example 1 of the present invention;

[0030] Fig. 9 This is a diagram of the experiment of simulating classical nerve reflex by the optoelectronic device of Example 1 of the present invention: (a) shows that the dog does not secrete saliva when hearing the bell alone, (b) shows that the dog secretes saliva when seeing food, (c) shows that the dog secretes saliva under the dual stimulation of food and bell, and (d) shows that the dog also secretes saliva when the food is removed and only the bell is kept;

[0031] Fig.10 is a photocurrent response curve diagram of the optoelectronic device of Example 2 of the present invention under 375nm wavelength light of different light intensities;

[0032] Fig.11 is a current-voltage curve diagram of the photoelectric device of Example 2 of the present invention under dark and light conditions;

[0033] Fig.12 is a photoresponse current diagram of the optoelectronic device of Example 2 of the present invention when different voltages are applied;

[0034] Fig.13 is a paired pulse facilitation (PPF) index diagram of the optoelectronic device of Example 2 of the present invention;

[0035] Fig.14The experimental diagrams of the photoelectric device simulation logic operation of the second embodiment of the present invention are as follows: (a) is the simulation of the logic operation of "OR", and (b) is the simulation of the logic operation of "AND";

[0036] Fig.15 is a schematic diagram of a vertical structure optoelectronic device of the present invention;

[0037] Fig.16 The photoelectric device with a vertical structure according to Example 3 of the present invention simulates the functions of long-term enhancement and long-term inhibition;

[0038] Fig.17 1 is a photoresponse current curve of the optoelectronic device of Comparative Example 1 of the present invention under light of 375 nm wavelength at different light intensities;

[0039] Fig.18 1 is a graph of the paired pulse facilitation (PPF) index of the optoelectronic device of Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0040] Example 1

[0041] A method for preparing an inorganic-organic hybrid nanofilm (Pt / ZnO / Zn-based hydroquinone / quartz) optoelectronic device for simulating neural synapses comprises the following steps:

[0042] (1) Growth of Photovoltaic Material Layer 3

[0043] The quartz wafer was ultrasonically cleaned in acetone, ethanol, isopropanol, and deionized water for 5 minutes respectively, and zinc-based hydroquinone and zinc oxide were sequentially deposited on the surface of the quartz substrate 1 by MLD and ALD methods to prepare the photoelectric material layer 3 thin film. The process conditions are: the growth temperature is 200°C, hydroquinone (C6H6O2), diethyl zinc (DEZ) and deionized water (H2O) are used as organic source, Zn source and O source respectively, the source temperature of hydroquinone is 130°C, and the source temperatures of diethyl zinc and deionized water are both room temperature. When MLD grows zinc-based hydroquinone, the cycle sequence of the precursor source is: hydroquinone (pulse 8s / cleaning 4s) + diethyl zinc (pulse 0.1s / cleaning 4s). When ALD grows zinc oxide, the cycle sequence of the precursor source is: diethyl zinc (pulse 0.1s / cleaning 4s) + water (pulse 0.1s / cleaning 4s). The source carrier gas and cleaning gas are both high-purity nitrogen (purity 99.999%), with a flow rate of 150 sccm. The thickness of the deposited film can be regulated by controlling the number of growth cycles.

[0044] The zinc-based hydroquinone film is about 50nm, and the zinc oxide film is about 10nm. Zinc-based hydroquinone has a nanoporous structure, such as Figure 2 The atomic force microscopy image shown, Figure 2 a Many uniformly distributed nanopores can be clearly observed. After zinc oxide is deposited, Figure 2 The number of holes in b is significantly reduced, indicating that zinc oxide effectively fills the holes and increases the area in contact with light, which is greatly beneficial for enhancing the photoelectric response of the device.

[0045] (2) Preparation of interdigitated electrodes 5

[0046] Platinum (Pt) was sputtered as an electrode by direct current magnetron sputtering. A mask was used to sputter interdigital electrodes 5 with an interdigital width and a gap of 100 μm. The sputtering current was 30 mA, the sputtering time was 600 s, and the sputtering thickness was 80 nm.

[0047] like Figure 1 The photoelectric device obtained in this embodiment is a planar structure device, which includes a quartz substrate 1, a photoelectric material layer 3, and a forked electrode 5 from bottom to top. The photoelectric material layer 3 is a double-layer nano stack structure composed of a zinc-based hydroquinone film and a zinc oxide film. The thickness of the inorganic-organic hybrid film 301 is 50nm, and the thickness of the metal oxide film 302 (zinc oxide film) is 10nm. The forked electrode 5 has a forked finger width and gap of 100μm and a thickness of 80nm.

