Release composition

By adjusting the molar ratio of siloxane units through the polyorganosiloxane composition, the problems of poor curing, low residual adhesion rate and insufficient binding force of the silicone release layer are solved, and stable release at room temperature and high temperature is achieved. Balanced type characteristics and peeling force.

CN118829698APending Publication Date: 2024-10-22LG CHEM LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380024306.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-22
Filing Date
2023-03-22
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing release layers based on silicone have problems with poor curing, low residual adhesion rate and insufficient bonding force. It is difficult to maintain release properties at room temperature and high temperature, and there is a lack of balance between high-speed peeling force and low-speed peeling force.

Method used

The polyorganosiloxane composition is used to form a release layer with excellent curability by adjusting the molar ratio and structure of the siloxane units, ensuring stable release properties at room temperature and high temperature, and at high and low speeds. Maintain balanced peeling force during peeling.

Benefits of technology

Stable curing of the release layer is achieved, maintaining a stable residual adhesion rate and desired release characteristics over multiple applications, ensuring appropriate peel force balance under different temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005016940780000291
    Figure BDA0005016940780000291
  • Figure BDA0005016940780000301
    Figure BDA0005016940780000301
  • Figure BDA0005016940780000311
    Figure BDA0005016940780000311
Patent Text Reader

Abstract

The invention provides a release composition, a release layer, a release film and a pressure-sensitive adhesive film. The release composition of the present application has excellent curability, and thus can be stably cured to form a release layer. When a release layer has been formed, the present application can provide a release composition that allows a stable residual adhesion rate to be exhibited even if the release layer is repeatedly applied to a pressure-sensitive adhesive layer or the like. The release layer of the present application can maintain desired release characteristics even at room temperature and high temperature for a long period of time. In addition, the release layer can stably maintain the balance between the high-speed release force and the low-speed release force.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority based on Korean Patent Application No. 10-2022-0035335 filed on March 22, 2022, the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0004] The present application relates to a release composition, a release layer, a release film and a pressure-sensitive adhesive film. Background Art

[0005] Release films are used to protect the surface of pressure-sensitive adhesives or adhesive surfaces, as carriers, and as coating base materials. For example, so-called light or medium-thin release films can be used to protect optically clear adhesives (OCA). In addition, release films can be used as carriers for tapes, etc., or as coating base materials for multi-layer ceramic capacitors (MLCCs), etc.

[0006] For example, Patent Document 1 discloses a release sheet having a release layer (release layer) formed of a release agent composition (release composition) containing a polyolefin, an isocyanate compound, and a polyolefin polyol.

[0007] In addition to the method disclosed in Patent Document 1, the release layer of the release film may also be formed using a silicone-based compound.

[0008] However, compared with release layers formed using non-organosilicon-based compounds, release layers formed using silicone-based compounds have problems of poor curing or low residual adhesion rate. In addition, such release layers generally do not have high bonding strength with the base film, and when they are attached to the base film for a long time, the pressure-sensitive adhesive force tends to increase.

[0009] Therefore, it is an important task to maintain the release peeling characteristics of the release layer even when the release layer is kept at room temperature and high temperature for a long time while ensuring appropriate curability and a high residual adhesion rate.

[0010] In addition, in terms of using the product or assembling other products, the release film needs to have a relatively low peeling force when peeling the protective film at a high speed (hereinafter, referred to as a high-speed peeling force). On the other hand, the peeling force when peeling at a low speed (hereinafter, referred to as a low-speed peeling force) needs to be relatively high.

[0011] If the release film does not have a suitable low-speed peel force, quality problems may occur, and if it does not have a suitable high-speed peel force, problems may occur in which the adherend is damaged during peeling. Therefore, having a balance between high-speed peel force and low-speed peel force is an important task for the release film.

[0012] (Patent Document 0001) Japanese Patent Publication No. 2011-52207 Summary of the invention

[0013] Technical issues

[0014] The present application provides a release composition, a release layer, a release film and a pressure-sensitive adhesive film.

[0015] The present application aims to provide a release composition capable of forming a release layer, wherein the release composition has excellent curability and can be stably cured.

[0016] When a release layer has been formed, the present application aims to provide a release composition that allows a stable residual adhesion rate to be exhibited even if the release layer is repeatedly applied to a pressure-sensitive adhesive layer or the like.

[0017] The present application aims to provide a release layer that can maintain desired release properties even when the release layer is kept at room temperature and high temperature for a long time.

[0018] In addition, the present application aims to provide a release layer that can stably maintain a balance between high-speed peeling force and low-speed peeling force.

[0019] Technical Solution

[0020] Among the physical properties mentioned in this specification, when measuring the influence of temperature on the relevant physical properties, the relevant physical properties are physical properties measured at room temperature unless otherwise specified.

[0021] The term room temperature is a natural temperature without artificial heating and cooling, which may mean, for example, any temperature in the range of 10°C to 30°C, or a temperature of about 27°C or lower and about 15°C or higher, about 18°C ​​or higher, about 20°C or higher, or about 23°C or higher, or a temperature of about 25°C or so.

[0022] Unless otherwise specified, the unit of temperature in this specification is ° C.

[0023] Among the physical properties mentioned in this application, when the measurement pressure affects the relevant physical properties, unless otherwise specified, the relevant physical properties are the physical properties measured under normal pressure.

[0024] In the present specification, the term "normal pressure" is a natural pressure without artificial pressurization or decompression, which may mean, for example, any pressure within the range of 0.9 atmospheres to 1.2 atmospheres or any pressure within the range of about 740 mmHg to 780 mmHg.

[0025] The term relative humidity as used in this application is expressed as a percentage (%) of the ratio of the amount of water vapor contained in the current air per unit volume to the saturated vapor pressure that the air per unit volume can contain at most, which can be expressed as RH%. Among the physical properties mentioned in this application, when relative humidity affects the physical properties, the relevant physical properties are the physical properties measured in a humid environment (about 30RH% to 70RH%) unless otherwise specified.

[0026] The term "a to b" as used in the present application means "within the range of a to b, including both a and b." For example, the fact that a to b parts by weight is included has the same meaning as comprising in the range of a to b parts by weight.

[0027] In this specification, the terms weight average molecular weight (Mw) and number average molecular weight (Mn) are

[0028] A physical property measured using GPC (gel permeation chromatography), and the term polydispersity index (PDI) is

[0029] A value (Mw / Mn) obtained by dividing the weight average molecular weight (Mw) by the number average molecular weight (Mn).

[0030] The unit of weight average molecular weight (Mw) and number average molecular weight (Mn) mentioned in this specification is g / mol.

[0031] Specific methods for measuring weight average molecular weight (Mw), number average molecular weight (Mn), and polydispersity index are summarized in the Examples section.

