In-situ synthesis method and application of amorphous Cu2O / biomass carbon catalyst

By generating amorphous Cu2O in situ on biomass carbon to form a Cu2O/biomass carbon catalyst, the problem of difficulty in obtaining and high cost of precious metal catalysts is solved, the effect of efficient PNP degradation is achieved, the treatment cost is reduced, and solid Resource utilization of waste.

CN115106083BActive Publication Date: 2024-10-22ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210749704.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-28
Publication Date
2024-10-22
Estimated Expiration
2042-06-28

AI Technical Summary

Technical Problem

In the existing technology, noble metal catalysts are difficult to obtain and costly, making it difficult to achieve a green and efficient NaBH4 reduction reaction when degrading nitrophenol (PNP). Finding a green and efficient non-precious metal catalyst is still a huge challenge.

Method used

By generating amorphous Cu2O in situ in a dispersion system containing biomass carbon, loading it on the biomass carbon, and using sodium borohydride to reduce copper nitrate, an amorphous Cu2O/biomass carbon catalyst is formed, which is used to catalytically reduce PNP to Para-aminophenol.

Benefits of technology

An amorphous Cu2O/biomass carbon catalyst with excellent catalytic activity and high selectivity has been realized, which can quickly degrade more than 90% of PNP at room temperature and pressure. All the conversion products are p-aminophenol, and no by-products are generated, reducing treatment costs. , and realize resource utilization of solid waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115106083B_ABST
    Figure CN115106083B_ABST
Patent Text Reader

Abstract

The invention discloses an in-situ synthesis method and application of an amorphous Cu2O / biomass carbon catalyst; the in-situ generation method comprises the following steps: first, grinding pecan shells, washing, drying, grinding, and screening to obtain biomass carbon; second, burning the biomass carbon in a nitrogen atmosphere to obtain biomass carbon powder; third, adding the biomass carbon powder obtained in step 2 to ultrapure water; continuously introducing oxygen into the obtained dispersion system, and dropping Cu(NO3)2 solution and NaBH4 solution to obtain Cu2O / biomass carbon powder; and finally adding Cu(NO3)2 solution and NaBH4 solution to the dispersion system. 2+ Reduced to Cu2O and loaded on biomass carbon. Afterwards, the solid phase in the dispersion is separated to obtain a catalyst. The amorphous Cu2O / biomass carbon catalyst prepared by the present invention has excellent catalytic activity and extremely high selectivity, and can degrade more than 90% of PNP within 5 minutes, and the conversion products are all p-aminophenol, without other by-products, and no secondary pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for in-situ synthesizing an amorphous Cu2O / biomass carbon catalyst and application thereof. Background Art

[0002] p-Nitrophenol (PNP) and its derivatives are typical aromatic pollutants emitted by industries such as pesticides, fuels, and herbicides. The treatment of such pollutants is a challenge for researchers. Among nitroaromatic compounds, nitrophenol compounds are generally highly toxic and carcinogenic. p-Aminophenol (PAP) obtained by reducing PNP is a very useful organic chemical raw material intermediate used in dyes, pharmaceuticals, photosensitive materials, antioxidants and other industries, and the toxicity of PAP is much less than that of PNP.

[0003] In the past few decades, people have devoted their efforts to remove PNP from wastewater. Common methods include chemical reduction, solid phase extraction, photocatalysis and Fenton oxidation. In the existing technology, NaBH4 is used as a reducing agent to reduce PNP to harmless p-aminophenol (PAP), which has attracted widespread attention due to its simple operation, high conversion efficiency and great industrial relevance. Many precious metals such as Ag, Ru, Au, and Pd are widely used as catalysts for this reaction. However, the difficulty in obtaining precious metals and their high cost limit their practical engineering applications. Therefore, researchers are committed to the exploration of non-precious metal catalysts to reduce costs. However, the catalytic performance and stability of non-precious metals are difficult to achieve the desired effect. So far, it is still a huge challenge to find a green, efficient and large-scale engineering application catalyst for the NaBH4 reduction and degradation of PNP reaction. Summary of the invention

[0004] In view of the above technical problems existing in the prior art, the object of the present invention is to provide an in-situ synthesized amorphous Cu2O / biomass carbon catalyst and a preparation method and application thereof.