[0048] The interdigital electrodes 5 in this embodiment can be replaced by indium tin oxide (ITO) or other conductive transparent materials, which are prepared by direct current sputtering and evaporation deposition processes.

[0049] The optoelectronic device of Example 1 was tested using a Keithly 4200 semiconductor parameter analyzer, a Keysight 33622A waveform generator, and an MDL series light source generator. A voltage was applied to one end of the interdigital electrode 5, and the other end was grounded. The light source was introduced into the gap between the interdigital electrodes through an optical fiber. Under 375 nm wavelength light of different powers, an obvious photoresponse current was measured at both ends of the interdigital electrode 5, and the photoresponse current increased with the increase of the light power, as shown in FIG. Figure 3 shown.

[0050] The device is continuously applied with a pulse width of 1 s and an optical power density of 2.3 mW / cm 2 The light pulses from Figure 4 It can be seen that as the number of light pulses increases, the photoresponse current gradually increases, and after 10 pulses, the increase in photocurrent is almost linearly related to the number of pulses. Figure 5 It can be seen that the photoresponse current increases with the increase of light pulse width, which is consistent with the general law of optoelectronic devices simulating neural synapses.

[0051] Simulate the transition from short-term potentiation (STP) to long-term potentiation (LTP) and paired-pulse facilitation (PPF). After applying a light pulse, the device will generate a light response current. After the light pulse ends, the response current will have a relaxation process, gradually decreasing to its original state over time. However, when the intensity of the applied light pulse is large enough, the number is large enough, and the time interval is small, the response current will take a longer time to return to its initial state after the pulse ends. This process realizes the transition from short-term plasticity to long-term plasticity, such as Figure 6 shown.

[0052] Double pulse facilitation is a manifestation of short-term plasticity. After applying a light pulse, there will be a peak value of the light response current A0. When the light pulse ends, the response current gradually decreases due to the relaxation process. When the response current decreases, the same light pulse is applied again, and a new response current peak value A1 will appear again. The PPF index is defined as the ratio of (A1-A0) to A0. Figure 7 As shown in Figure 1, as the time interval between two light pulses increases, the PPF index decreases.

[0053] Generally speaking, the learning experience of the human brain includes three processes: learning, forgetting and relearning, which can also be achieved by the optoelectronic device of this embodiment. First, by applying 30 light pulses, the current is increased from 78.5 to 95μA (equivalent to increasing the synaptic weight from 0 to 100%) to achieve the learning process. After the light stimulus disappears for 160s (forgetting process), the synaptic weight spontaneously drops from 100% to about 40%. Then, applying 15 consecutive light pulses can increase the synaptic weight back to 100%. It is worth noting that the number of light pulses used in the relearning process is less than the number of light pulses used in the first learning process, and after the same forgetting time, the second forgetting is less than the first. This shows that repeated stimulation helps to produce a faster relearning speed, which is similar to the transition from short-term memory (STM) to long-term memory (LTM).

[0054] Simulate the classic nerve reflex experiment. Fig. 9 , the device is at 10 1.6mW / cm 2 When stimulated by a 0.5s light pulse, the current gradually increases from 28.42μA to 28.93μA, but it is always lower than the threshold current of 29μA. This characteristic is similar to the dog in Figure (a) not secreting saliva when hearing the bell alone. 2When the light pulse is 0.5s, the first pulse current reaches the threshold current of 29μA, and the subsequent pulse currents are all greater than the threshold current. This characteristic is similar to the dog in Figure (b) secreting saliva when seeing food; but when the 1.6mW / cm 2 0.5s and 2.3mW / cm 2 0.5s light pulses were applied simultaneously (i.e. 3.9mW / cm 2 0.5s), and after multiple stimulations, the initial current of the device increased from 28.42μA to 28.6μA. At this time, 1.6mW / cm 2 When the light pulse is 0.5s, the current will quickly exceed 29μA. This characteristic is similar to the dog in Figures (c) and (d) who will secrete saliva after being trained with dual stimulation of food and bell, but only keeping the bell after the food is removed. These results simulate the classic synaptic conditioning experiment.