[0032] In this specification, unless otherwise stated, the term alkyl or alkoxy can be a linear or branched alkyl or alkoxy with 1 to 20 carbon atoms, or 1 to 16 carbon atoms, or 1 to 12 carbon atoms, or 1 to 8 carbon atoms, or 1 to 6 carbon atoms, or 1 to 4 carbon atoms, or can be a cyclic alkyl or alkoxy with 3 to 20 carbon atoms, or 3 to 16 carbon atoms, or 3 to 12 carbon atoms, or 3 to 8 carbon atoms, or 3 to 6 carbon atoms. Cyclic alkyl or alkoxy also includes alkyl or alkoxy with only ring structure, and alkyl or alkoxy containing ring structure. For example, cyclohexyl and methylcyclohexyl correspond to cyclic alkyl.

[0033] In this specification, unless otherwise specified, the term alkenyl can be a linear or branched acyclic alkenyl having 2 to 20 carbon atoms, or 2 to 16 carbon atoms, or 2 to 12 carbon atoms, or 2 to 8 carbon atoms, or 2 to 6 carbon atoms, or 2 to 4 carbon atoms, or can be a cyclic alkenyl having 3 to 20 carbon atoms, or 3 to 16 carbon atoms, or 3 to 12 carbon atoms, or 3 to 8 carbon atoms, or 3 to 6 carbon atoms. Here, the category of cyclic alkenyl also includes alkenyl having only a ring structure and alkenyl containing a ring structure.

[0034] In this specification, unless otherwise indicated, the term alkynyl can be a linear or branched acyclic alkynyl having 2 to 20 carbon atoms, or 2 to 16 carbon atoms, or 2 to 12 carbon atoms, or 2 to 8 carbon atoms, or 2 to 6 carbon atoms, or 2 to 4 carbon atoms, or can be a cyclic alkynyl having 3 to 20 carbon atoms, or 3 to 16 carbon atoms, or 3 to 12 carbon atoms, or 3 to 8 carbon atoms, or 3 to 6 carbon atoms. Here, if an alkynyl having a ring structure is included, it corresponds to a cyclic alkynyl.

[0035] Alkyl, alkoxy, alkenyl and alkynyl may also be substituted with any one or more substituents. In this case, the substituent may be one or more selected from the following: halogen (chlorine (Cl), iodine (I), bromine (Br), fluorine (F)), aryl, heteroaryl, epoxy, alkoxy, cyano, carboxyl, acryloyl, methacryloyl, acryloyloxy, methacryloyloxy, carbonyl and hydroxyl, but not limited thereto.

[0036] In the present specification, the term aryl group means a substituent formed by removing one hydrogen from an aromatic hydrocarbon ring compound, wherein the aromatic hydrocarbon ring compound may be a monocyclic or polycyclic compound. The number of carbon atoms of the aryl group is not particularly limited, but unless otherwise specified, the aryl group may be an aryl group having 6 to 20 carbon atoms, 6 to 18 carbon atoms, or 2 to 15 carbon atoms.

[0037] The aryl group may be exemplified by phenyl, phenylethyl, phenylpropyl, benzyl, tolyl, xylyl, naphthyl, or the like, but is not limited thereto.

[0038] The aryl group may also be optionally substituted with one or more substituents. In this case, the substituent may be one or more selected from the following: halogen (chlorine (Cl), iodine (I), bromine (Br), fluorine (F)), aryl, heteroaryl, epoxy, alkoxy, cyano, carboxyl, acryloyl, methacryloyl, acryloyloxy, methacryloyloxy, carbonyl and hydroxyl, but is not limited thereto.

[0039] In this specification, the term monovalent hydrocarbon group means a monovalent substituent derived from a hydrocarbon (an organic compound consisting of carbon and hydrogen). The carbon number of such a monovalent hydrocarbon group can be in the range of 1 to 20, 1 to 16, 1 to 12, 1 to 8 or 1 to 4. Examples of monovalent hydrocarbon groups include alkyl, alkenyl, alkynyl or aryl. Alkyl, alkenyl, alkynyl or aryl can each be an alkyl, alkenyl, alkynyl or aryl group as specifically described at the beginning of this specification.

[0040] The present application relates to a release composition. The term release composition means a composition capable of forming a release layer, and in this case, the meaning of a release layer is as known in the industry.

[0041] The release composition may be a curable composition, and in this case, the composition may form a release layer before or after curing.

[0042] The release composition of the present application may include a polyorganosiloxane component.

[0043] As is known, the term polyorganosiloxane means a polymer comprising a chain formed by siloxane bonds (Si-O-Si). The polyorganosiloxane mentioned in this specification may be a monomolecular polyorganosiloxane or a mixture of bimolecular or higher polyorganosiloxanes. Polyorganosiloxanes are polymer compounds, and in some cases, only monomolecular polymers are produced in the polymerization process for forming the polymer compound, but in some cases, bimolecular or higher polymers are produced, so that the meaning of the term polyorganosiloxane also includes mixtures of bimolecular or higher polyorganosiloxanes.

[0044] The polyorganosiloxane is generally formed by containing one or more siloxane units selected from so-called M units, D units, T units, and Q units.

[0045] In the present specification, the M unit is a so-called monofunctional siloxane unit (ie, a siloxane unit having a structure in which a silicon atom is bonded to one oxygen atom), which can be generally represented by (R3SiO 1 / 2 ); the D unit is a so-called difunctional siloxane unit (i.e., a siloxane unit having a structure in which a silicon atom is connected to two oxygen atoms), which can be generally represented as (R2SiO 2 / 2 ); T unit is a so-called trifunctional siloxane unit (i.e., a siloxane unit having a structure in which a silicon atom is connected to three oxygen atoms), which can be generally represented as (RSiO 3 / 2 ); and the Q unit is a so-called tetrafunctional siloxane unit (i.e., a siloxane unit having a structure in which a silicon atom is connected to four oxygen atoms), which can be generally represented as (SiO 4 / 2 ).

[0046] The polyorganosiloxane of the present application includes specific siloxane units, and thus it can form the release layer intended in the present application.

[0047] As described above, the polyorganosiloxane may be a monomolecular polyorganosiloxane or a mixture of bimolecular or higher polyorganosiloxanes. For example, the monomolecular polyorganosiloxane or the mixture of bimolecular or higher polyorganosiloxanes may have the following average units.

[0048] The polyorganosiloxane component of the present application may be a polyorganosiloxane having a siloxane unit of the following Formula 1, a siloxane unit of the following Formula 2, and a siloxane unit of the following Formula 3.

[0049] [Formula 1]

[0050] (R 1 2SiO 2 / 2 )

[0051] [Formula 2]

[0052] (R 1 R 2 SiO 2 / 2 )

[0053] [Formula 3]

[0054] (R 3 2SiO 2 / 2 )

[0055] In equations 1 to 3, R 1 It can be an alkyl group, R 2 It can be an alkenyl group, and R 3 Specific types of the alkyl group, alkenyl group and aryl group contained in Formulae 1 to 3 are as described at the beginning of this specification.