[0005] In a first aspect, the present invention provides an amorphous Cu2O / biomass carbon catalyst, which is obtained by in-situ generating Cu2O in a dispersion system containing biomass carbon, so that Cu2O is loaded on biomass carbon. The in-situ generating Cu2O is: using sodium borohydride to reduce copper nitrate in a dispersion system containing biomass carbon to obtain Cu2O.

[0006] Preferably, the sodium borohydride solution and the copper nitrate solution are simultaneously added dropwise to the dispersion system containing the biomass carbon while maintaining oxygen flow, so that the in-situ generated Cu2O is evenly loaded on the biomass carbon.

[0007] Preferably, the biomass carbon is obtained by grinding pecan shells into powder.

[0008] The in-situ generation method of the amorphous Cu2O / biomass carbon catalyst comprises the following steps:

[0009] Step 1: After grinding the pecan shells into pecan particles, the obtained pecan particles are washed, dried, ground, and sieved to obtain biomass carbon with a mesh size of more than 100.

[0010] Step 2: burning the biomass carbon obtained in step 1 under a nitrogen atmosphere to obtain biomass carbon powder;

[0011] Step 3: Add the biomass carbon powder obtained in step 2 into ultrapure water; continue to introduce oxygen into the obtained dispersion, and dropwise add Cu(NO3)2 solution and NaBH4 solution to 2+ The Cu2O is reduced to Cu2O and loaded on biomass carbon. After that, the solid phase in the dispersion is separated to obtain an amorphous Cu2O / biomass carbon catalyst.

[0012] Preferably, in step 2, the flow rate of nitrogen is 4 mol / h.

[0013] Preferably, in step 2, the calcination temperature is 250°C.

[0014] Preferably, in step three, the solid phase in the dispersion is separated by washing and air-drying after centrifugation.

[0015] Preferably, in step three, the reaction temperature is 10-50°C.

[0016] Preferably, in step 3, the concentration of the Cu(NO3)2 solution is 0.2 mmol·L -1 ; NaBH4 solution concentration is 26 mmol·L -1 .

[0017] In a second aspect, the present invention provides the use of the aforementioned amorphous Cu2O / biomass carbon catalyst for catalytic reduction of p-nitrophenol in wastewater.

[0018] Preferably, a hydrogen-containing reducing agent is added during the catalytic reduction of p-nitrophenol, so that p-nitrophenol generates p-aminophenol.

[0019] Preferably, the hydrogen-containing reducing agent is sodium borohydride.

[0020] Preferably, the reaction temperature for the catalytic reduction of p-nitrophenol is 25°C.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The amorphous Cu2O / biomass carbon catalyst prepared by the present invention has excellent catalytic activity and extremely high selectivity, and can degrade more than 90% of PNP within 5 minutes, and all the conversion products are p-aminophenol, without any other by-products, and no secondary pollution will be generated.

[0023] 2. The catalyst provided by the present invention uses Cu to replace general precious metal raw materials, and the catalyst provided by the present invention has simple application conditions and no special requirements for reaction equipment, and can catalytically reduce PNP at normal temperature and pressure, which greatly reduces the treatment cost of PNP wastewater.

[0024] 3. The present invention uses waste walnut shells as raw materials and adopts a green and environmentally friendly method to synthesize amorphous Cu2O / biomass carbon catalyst, thereby realizing the resource utilization of solid waste. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The figure is a diagram showing the catalytic degradation effect of the catalyst prepared in the present invention on PNP;

[0026] Figure 2 The X-ray photoelectron spectrum of the catalyst prepared by the present invention;

[0027] Figure 3 The X-ray diffraction pattern of the catalyst prepared in the present invention. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0029] An in-situ synthesis method of an amorphous Cu2O / biomass carbon catalyst comprises the following steps:

[0030] Step 1: Grind the discarded pecan shells into pecan particles; then, wash the obtained pecan particles with pure water, naturally air-dry, grind, and sieve to obtain pecan powder with a mesh size of more than 100. The obtained pecan powder is biomass carbon.