[0055] Example 2

[0056] A method for preparing an inorganic-organic hybrid nanofilm (Pt / SnO2 / Ti-based hydroquinone / quartz) optoelectronic device for simulating neural synapses comprises the following steps:

[0057] (1) Growth of Photovoltaic Material Layer 3

[0058] The quartz wafer was ultrasonically cleaned in acetone, ethanol, isopropanol, and deionized water for 5 minutes respectively, and Ti-based hydroquinone and tin oxide were deposited in sequence by MLD and ALD methods to prepare the photoelectric material layer 3 film. The process conditions are: growth temperature is 190℃, source temperature of hydroquinone is 130℃, source temperature of tetra(dimethylamino)tin is 60℃, and source temperature of titanium tetrachloride and deionized water is room temperature. When MLD grows Ti-based hydroquinone, the cycle sequence of the precursor source is: hydroquinone (pulse 8s / cleaning 4s) + titanium tetrachloride (pulse 0.1s / cleaning 4s); when ALD grows tin oxide, the cycle sequence of the precursor source is: tetra(dimethylamino)tin (pulse 0.2s / cleaning 6s) + water (pulse 0.2s / cleaning 6s). The carrier gas and cleaning gas of the source are both high-purity nitrogen (purity 99.999%), with a flow rate of 150sccm. By controlling the number of growth cycles, the thickness of the deposited film can be controlled. The thickness of Ti-based hydroquinone film is about 20nm, and that of tin oxide film is about 14nm.

[0059] (2) Preparation of interdigitated electrodes 5

[0060] Platinum (Pt) is sputtered as an electrode by direct current magnetron sputtering. A mask is used to sputter interdigitated electrodes 5 with a width and a gap of 100 μm. The sputtering current is 30 mA, the sputtering time is 600 s, and the sputtering thickness is 80 nm. In the actual operation process, indium tin oxide (ITO) or other conductive transparent materials can be used to prepare optoelectronic device electrodes by direct current sputtering and evaporation deposition processes.

[0061] The testing method of the optoelectronic device in this embodiment is the same as that in Embodiment 1.

[0062] like Fig.10 As shown, under different powers of 375 nm wavelength light, obvious photoresponse current is measured at both ends of the interdigital electrode 5, and the photoresponse current increases with the increase of light power.

[0063] like Fig.11 As shown, compared with the dark environment, the device is at 2.3mW / cm 2 Under the irradiation of 375nm wavelength light, the current-voltage curve increased by two orders of magnitude, showing excellent photoelectric response characteristics.

[0064] Different voltages are applied to one end of the interdigital electrode 5, ranging from 0.1V to 5V. Fig.12 It can be seen that the larger the reading voltage, the higher the photocurrent and the longer the retention time, showing higher learning and memory ability at a larger voltage.

[0065] Similar to Example 1, the photoelectric device of Example 2 can also realize double pulse facilitation, such as Fig.13 shown.

[0066] Simulate the logical operation of "OR" and "AND". Light with wavelengths of 375nm and 405nm is introduced into the interdigital gap of the device through optical fiber. When light pulse 1 (375nm) and light pulse 2 (405nm) are both at 2.5mW / cm 2 When the device is irradiated with a power of , whether light pulse 1 is applied alone, light pulse 2 is applied alone, or light pulses 1 and 2 are applied simultaneously, the response current is greater than the threshold current 4nA. Fig.14 As shown in (a), this characteristic can simulate the logical operation of "OR". 2 When the device is irradiated with a power of 1, the response current is less than the threshold current 4nA when light pulse 1 or light pulse 2 is applied alone. Only when light pulse 1 and light pulse 2 are applied at the same time, the response current is greater than the threshold current 4nA. Fig.14 As shown in (b), this feature can simulate the logical operation of "AND".

[0067] Example 3

[0068] A method for preparing an inorganic-organic hybrid nanofilm (Pt / ZnO / Zn-based hydroquinone / TiN / SiO2 / Si) photoelectric device for simulating neural synapses comprises the following steps:

[0069] (1) Preparation of bottom electrode 2

[0070] The Si substrate with SiO2 on the surface was ultrasonically cleaned in acetone, isopropanol and deionized water for 5 minutes, and a 10 nm thick TiN film was deposited on the SiO2 / Si substrate at 350°C using thermal ALD with TiCl4 and NH3 as Ti source and N source with pulse parameters of 1s TiCl4 / 5s N2 / 3s NH3 / 10s N2 as the bottom electrode 2.

[0071] (2) Preparation of Photoelectric Material Layer 3

[0072] The photoelectric material layer 3 thin film is prepared by sequentially depositing zinc-based hydroquinone and zinc oxide on the bottom electrode 2 using MLD and ALD methods. The specific process conditions are the same as those in Example 1.