[0056] The ratio of the total moles of the siloxane units of the above formulas 1 to 3 can be adjusted based on the total moles of all siloxane units contained in the polyorganosiloxane of the present application. For example, the lower limit of the ratio of the total moles of the siloxane units of formulas 1 to 3 (based on the total moles of all siloxane units) can be 85mol%, 86mol%, 87mol%, 88mol%, 89mol%, 90mol%, 91mol%, 92mol%, 93mol%, 94mol%, 95mol%, 96mol%, 97mol%, 98mol%, or about 99mol%, and its upper limit can be 100mol%, or about 99.9mol%. The ratio can be greater than or equal to, or greater than any one of the above lower limits, or can be less than or equal to, or less than any one of the above upper limits, or can be less than or equal to, or less than any one of the above upper limits and greater than or equal to, or greater than any one of the above lower limits. At such a ratio, appropriate curability can be ensured, and a release layer having desired release characteristics can be formed.

[0057] In the polyorganosiloxane of the present application, the ratio between the siloxane units of Formulae 1 to 3 may also be adjusted.

[0058] For example, the lower limit of the ratio of the number of moles of the siloxane unit of Formula 1 to the number of moles of the siloxane unit of Formula 2 contained in the polyorganosiloxane may be about 0.5, 1, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, or 90, and the upper limit thereof may be about 2,000, 1,500, 1,000, 500, 400, 300, 200, 100, 90, 80, 70, 60, 50, 40, 30, or 20. The ratio may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. At such a ratio, appropriate curability can be ensured, and a release layer having desired release characteristics can be formed.

[0059] The lower limit of the ratio of the number of moles of the siloxane units of Formula 1 to the number of moles of the siloxane units of Formula 3 contained in the polyorganosiloxane of the present application may be about 0.5, 1, 5, 10, 12, 14, 16, 18, 20, 25, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, or 130, and the upper limit thereof may be about 2,000, 1000, 500, 300, 200, 150, 140, 130, 120, 110, 100, 90, 80, 70, 60, 50, 40, 30, or 20. The ratio may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. At such a ratio, appropriate curability can be ensured, and a release layer having desired release characteristics can be formed.If the polyorganosiloxane includes the siloxane units of Formulae 1 to 3 above, it may have additional other siloxane units.

[0060] For example, the polyorganosiloxane of the present application may further include one or more siloxane units selected from the group consisting of the siloxane units of the following Formula 4 and the siloxane units of the following Formula 5.

[0061] [Formula 4]

[0062] (R 1 3SiO 1 / 2 )

[0063] [Formula 5]

[0064] (R 2 R 1 2SiO 1 / 2 )

[0065] In equations 4 and 5, R 1 can be an alkyl group, and R 2 It may be an alkenyl group.

[0066] Specific types of the alkyl and alkenyl groups of Formula 4 and Formula 5 are as described at the beginning of this specification.

[0067] The siloxane units of Formula 4 and Formula 5 are each a so-called M unit, and such a unit may be bonded to the terminal and / or side chain of the polymer chain of the polyorganosiloxane to thereby exist. In one example, the polyorganosiloxane may include only one of the siloxane units of Formula 4 and Formula 5 above, or may include both of the foregoing.

[0068] For example, such a polyorganosiloxane of the present application may have an average unit of the following Formula 6.

[0069] [Formula 6]

[0070] R 1 a R 2 b R 3 c R 4 d SiO (4-a-b-c-d) / 2

[0071] In formula 6, R 1 It can be an alkyl group, R 2 It can be an alkenyl group, R 3 It can be an aryl group, and R 4 It may be an alkoxy group, a hydroxyl group or a monovalent hydrocarbon group, but is not limited thereto.

[0072] Specific types of the alkyl group, alkenyl group, aryl group, alkoxy group and monovalent hydrocarbon group of Formula 6 are as described at the beginning of this specification.

[0073] In this specification, the term average unit of polyorganosiloxane means a formula expressed by converting the number of moles of functional groups and linking groups (linking groups linking silicon atoms to silicon atoms) contained in polyorganosiloxane based on the fact that the number of moles of silicon atoms contained in polyorganosiloxane is assumed to be 1 mole. Such an average unit may be for a single molecule of polyorganosiloxane, or may be for a mixture of bimolecular or higher polyorganosiloxanes. When the average unit is for a mixture of bimolecular or higher polyorganosiloxanes, the ratio of other functional groups or linking groups is calculated by assuming that the number of all silicon atoms contained in the mixture is 1 mole.

[0074] In Formula 6, R represented on the left side of the silicon atom (Si) 1 , R 2 , R 3 and R 4 represents a functional group directly connected to a silicon atom, and an oxygen atom (O) on the right side represents a linking group connecting silicon atoms to silicon atoms.

[0075] In Formula 6, a is a functional group R converted by assuming that the number of moles of silicon atoms contained in the compound is 1 mole. 1 In Formula 6, b is a functional group R converted by assuming that the molar number of silicon atoms contained in the compound is 1 mole 2 In Formula 6, c is a functional group R converted by assuming that the molar number of silicon atoms contained in the compound is 1 mole 3 In Formula 6, d is a functional group R converted by assuming that the molar number of silicon atoms contained in the compound is 1 mole. 4 The number of moles.

[0076] In addition, (4-abcd) in Formula 6 is the number of moles of oxygen atoms (O) as a linking group, which is converted by assuming that the number of moles of silicon atoms contained in the compound is 1 mole. In the case of a linking group oxygen atom (O), two silicon atoms are bonded thereto, so that the number of moles is expressed by dividing by 2.

[0077] In Formula 6, the lower limit of a may be about 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, or 1.9, and the upper limit thereof may be about 6, 5.5, 5, 4.5, 4, 3.5, 3, 2.5, or 2. a may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0078] In Formula 6, the lower limit of b may be about 0.001, 0.005, 0.01, 0.02, 0.04, or 0.05, and the upper limit thereof may be about 0.7, 0.6, 0.5, 0.4, 0.2, 0.1, 0.05, 0.03, or 0.02. b may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0079] In Formula 6, the lower limit of c may be about 0.001, 0.01, 0.03, 0.05, 0.07, or 0.09, and the upper limit thereof may be about 2, 1.8, 1.6, 1.4, 1.2, 1, 0.8, 0.5, 0.2, 0.1, or 0.05. c may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0080] In Formula 6, the upper limit of d may be about 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1, 0.05, 0.01, or 0.001, and the lower limit thereof may be 0. d may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0081] By using the polyorganosiloxane having the above average unit, a release composition that forms a release layer having desired characteristics after curing while having appropriate curability can be provided.

[0082] The polyorganosiloxane may have a substantially linear structure. For example, the polyorganosiloxane may consist essentially of only M units and D units, or may further contain T units and / or Q units in addition to M units and D units, but may have a structure in which the ratio of T units and / or Q units is below a specific level.