[0031] Step 2: burning the biomass carbon obtained in step 1 under a nitrogen atmosphere to obtain biomass carbon powder;

[0032] Step 3: Add the prepared biomass carbon powder into a customized device filled with ultrapure water; then continue to introduce oxygen into the obtained dispersion system while continuously adding 0.2 mmol·L -1 Cu(NO3)2 solution and 26mmol·L -1 The whole process was carried out in a water bath at 30°C. After the dispersion system after the reaction was centrifuged, the obtained solid phase was washed with ethanol and naturally air-dried to obtain an amorphous Cu2O / biomass carbon catalyst.

[0033] The obtained amorphous Cu2O / biomass carbon catalyst was applied to the catalytic degradation of PNP-containing wastewater, and the process was as follows:

[0034] Add 54 mL of a mixed solution of PNP and freshly prepared NaBH4 (the molar concentration of NaBH4 is 26 mmol·L) into a 100 mL beaker. -1 , the molar concentration of PNP is 0.13mmol·L -1 ), place the beaker in a 30°C constant temperature water bath, add 0.1g of amorphous Cu2O / biomass carbon catalyst, and stir continuously during the reaction. Take samples from the beaker every 1 minute, and measure the PNP concentration in the sample using a UV spectrophotometer. The results are as follows Figure 1 As shown. Figure 1 It can be seen that after adding the catalyst prepared in this example, the concentration of PNP decreases rapidly, and after 5 minutes of reaction, PNP is completely degraded. In addition, during the reaction, the product peak only appears at the absorption wavelength (300 nm) corresponding to PNP, which shows that the catalyst prepared in this example has extremely high selectivity.

[0035] The chemical composition of the amorphous Cu2O / biomass carbon catalyst prepared by the above method was analyzed by X-ray photoelectron spectroscopy (XPS, Thermo Scientific K-Alpha), using an Al Kα X-ray source (hν=1486.6eV). Figure 2 As shown in the figure, the catalyst prepared in this embodiment has two obvious peaks at binding energies of 931.6eV and 951.8eV, corresponding to Cu 2p1 / 2 and Cu 2p3 / 2, respectively. The O1s energy spectrum in the figure shows that there is only one O peak in the sample, which appears at 532.4eV. The Cu 2p and O1s energy spectra show that the only existing form of Cu in the catalyst is Cu2O, indicating that the preparation method provided in this embodiment can make full use of the raw materials and obtain a catalyst with high catalytic efficiency.

[0036] The amorphous Cu2O / biomass carbon catalyst prepared by the above method was determined by X-ray diffraction (XRD, Rigaku Ultima IV). Figure 3 As shown in the figure, it can be seen that the catalyst does not produce an obvious absorption peak corresponding to Cu, which indicates that the catalyst generates an amorphous Cu2O. Amorphous Cu2O is more likely to produce defects, and most of these defects are active sites for catalytic reactions.

Claims

1. An in-situ synthesis method of an amorphous Cu2O / biomass carbon catalyst, characterized in that: Step 1: After grinding the pecan shell into pecan particles, the obtained pecan particles are washed, dried, ground, and sieved to obtain biomass carbon with a mesh size of more than 100; Step 2: Burn the biomass carbon obtained in step 1 under a nitrogen atmosphere to obtain biomass carbon powder; the flow rate of nitrogen is 4 mol / h, and the burning temperature is 250° C.; Step 3: Add the biomass carbon powder obtained in step 2 into ultrapure water; continue to introduce oxygen into the obtained dispersion, and dropwise add Cu(NO3)2 solution and NaBH4 solution to 2+ The catalyst was reduced to Cu2O and loaded on biomass carbon. Then, the solid phase in the dispersion was separated by centrifugation, washing and air drying to obtain an amorphous Cu2O / biomass carbon catalyst. The concentration of the Cu(NO3)2 solution was 0.2 mmol∙L -1 ; NaBH4 solution concentration is 26 mmol∙L -1 ; The reaction temperature is 10~50℃.

2. An amorphous Cu2O / biomass carbon catalyst, characterized in that: It is prepared by the in-situ synthesis method described in claim 1.

3. Use of the amorphous Cu2O / biomass carbon catalyst as claimed in claim 2 for catalytic reduction of p-nitrophenol in wastewater.

4. The use according to claim 3, characterized in that: A hydrogen-containing reducing agent is added during the catalytic reduction of p-nitrophenol, so that p-nitrophenol generates p-aminophenol.

5. The use according to claim 3, characterized in that: The reaction temperature for the catalytic reduction of p-nitrophenol is 25°C.