[0073] (3) Preparation of top electrode 4

[0074] The top electrode 4 of the optoelectronic device is prepared by a DC sputtering deposition process using a platinum (Pt) conductive metal material. The edge of the device is scraped and coated with silver paste to lead out the bottom electrode 2 for testing. The test method is to apply voltage to the top electrode 4 and ground the bottom electrode 2, and the rest is the same as in Example 1.

[0075] The optoelectronic device obtained in this embodiment is a vertical structure device, such as Fig.15 As shown, from bottom to top, it includes SiO2 / Si substrate 1, bottom electrode 2, photoelectric material layer 3, and top electrode 4. Photoelectric material layer 3 is exactly the same as that in Example 1. Top electrode 4 is a circular Pt electrode with a diameter of 50 microns deposited by magnetron sputtering using a mask plate, and the deposition thickness is 30nm.

[0076] The test method is to apply voltage to the top electrode 4 and ground the bottom electrode 2. A 375nm light source and a 4225-RPM module are used to simulate the long-term potentiation (LTP) and long-term depression (LTD) functions of the vertical electrode structure photoelectric device of this embodiment. Fig.16 As shown. The optical pulse width used to enhance the current is 0.5s, the interval time is 0.5s, and the optical power density is 2.3mW / cm 2, 20 light pulses are applied continuously, and the current gradually increases; the width of the electric pulse used to suppress the current is 10μs, and the voltage is 0.6V. After each electric pulse is applied, the current of the device is read with a reading voltage of 0.1V. It can be seen that after applying 20 electric pulses, the current basically returns to the original value. This feature can be used to simulate the synaptic weights of the neural network model to perform the task of MNIST handwritten digit image recognition. After 140 iterations, the recognition accuracy is close to 90%.

[0077] Example 4

[0078] A method for preparing an inorganic-organic hybrid nanofilm (Ag / Ti-based maleic acid / TiO2 / TaN / SiO2 / Si) photoelectric device for simulating neural synapses comprises the following steps:

[0079] (1) Preparation of bottom electrode 2

[0080] The Si substrate with SiO2 on the surface was ultrasonically cleaned in acetone, isopropanol and deionized water for 5 minutes respectively, and then dried with N2. A TaN bottom electrode 2 with a thickness of 20 nm was sputtered on the substrate 1 at room temperature by magnetron sputtering.

[0081] (2) Preparation of Photoelectric Material Layer 3

[0082] The photoelectric material layer 3 thin film is prepared by sequentially depositing Ti-based maleic acid and titanium oxide on the bottom electrode 2 using the MLD and ALD methods. The process conditions are: the deposition temperature is 190°C, the source temperature of maleic acid is 125°C, and the source temperatures of titanium tetrachloride and deionized water are both room temperature. When MLD grows Ti-based maleic acid, the cycle sequence of the precursor source is: maleic acid (pulse 2s / cleaning 10s) + titanium tetrachloride (pulse 0.3s / cleaning 4s); when ALD grows titanium oxide, the cycle sequence is: titanium tetrachloride (pulse 0.1s / cleaning 4s) + water (pulse 0.1s / cleaning 4s). The carrier gas and cleaning gas of the source are both high-purity nitrogen (purity 99.999%), with a flow rate of 150sccm. By controlling the number of growth cycles, the thickness of the deposited film can be adjusted. The Ti-based maleic acid film is 25nm, and the titanium oxide film is 5nm.

[0083] (3) Preparation of top electrode 4

[0084] Ag is prepared as the top electrode 4 by magnetron sputtering. A circular electrode with a diameter of 100 microns is sputtered by using a mask plate. The deposition thickness is 8nm. In the actual operation process, conductive metal materials such as platinum (Pt) or ruthenium (Ru) can be used to prepare the top electrode 4 of the optoelectronic device by DC sputtering and evaporation deposition process. The edge of the device is scraped and coated with silver glue to lead out the bottom electrode 2 for testing. The test method is the same as that of Example 3.

[0085] Example 5

[0086] A method for preparing an inorganic-organic hybrid nanofilm (ITO / HfO2 / Hf-based p-aminophenol / Au / quartz) optoelectronic device for simulating neural synapses comprises the following steps:

[0087] (1) Preparation of bottom electrode 2

[0088] The quartz substrate was ultrasonically cleaned in acetone, isopropanol and deionized water for 5 minutes respectively, and then dried with N2. A plurality of parallel horizontal strip-shaped Au bottom electrodes 2 with a width of 50 μm and a thickness of 20 nm were deposited on the quartz substrate 1 through a mask by thermal evaporation.