[0083] For example, the upper limit of the ratio of the total number of moles of trifunctional siloxane units (T units) and tetrafunctional siloxane units (Q units) to the total number of moles of siloxane units contained in the polyorganosiloxane (100×(the number of moles of T units+the number of moles of Q units) / the number of moles of all siloxane units) may be about 10 mol%, 9 mol%, 8 mol%, 7 mol%, 6 mol%, 4 mol%, 3 mol%, 2 mol%, 1 mol%, 0.5 mol%, or 0.1 mol%, and the lower limit thereof may be 0 mol%. The ratio may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. At such a ratio, appropriate curability can be ensured, and a release layer having desired release characteristics can be formed.

[0084] The polyorganosiloxane may have a certain level of weight average molecular weight. For example, the lower limit of the weight average molecular weight may be about 20,000 g / mol, 50,000 g / mol, 100,000 g / mol, 150,000 g / mol, 200,000 g / mol, 250,000 g / mol, 300,000 g / mol, 350,000 g / mol, 400,000 g / mol, 450,000 g / mol, 500,000 g / mol, or 550,000 g / mol, and the upper limit thereof may be about 2,000,000 g / mol, 1,500,000 g / mol, 1,000,000 g / mol, 900,000 g / mol, 800,000 g / mol, 700,000 g / mol, or 650,000 g / mol. The weight average molecular weight may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0085] The polyorganosiloxane of the present application may have a certain level of polydispersity index. The polydispersity index is a value (Mw / Mn) obtained by dividing the weight average molecular weight (Mw) of the compound by the number average molecular weight (Mn).

[0086] The lower limit of the polydispersity index (PDI) may be about 1, 1.25, 1.5, 1.75, or 1.8, and the upper limit thereof may be about 5, 3.5, 3, 2.5, 2.2, or 2. The polydispersity index may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. When the polydispersity index of the polyorganosiloxane component is within the above range, excellent release properties and smooth film-forming properties may be ensured.

[0087] The lower limit of the content of the polyorganosiloxane component in the release composition can be about 0.5 wt%, 1 wt%, 3 wt%, 5 wt%, 7 wt%, 8 wt%, 10 wt%, 20 wt%, 30 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%, or 75 wt%, and the upper limit can be about 95 wt%, 90 wt%, 85 wt%, 80 wt%, 75 wt%, 70 wt%, 65 wt%, 60 wt%, 55 wt%, 50 wt%, 45 wt%, 40 wt%, 35 wt%, 30 wt%, 25 wt%, 20 wt%, 15 wt%, or 10 wt%. The ratio can be greater than or equal to, or greater than any of the above lower limits, or can be less than or equal to, or less than any of the above upper limits, or can be less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. The ratio is a ratio based on solid content, and therefore, when the release composition contains a solvent, the ratio is a ratio relative to the total weight of the release composition excluding the weight of the solvent. By containing the polyorganosiloxane within the above range, a release composition having excellent curability and forming a release layer having desired physical properties can be provided.

[0088] Such polyorganosiloxane can be produced by a known method. Generally, polyorganosiloxane can be produced by polymerizing an alkoxysilane compound or a partial condensate thereof, or by ring-opening polymerization of a cyclic siloxane compound, and such known methods can be equally applied to the present application.

[0089] If the release composition of the present application contains polyorganosiloxane, it may further contain other components.

[0090] For example, the release composition may include a curable silicone resin component in addition to the polyorganosiloxane.

[0091] The term curable silicone resin component may be a silicone resin component that can be cured. The term curing means a phenomenon in which the viscosity of the release composition increases or the release composition hardens by a chemical or physical reaction or interaction as known.

[0092] Such a curable silicone resin component may include a compound having a functional group capable of curing. However, the scope of the curable silicone resin component or curable compound mentioned in this specification does not include polyorganosiloxane having a siloxane unit of Formulae 1 to 3 above.

[0093] For example, the curable silicone resin component can be an addition-cured silicone resin component to be described below, wherein such an addition-cured silicone resin component can include a polyorganosiloxane having an alkenyl group such as a vinyl group. However, since the polyorganosiloxane having the siloxane unit of the above formula 1 to formula 3 also has an alkenyl group, the polyorganosiloxane can also be strictly classified as a curable silicone resin component, but for ease of explanation, the components or compounds mentioned as curable silicone resin components in this specification do not include polyorganosiloxane having the siloxane unit of the above formula 1 to formula 3. However, such an interpretation method does not mean that the polyorganosiloxane having the siloxane unit of the above formula 1 to formula 3 does not have curability.

[0094] In the present specification, the polyorganosiloxane having the siloxane units of Formulae 1 to 3 above may be referred to as an additive polyorganosiloxane to distinguish it from the polyorganosiloxane contained in the curable silicone resin component.

[0095] Meanwhile, the curable silicone resin component may be composed of one polyorganosiloxane, or may be composed of a mixture of two or more polyorganosiloxanes.

[0096] In one example, the silicone resin component of the release composition may be a so-called addition curing component. Such a resin component may include, for example, a polyorganosiloxane containing a siloxane unit having an alkenyl group bonded to a silicon atom (hereinafter, may be referred to as a first polyorganosiloxane or a first polyorganosiloxane component).

[0097] The first polyorganosiloxane or the first polyorganosiloxane component may have, for example, an average unit of the following Formula 7. Here, the average unit has the same meaning as described above.

[0098] [Formula 7]

[0099] P 2 c Q 2d SiO (4-c-d) / 2

[0100] In formula 7, P 2 may be alkenyl, and Q 2 It may be an alkoxy group, a hydroxy group or a monovalent hydrocarbon group.

[0101] In Formula 7, c and d are arbitrary numbers.

[0102] In Formula 7, specific types of the alkenyl group, alkoxy group and monovalent hydrocarbon group are as described at the beginning of this specification.

[0103] In one example, the lower limit of c can be about 0.0001, 0.0005, 0.001, 0.002, 0.005, or 0.01, and the upper limit can be about 0.1, 0.09, 0.08, 0.07, 0.06, 0.05, 0.04, 0.03, 0.02, 0.01, 0.009, 0.008, 0.007, 0.006, 0.005, 0.004, or 0.003. c can be greater than or equal to, or greater than any of the above lower limits, or can be less than or equal to, or less than any of the above upper limits, or can be less than or equal to, or less than any of the above upper limits while being greater than or equal to, or greater than any of the above lower limits.

[0104] In one example, the lower limit of d may be about 0.5, 1, 1.5, 1.7, or 1.9, and the upper limit thereof may be about 5, 4, 3.5, 3, 2.5, or 2. d may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0105] The first polyorganosiloxane may include alkenyl groups bonded to silicon atoms, and the ratio of the alkenyl groups may be adjusted based on the number of moles of organic groups bonded to all silicon atoms included in the polyorganosiloxane. For example, the lower limit of the ratio of the molar number of silicon-bonded alkenyl groups based on the molar number of organic groups bonded to all silicon atoms contained in the first polyorganosiloxane may be about 0.01 mol%, 0.05 mol%, 0.1 mol%, 0.15 mol%, 0.2 mol%, 0.25 mol%, 0.3 mol%, 0.35 mol%, 0.4 mol%, 0.45 mol% or 0.5 mol%, 0.6 mol%, 0.7 mol%, 0.8 mol%, 0.9 mol%, or 1 mol%, and the upper limit thereof may be about 1.5 mol%, 1.4 mol%, 1.3 mol%, 1.2 mol%, 1.1 mol%, 0.9 mol%, 0.8 mol%, 0.7 mol%, or 0.6 mol%, 0.5 mol%, 0.4 mol%, 0.3 mol%, 0.2 mol%, or 0.1 mol%. The ratio may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. At such a ratio, appropriate curability can be ensured, and a release layer having desired release characteristics can be formed.

[0106] Such an alkenyl group may be included in a siloxane unit of a specific structure in the polyorganosiloxane. For example, the first polyorganosiloxane may include one or more siloxane units selected from the siloxane unit of the following Formula 9 and the siloxane unit of the following Formula 10.

[0107] [Formula 9]

[0108] ViR 3 2SiO 1 / 2

[0109] [Formula 10]

[0110] ViR 3 SiO 2 / 2

[0111] In Formula 9 and Formula 10, Vi may be an alkenyl group, and R 3 It can be a hydroxyl group, an alkoxy group or a monovalent hydrocarbon group. The specific types of the above alkenyl group, alkoxy group and monovalent hydrocarbon group are as described in Formula 7.

[0112] Based on all siloxane units in the first polyorganosiloxane component, the lower limit of the ratio of the siloxane units of the above formula 9 may be about 0.001 mol%, 0.005 mol%, 0.01 mol%, 0.02 mol%, 0.03 mol%, 0.04 mol%, 0.05 mol%, 0.06 mol%, 0.07 mol%, 0.08 mol%, 0.09 mol%, or 0.095 mol%, and the upper limit thereof may be about 0.5 mol%, 0.4 mol%, 0.3 mol%, 0.2 mol%, 0.1 mol%, 0.09 mol%, 0.08 mol%, or 0.07 mol%. The ratio may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be less than or equal to, or less than any of the above upper limits while being greater than or equal to, or greater than any of the above lower limits.

[0113] The lower limit of the ratio of the siloxane units of the above formula 10 based on all the siloxane units in the first polyorganosiloxane component may be about 0.01 mol%, 0.05 mol%, 0.1 mol%, 0.15 mol%, 0.2 mol%, 0.3 mol%, 0.4 mol%, 0.5 mol%, 0.6 mol%, 0.7 mol%, 0.8 mol%, or 0.9 mol%, and the upper limit thereof may be about 10 mol%, 9 mol%, 8 mol%, 7 mol%, 6 mol%, 5 mol%, 4 mol%, 3 mol%, 2 mol%, or 1 mol%. The ratio may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0114] The first polyorganosiloxane component may include both the siloxane units of the above formula 9 and the siloxane units of the above formula 10. In this case, the molar ratio of the siloxane units of the above formula 10 to the siloxane units of the above formula 9 may have a lower limit of about 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 4, 5, 6, 7, 8, 9, or 9.5, and an upper limit thereof may be about 20, 18, 16, 14, 12, 11, 10, 9, 8, 7, 6, 5, 4, or 3. It may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits while being greater than or equal to, or greater than any of the above lower limits.

[0115] The lower limit of the number of silicon atoms contained in the first polyorganosiloxane component may be about 500, 1,500, 2,000, 2,500, or 3,000, and the upper limit thereof may be about 10,000, 5,000, 4,000, 3,500, 3,000, 2,500, or 2,100. The number of silicon atoms may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits while being greater than or equal to, or greater than any of the above lower limits.

[0116] The first polyorganosiloxane component may have a substantially linear structure. In this case, the polyorganosiloxane may be substantially composed of only M units (monofunctional siloxane units) and D units (difunctional siloxane units), or may further contain T units (trifunctional siloxane units) and / or Q units (tetrafunctional siloxane units) in addition to M units (monofunctional siloxane units) and D units (difunctional siloxane units), but may have a structure in which the ratio of T units (trifunctional siloxane units) and / or Q units (tetrafunctional siloxane units) is below a certain level.

[0117] For example, in the first polyorganosiloxane component, the upper limit of the ratio of the total number of moles of T units and Q units to the number of moles of all siloxane units contained in the polyorganosiloxane (100×(number of moles of T units+number of moles of Q units) / number of moles of all siloxane units) may be about 10 mol%, 9 mol%, 8 mol%, 7 mol%, 6 mol%, 5 mol%, 4 mol%, 3 mol%, 2 mol%, 1 mol%, or 0.5 mol%, and the lower limit thereof may be 0 mol%. The ratio may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0118] The weight average molecular weight of the first polyorganosiloxane component may have a lower limit of about 100,000 g / mol, 150,000 g / mol, 200,000 g / mol, 250,000 g / mol, or 300,000 g / mol, and an upper limit thereof may be about 1,000,000 g / mol, 950,000 g / mol, 900,000 g / mol, 850,000 g / mol, 800,000 g / mol, 750,000 g / mol, 700,000 g / mol, 650,000 g / mol, 600,000 g / mol, 550,000 g / mol, 500,000 g / mol, 450,000 g / mol, or 400,000 g / mol. The weight average molecular weight may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. Since the first polyorganosiloxane has a weight average molecular weight within the above range, an appropriate viscosity can be ensured to exhibit excellent coating properties.

[0119] The lower limit of the polydispersity index (PDI) of the first polyorganosiloxane component may be about 1, 1.25, or 1.5, and the upper limit thereof may be about 5, 3.5, or 2.5. The polydispersity index may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits while being greater than or equal to, or greater than any of the above lower limits.

[0120] In addition to the first polyorganosiloxane described above, the curable silicone resin component may also include a polyorganosiloxane having an average unit of the following formula 8 (hereinafter, may be referred to as a second polyorganosiloxane or a second polyorganosiloxane component). The meaning of the average unit is as described above. The average unit may be for a single molecule polyorganosiloxane, or may be for a mixture of bimolecular or higher polyorganosiloxanes.

[0121] [Formula 8]

[0122] H e Q 3 f SiO (4-e-f) / 2

[0123] In formula 8, Q 3 It may be an alkoxy group, a hydroxy group or a monovalent hydrocarbon group.

[0124] In Formula 8, e and f are arbitrary numbers.

[0125] Specific examples of the alkoxy group or the monovalent hydrocarbon group of Formula 8 above are the same as those of Formula 7.