[0089] (2) Preparation of Photoelectric Material Layer 3

[0090] The photoelectric material layer 3 thin film is prepared by sequentially depositing Hf-based p-aminophenol and hafnium oxide on the bottom electrode 2 using MLD and ALD methods. The process conditions are: the deposition temperature is 200°C, the source temperature of p-aminophenol is 130°C, and the source temperatures of tetrakis(dimethylamino)hafnium and deionized water are both at room temperature. When MLD grows Hf-based p-aminophenol, the cycle sequence of the precursor source is: p-aminophenol (pulse 8s / cleaning 4s) + tetrakis(dimethylamino)hafnium (pulse 1s / cleaning 5s); when ALD grows hafnium oxide, the cycle sequence is: tetrakis(dimethylamino)hafnium (pulse 1s / cleaning 5s) + water (pulse 0.1s / cleaning 4s). The carrier gas and cleaning gas of the source are both high-purity nitrogen (purity 99.999%), with a flow rate of 150sccm. By controlling the number of growth cycles, the thickness of the deposited film can be adjusted. The Hf-based p-aminophenol film is 30nm, and the hafnium oxide film is 10nm.

[0091] (3) Preparation of top electrode 4

[0092] ITO was prepared as the top electrode 4 by magnetron sputtering. A plurality of parallel vertical strips of ITO top electrodes 4 with a width of 50 μm and a thickness of 20 nm were sputtered using a mask plate, perpendicular to the bottom electrode 2. The edge of the bottom electrode 2 of the device was scraped and coated with silver glue to lead out the bottom electrode 2 for testing. The testing method was the same as that of Example 3.

[0093] Example 6

[0094] A method for preparing an inorganic-organic hybrid nanofilm (AZO / Al-based hydroquinone / MoO3 / PET) optoelectronic device for simulating neural synapses comprises the following steps:

[0095] (1) Growth of Photovoltaic Material Layer 3

[0096] PET was ultrasonically cleaned in acetone, ethanol, isopropanol, and deionized water for 5 minutes respectively, and Al-based hydroquinone and molybdenum oxide were deposited in sequence by MLD and ALD methods to prepare the photoelectric material layer 3 film. The process conditions are: growth temperature is 250℃, source temperature of hydroquinone is 130℃, source temperature of tetrakis(dimethylamino)molybdenum is 60℃, and source temperature of trimethylaluminum and deionized water is room temperature. When MLD grows Al-based hydroquinone, the cycle sequence of the precursor source is: hydroquinone (pulse 8s / cleaning 4s) + trimethylaluminum (pulse 0.1s / cleaning 4s); when ALD grows molybdenum oxide, the cycle sequence of the precursor source is: tetrakis(dimethylamino)molybdenum (pulse 1s / cleaning 6s) + water (pulse 0.1s / cleaning 6s). The carrier gas and cleaning gas of the source are both high-purity nitrogen (purity 99.999%), with a flow rate of 150sccm. By controlling the number of growth cycles, the thickness of the deposited film can be controlled. The thickness of the molybdenum oxide film is about 10 nm, and that of the Al-based hydroquinone film is about 30 nm.

[0097] (2) Preparation of interdigitated electrodes 5

[0098] AZO was sputtered as an electrode by magnetron sputtering. A mask was used to sputter a finger electrode 5 with a finger width and a gap of 100 μm, and a sputtering thickness of 30 nm. In the actual operation process, indium tin oxide (ITO) or other conductive transparent materials can be used to prepare optoelectronic device electrodes by direct current sputtering and evaporation deposition processes. The test method is the same as that of Example 1.

[0099] Among the above embodiments, the best embodiments are Embodiment 1 and Embodiment 3.

[0100] Comparative Example 1

[0101] The remaining steps of this comparative example are the same as those of Example 1, except that the thickness of the metal oxide film (302) zinc oxide film in the photoelectric material layer (3) is about 3 nm. Photoelectric response test and double pulse facilitation function simulation were performed, and it was found that under different powers of 375 nm wavelength light, although the photoresponse current was measured, compared with Example 1, the photoresponse intensity was very weak, only in the pA order, such as Fig.17 When simulating the double pulse facilitation function, the PPF index is significantly smaller than that of Example 1, as shown in FIG. Fig.18 As shown. This shows that the thickness of the metal oxide in the optoelectronic material layer has a great influence on the optoelectronic performance of the device. This discovery has important guiding significance for the design and preparation of high-performance optoelectronic devices.