[0126] In Formula 8, the lower limit of e may be about 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, or 0.6, and the upper limit thereof may be about 2, 1.5, 1, 0.9, 0.8, 0.7, 0.65, 0.6, 0.5, 0.4, 0.39, 0.38, 0.37, 0.36, or 0.35. e may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0127] In Formula 8, the lower limit of f may be about 0.5, 1, 1.1, 1.2, 1.3, 1.4, 1.5, or 1.6, and the upper limit thereof may be about 4, 3.5, 3, 2.5, 2, 1.9, 1.8, 1.7, 1.6, or 1.5. f may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0128] The second polyorganosiloxane may contain hydrogen atoms bonded to silicon atoms, and the ratio of hydrogen atoms may be adjusted based on the molar number of organic groups bonded to all silicon atoms contained in the polyorganosiloxane. For example, based on the molar number of organic groups bonded to all silicon atoms contained in the second polyorganosiloxane, the lower limit of the ratio of the molar number of hydrogen atoms bonded to silicon atoms may be about 1 mol%, 5 mol%, 10 mol%, 15 mol%, 20 mol%, 25 mol%, or 30 mol%, and the upper limit thereof may be about 85 mol%, 80 mol%, 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, or 20 mol%. The ratio may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. At such a ratio, appropriate curability can be ensured, and a release layer having desired release characteristics can be formed.

[0129] Such hydrogen atoms may be contained in a siloxane unit of a specific structure in the polyorganosiloxane.

[0130] For example, hydrogen atoms bonded to silicon atoms may be present in at least the siloxane unit of the following formula 11:

[0131] [Formula 11]

[0132] HR 4 SiO 2 / 2

[0133] In formula 11, R 4 The specific types of the alkoxy group and the monovalent hydrocarbon group of Formula 11 are the same as those of Formula 8.

[0134] The lower limit of the ratio of the molar number of the siloxane units of Formula 11 based on the total molar number of the siloxane units containing hydrogen atoms bonded to silicon atoms in all the siloxane units contained in the second polyorganosiloxane component may be about 85 mol%, 90 mol%, 95 mol%, 96 mol%, 97 mol%, 98 mol%, 99 mol%, or 99.5 mol%, and the upper limit thereof may be about 100 mol%. The ratio may be greater than or equal to, or greater than any of the above lower limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0135] The lower limit of the ratio of the siloxane units of the above formula 11 based on all the siloxane units in the second polyorganosiloxane component may be about 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, 35 mol%, 40 mol%, 45 mol%, 50 mol%, 55 mol%, or 60 mol%, and the upper limit thereof may be about 85 mol%, 80 mol%, 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, or 50 mol%. The ratio may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be less than or equal to, or less than any of the above upper limits while being greater than or equal to, or greater than any of the above lower limits.

[0136] The lower limit of the number of silicon atoms contained in the second polyorganosiloxane component may be about 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, or 90, and the upper limit thereof may be about 1,000, 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, or 50. The number of silicon atoms may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits while being greater than or equal to, or greater than any of the above lower limits.

[0137] The second polyorganosiloxane component may have a substantially linear structure. In this case, the polyorganosiloxane may be substantially composed of only M units and D units, or may further contain T units and / or Q units in addition to M units and D units, but may have a structure in which the ratio of T units and / or Q units is lower than a certain level.

[0138] For example, in the second polyorganosiloxane component, the upper limit of the ratio of the total number of moles of T units and Q units to the number of moles of all siloxane units contained in the polyorganosiloxane (100×(number of moles of T units+number of moles of Q units) / number of moles of all siloxane units) may be about 10 mol%, 9 mol%, 8 mol%, 7 mol%, 6 mol%, 5 mol%, 4 mol%, 3 mol%, 2 mol%, 1 mol%, or 0.5 mol%, and the lower limit thereof may be 0 mol%. The ratio may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0139] The weight average molecular weight of the second polyorganosiloxane may have a lower limit of about 1,000 g / mol, 2,000 g / mol, 3,000 g / mol, 4,000 g / mol, 5,000 g / mol, 6,000 g / mol, 7,000 g / mol, 8,000 g / mol, or 9,000 g / mol, and an upper limit thereof may be about 100,000 g / mol, 90,000 g / mol, 80,000 g / mol, 70,000 g / mol, 60,000 g / mol, 50,000 g / mol, 45,000 g / mol, 40,000 g / mol, 30,000 g / mol, 20,000 g / mol, 15,000 g / mol, or 12,000 g / mol. The weight average molecular weight may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. Since the second polyorganosiloxane has a weight average molecular weight within the above range, excellent curing characteristics can be ensured.

[0140] The lower limit of the polydispersity index of the second polyorganosiloxane may be about 1, 1.25, or 1.5, and the upper limit thereof may be about 5, 3.5, or 2.5. The polydispersity index may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits while being greater than or equal to, or greater than any of the above lower limits.

[0141] The lower limit of the first polyorganosiloxane component in the curable silicone resin component or the release composition can be about 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, or 90 wt%, and the upper limit thereof can be about 98 wt%, 96 wt%, 94 wt%, 92 wt%, 90 wt%, 85 wt%, 80 wt%, 75 wt%, 70 wt%, 65 wt%, 60 wt%, 55 wt%, 50 wt%, 45 wt%, 40 wt%, 35 wt%, or 30 wt%. The ratio may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. The ratio is a ratio based on solid content, and therefore, when the release composition contains a solvent, the ratio is a ratio relative to the total weight of the release composition excluding the weight of the solvent. By containing the first polyorganosiloxane within the above range, an appropriate level of release peeling force and an excellent residual adhesion rate of the release layer to be described below can be ensured.

[0142] The lower limit of the weight of the second polyorganosiloxane in the curable silicone resin component or the release composition relative to 100 parts by weight of the first polyorganosiloxane may be 0.1 parts by weight, 0.25 parts by weight, 0.5 parts by weight, 0.75 parts by weight, 1 part by weight, 1.25 parts by weight, 1.5 parts by weight, 1.75 parts by weight, or about 2 parts by weight, and the upper limit thereof may be 10 parts by weight, 8 parts by weight, 6 parts by weight, 4 parts by weight, or about 3.5 parts by weight, 3 parts by weight, or about 2.5 parts by weight. The ratio may be greater than or equal to, or greater than any one of the above lower limits, or may be less than or equal to, or less than any one of the above upper limits, or may be less than or equal to, or less than any one of the above upper limits while being greater than or equal to, or greater than any one of the above lower limits. When the second polyorganosiloxane is included in the above range, the crosslinking density may be improved to ensure a cured product having excellent durability.

[0143] In the release composition of the present application, the lower limit of the weight of the additive polyorganosiloxane relative to 100 parts by weight of the curable silicone resin component can be 1 part by weight, 5 parts by weight, 10 parts by weight, 50 parts by weight, 100 parts by weight, 200 parts by weight, 300 parts by weight, or 350 parts by weight, and the upper limit can be 1000 parts by weight, 900 parts by weight, 800 parts by weight, 700 parts by weight, 600 parts by weight, 500 parts by weight, 400 parts by weight, 300 parts by weight, and 200 parts by weight, 100 parts by weight, 50 parts by weight, 40 parts by weight, 30 parts by weight, 20 parts by weight, or 10 parts by weight. The ratio can be greater than or equal to, or greater than any of the above lower limits, or can be less than or equal to, or less than any of the above upper limits, or can be less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. By controlling the ratio of the additive polyorganosiloxane, a desired release layer can be formed more effectively.

[0144] In view of curability, if necessary, the release composition of the present application may also include a catalyst. As a catalyst, a suitable known catalyst may be used considering the curing type of the curable silicone resin component. For example, when the curable silicone resin component is an addition-cured type, a metal catalyst may be used as a catalyst. The metal catalyst may include one or more selected from aluminum, bismuth, lead, mercury, tin, zinc, platinum, silver and zirconium as a central metal element. As a metal catalyst, for example, bis[1,3-bis(2-vinyl)-1,1,3,3-tetramethyldisiloxane] platinum (CAS No.81032-58-8), dibutyltin dilaurate or dimethyltin diacetate, etc. may be used, but are not particularly limited thereto. For example, as a catalyst, a catalyst known in industry as a so-called addition-cured catalyst may be used.

[0145] If the catalyst is included in a catalytic amount, the content of the catalyst is not particularly limited. For example, relative to 100 parts by weight of the curable silicone resin component, the lower limit of the weight of the catalyst can be about 0.1 parts by weight, 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, or about 3 parts by weight, and its upper limit can be about 10 parts by weight, 9 parts by weight, 8 parts by weight, 7 parts by weight, 6 parts by weight, 5 parts by weight, 4 parts by weight, or about 3 parts by weight. It can be greater than or equal to or greater than any one of the above-mentioned lower limits, or can be less than or equal to or less than any one of the above-mentioned upper limits, or can be less than or equal to or less than any one of the above-mentioned upper limits and greater than or equal to or greater than any one of the above-mentioned lower limits in the range. By including a catalyst in the above-mentioned range, while reducing side reactions, it is possible to effectively promote the formation reaction of cured products.

[0146] The release composition according to one example of the present application may further include an organic solvent. Considering the composition of the release composition, the solvent may be suitably an organic solvent. The organic solvent is not particularly limited as long as it is commonly used in industry, and tetrahydrofuran, methyl ethyl ketone, toluene and heptane, etc., or a mixed solvent of the foregoing may be used. In addition, their mixing ratio is not particularly limited, and they may be appropriately formulated as needed.

[0147] The amount of the solvent can be adjusted as needed, and is not particularly limited.

[0148] The present application also relates to a release layer. The release layer may include the above release composition or a cured product thereof.

[0149] Therefore, the release layer may contain an additive polyorganosiloxane, may further contain a curable silicone resin component, and may optionally contain a reactant of the component. The release layer may be formed, for example, by curing a release composition according to an example of the present application as described above. The method for performing the curing is not particularly limited, and a suitable curing method may be adopted according to the type of the curable resin component.

[0150] By including the release composition or a cured product thereof, the release layer can effectively satisfy the physical properties desired in the present application.

[0151] That is, regardless of the temperature, the release layer can stably maintain the desired release characteristics even after being maintained for a long time. In addition, the release layer can stably maintain the balance between the so-called high-speed peeling force and the low-speed peeling force. In addition, the release layer can stably maintain the release characteristics even when the pressure-sensitive adhesive or the like is attached and peeled off multiple times. The release composition can have excellent curing characteristics and can therefore be stably cured to form the above-mentioned release layer.

[0152] For example, the release layer may satisfy physical properties according to one or more of the following formulas 1 to 5. That is, the release layer may satisfy physical properties according to any one of the following formulas 1 to 5, may satisfy two or more of the physical properties thereof at the same time, or may satisfy all of the physical properties according to the following formulas 1 to 5.

[0153] For example, the peeling force aging change rate (A) of the release layer according to the following formula 1: R1 ) can be within a predetermined range. For example, the peel force aging change rate (A R1 ) can be about 18%, 17%, 16%, 15%, 14%, 13%, 12%, 11%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.9%, 0.8%, 0.7%, or 0.6%, and its lower limit can be about 0%. The peel force aging change rate (A R1) may be less than or equal to, or less than any of the above upper limits, or may be less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. When the peel force aging change rate satisfies the above range, the present application can provide a release layer having an appropriate level of release peel force and residual adhesion rate.

[0154] [Formula 1]

[0155] A R1 =100×|A7-A1| / A1

[0156] In Formula 1, A1 may be the release force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 25° C. for 24 hours and then the pressure-sensitive adhesive layer is peeled off from the release layer at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min at 25° C., and A7 may be the release force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 25° C. for 168 hours and then the pressure-sensitive adhesive layer is peeled off from the release layer at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min at 25° C.

[0157] In Formula 1, |A7-A1| means the absolute value of the difference between A7 and A1.

[0158] The peel force aging change rate (A R1 ) (including the measurement method of release peel force A7 and A1) is described in the Examples section.

[0159] Since A in the above formula 1 R1 The above range is satisfied, and thus the release layer of the present application can exhibit an appropriate level of release peeling force even after a long period of time.

[0160] The upper limit of the release peeling force A7 in Formula 1 may be about 500 gf / inch, 400 gf / inch, 300 gf / inch, 200 gf / inch, 100 gf / inch, 50 gf / inch, 30 gf / inch, 20 gf / inch, 15 gf / inch, or 10 gf / inch, and the lower limit thereof may be about 1 gf / inch, or 5 gf / inch. The release peeling force A7 may be less than or equal to, or less than any of the above upper limits, or may be less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. Since the release layer of the present application has a release peeling force A7 that satisfies the above range, it can exhibit desired release characteristics in various applications.

[0161] The peeling force aging change rate (A) of the release layer of the present application according to the following formula 2 R2) can be within a predetermined range. For example, the peel force aging change rate (A R2 ) may be 0%, or about 1%, and its upper limit may be about 20%, 19%, 18%, 17%, 16%, 15%, 14%, 13%, 12%, 11%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, or about 0.5%. The peel force aging change rate may be less than or equal to, or less than any of the above upper limits, or may be less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. In the present application, the peel force aging change rate satisfies the above range, so that even when the release layer is kept at high temperature for a long time, the desired release characteristics can be stably maintained.

[0162] [Formula 2]

[0163] A R2 =100×|A 60℃,7 -A 60℃,1 | / A 60℃,1

[0164] In formula 2, A 60℃,1 The peeling force may be the peeling force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 60° C. for 24 hours and then peeled from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min, and A 60℃,7 The release force may be measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 60° C. for 168 hours and then peeled from the release layer at 25° C. at a peel angle of 180 degrees and a peel rate of 0.3 m / min.

[0165] In Formula 2, |A 60℃,7 -A 60℃,1 | Meaning A 60℃,7 With A 60℃,1 The absolute value of the difference.

[0166] According to the above formula 2, the peel force aging change rate (A R2 ) (including the release peeling force A 60℃,7 and A 60℃,1 The measurement method of ) is described in the Examples section of this specification.