Claims

1. An inorganic-organic hybrid nanofilm optoelectronic device that simulates neural synapses, Features: The vertical structure comprises, from bottom to top, a substrate (1), a bottom electrode (2), a photoelectric material layer (3), and a top electrode (4); the photoelectric material layer (3) is a double-layer nano-stack structure composed of an inorganic-organic hybrid film (301) and a metal oxide film (302); the inorganic-organic hybrid film (301) is metal-based hydroquinone, metal-based p-aminophenol or metal-based maleic acid, and the metal oxide film (302) is ZnO, TiO 2 , HfO 2 、ZrO 2 、MoO 3 、 2 O 5 ,GeO 2 , WO 3 SnO 2 Or IGZO.

2. The inorganic-organic hybrid nano-thin film optoelectronic device simulating neural synapses according to claim 1, Features: The thickness of the inorganic-organic hybrid film (301) is 5 to 50 nm, and the thickness of the metal oxide film (302) is 5 to 20 nm.

3. The inorganic-organic hybrid nano-thin film optoelectronic device simulating neural synapses according to claim 1, Features: The metal base of the inorganic-organic hybrid film (301) is one or more of Al, Ti, Zn, Sn, Hf, Zr, Ni, and Co.

4. The inorganic-organic hybrid nano-thin film optoelectronic device simulating neural synapses according to claim 1, Features: The bottom electrode (2) and the top electrode (4) are made of one or more of Pt, Au, Ru, W, Ti, Cu, ITO, TiN, AZO, and Al alloy, and the substrate (1) is a semiconductor substrate, an insulator substrate, or a flexible polymer substrate having an insulating layer on the surface.

5. A method for preparing the inorganic-organic hybrid nano-thin film optoelectronic device simulating neural synapses according to any one of claims 1 to 4, It is characterized in that The following steps are involved: Step 1: preparing a bottom electrode (2) on a substrate (1); Step 2: using molecular layer deposition and atomic layer deposition methods to grow a photoelectric material layer (3) on the prepared bottom electrode (2) at 80 to 350° C.; Step three, preparing a top electrode (4) on the optoelectronic material layer (3) by magnetron sputtering and evaporation deposition, thereby obtaining an inorganic-organic hybrid nano-thin film optoelectronic device that simulates a neural synapse.

6. An inorganic-organic hybrid nanofilm optoelectronic device that simulates neural synapses, Features: The planar structure comprises, from bottom to top, a substrate (1), a photoelectric material layer (3), and an interdigitated electrode (5); the photoelectric material layer (3) is a double-layer nano-stack structure composed of an inorganic-organic hybrid film (301) and a metal oxide film (302); the inorganic-organic hybrid film (301) is metal-based hydroquinone, metal-based p-aminophenol or metal-based maleic acid, and the metal oxide film (302) is ZnO, TiO 2 , HfO 2 、ZrO 2 、MoO 3 、 2 O 5 ,GeO 2 , WO 3 SnO 2 Or IGZO.

7. The inorganic-organic hybrid nano-thin film optoelectronic device for simulating neural synapses according to claim 6, Features: The thickness of the inorganic-organic hybrid film (301) is 5 to 50 nm, and the thickness of the metal oxide film (302) is 5 to 20 nm.

8. The inorganic-organic hybrid nano-thin film optoelectronic device for simulating neural synapses according to claim 6, Features: The metal base of the inorganic-organic hybrid film (301) is one or more of Al, Ti, Zn, Sn, Hf, Zr, Ni, and Co.

9. The inorganic-organic hybrid nano-thin film optoelectronic device simulating neural synapses according to claim 6, Features: The interdigitated electrodes (5) may also be parallel strip electrodes, and the substrate (1) is a semiconductor substrate, an insulator substrate or a flexible polymer substrate having an insulating layer on the surface.

10. A method for preparing the inorganic-organic hybrid nano-thin film optoelectronic device simulating neural synapses according to any one of claims 6 to 9, It is characterized in that The following steps are involved: Step 1: growing a photoelectric material layer (3) on a substrate (1) at 80 to 350° C. by using a molecular layer deposition or atomic layer deposition method; Step 2: preparing interdigitated electrodes (5) on the optoelectronic material layer (3) by magnetron sputtering and evaporative deposition to obtain an inorganic-organic hybrid nano-thin film optoelectronic device simulating a neural synapse.

Citation Information

Cited By

  • Erasable organic-inorganic hybrid patterned film prepared by molecular layer deposition

    CN120122387A