[0167] The release force A in the above formula 2 60℃,1The upper limit of the release force may be about 500 gf / inch, 400 gf / inch, 300 gf / inch, 200 gf / inch, 100 gf / inch, 50 gf / inch, 30 gf / inch, 20 gf / inch, or 10 gf / inch, and the lower limit thereof may be about 1 gf / inch, or 5 gf / inch. The release peel force may be less than or equal to, or less than any of the above upper limits, or may be less than or equal to, or less than any of the above upper limits while being greater than or equal to, or greater than any of the above lower limits. Since the present application has a release peel force (A) satisfying the above range, 60℃,1 ), and thus a release layer having an appropriate level of release peel force and residual adhesion rate even at high temperatures can be provided.

[0168] The release force A in the above formula 2 60℃,7 The upper limit may be about 500 gf / inch, 400 gf / inch, 300 gf / inch, 200 gf / inch, 100 gf / inch, 50 gf / inch, 30 gf / inch, 20 gf / inch, or about 10 gf / inch, and the lower limit may be about 1 gf / inch, or about 5 gf / inch. The release peel force may be less than or equal to, or less than any one of the above upper limits, or may be less than or equal to, or less than any one of the above upper limits while being greater than or equal to, or greater than any one of the above lower limits. By satisfying the above ranges, the present application can provide a release layer having an appropriate level of release peel force and residual adhesion rate over time even at high temperatures.

[0169] The peeling force aging change rate (A) of the release layer of the present application at room temperature (about 25°C)-60°C according to the following formula 3 R3 ) may have an upper limit of about 30%, 29%, 28%, 27%, 26%, 25%, 20%, 15%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, or about 1%, and a lower limit thereof may be about 0%, or about 0.1%. The peel force aging change rate at room temperature (about 25°C)-60°C may be less than or equal to, or less than any of the above upper limits, or may be within a range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits. By satisfying the above range, the present application can stably maintain the desired release properties even when the release layer is maintained in an environment with temperature changes for a long time.

[0170] [Formula 3]

[0171] A R3 =100×|A 60℃,7 -A1| / A1

[0172] In Formula 3, A1 may be the release peeling force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 25° C. for 24 hours and then the pressure-sensitive adhesive layer is peeled off from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min, and A 60℃,7 The release force may be measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 60° C. for 168 hours and then peeled from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min.

[0173] In Formula 3, |A 60℃,7 -A1|means A 60℃,7 The absolute value of the difference from A1.

[0174] According to the above formula 3, the peeling force aging change rate (A R3 ) specific measurement method (release peeling force A 60℃,7 and A1) are described in the Examples section of this specification.

[0175] The peeling force ratio (A) of the release layer of the present application that depends on the peeling rate according to the following formula 4: R4 ) may be within a predetermined range. For example, depending on the peeling force ratio (A R4 ) may have a lower limit of about 50%, 100%, 150%, 155%, 160%, 165%, 170%, 175%, 180%, or 185%, and an upper limit thereof may be about 600%, 590%, 580%, 570%, 560%, 550%, 540%, 530%, or 520%, 500%, 450%, 400%, 350%, 300%, 250%, 200%, or 190%. The peeling force ratio depending on the peeling rate may be less than or equal to, or less than any of the above upper limits, or may be less than or equal to, or less than any of the above upper limits while being greater than or equal to, or greater than any of the above lower limits. By satisfying the above ranges, the present application can provide a release layer that exhibits a relatively high peeling force when peeled at a relatively low speed and a relatively low peeling force when peeled at a relatively high speed. Even under high temperature conditions, the release layer can stably exhibit a balance of peeling force that depends on the peeling rate.

[0176] [Formula 4]

[0177] A R4 =100×A H / A L

[0178] In formula 4, A HThe peeling force may be the peeling force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 60° C. for 24 hours and then peeled from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 30 m / min, and A L The release force may be measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 60° C. for 24 hours and then peeled from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min.

[0179] The peeling force ratio (A) depending on the peeling rate according to the above formula 4 is R4 ) specific measurement method (release peeling force A H and A L The measurement method of ) is described in the Examples section of this specification.

[0180] The residual adhesion rate (A) of the release layer of the present application according to the following formula 5 d ) may be within a predetermined range. For example, the residual adhesion rate (A d The lower limit of the residual adhesion rate may be about 80%, 82.5%, 85%, 87.5%, or 90%, and the upper limit thereof may be about 100%, or 99%. The residual adhesion rate may be greater than or equal to, or greater than any of the above lower limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0181] When the release layer according to one embodiment of the present application has a residual adhesion rate (A d ), even after the pressure-sensitive adhesive layer is attached to the release layer several times and then peeled off, the release property can be stably maintained.

[0182] [Formula 5]

[0183] Residual adhesion rate (A d )=100×A f / A i

[0184] In Formula 5, A i The peeling force may be the peeling force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 25° C. for 24 hours and then peeled from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min, and A f It can be measured for A i The release force was measured when the pressure-sensitive adhesive layer was kept attached to the release layer at 25° C. for 24 hours and then peeled from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min.

[0185] The residual adhesion rate (A d ) specific measurement method (measurement of release peeling force A f and A i The method of ) is described in the Examples section.

[0186] In the release layer of the present application, the release peeling force A of the above formula 5 is i The upper limit may be about 500 gf / inch, 400 gf / inch, 300 gf / inch, 200 gf / inch, 100 gf / inch, 50 gf / inch, or 25 gf / inch, and the lower limit may be about 1 gf / inch, or 5 gf / inch. The release peel force may be greater than or equal to, or greater than any one of the above lower limits, or may be less than or equal to, or less than any one of the above upper limits, or may be less than or equal to, or less than any one of the above upper limits and greater than or equal to, or greater than any one of the above lower limits. When a release layer according to an example of the present application has a release peel force that satisfies the above range, it can be said that it has an appropriate level of release peel force and residual adhesion rate.

[0187] In the release layer of the present application, the release peeling force A of the above formula 5 is f The lower limit may be about 1 gf / inch, or 5 gf / inch, and the upper limit may be about 500 gf / inch, 400 gf / inch, 300 gf / inch, 200 gf / inch, 100 gf / inch, 50 gf / inch, or 25 gf / inch. The release peel force may be greater than or equal to, or greater than any of the above lower limits, or may be less than or equal to, or less than any of the above upper limits, or may be within the range of less than or equal to, or less than any of the above upper limits and greater than or equal to, or greater than any of the above lower limits.

[0188] By having a release peeling force (A f ) while satisfying the residual adhesion rate (A) according to the above formula 5 d ), the present application can provide a release layer with an appropriate level of release peeling force and residual adhesion rate.

[0189] The present application also relates to a release film.

[0190] The release film may include a base film and a release layer formed on one side or both sides of the base film.

[0191] The specific details of the release layer are as described above.

[0192] The type of the base film of the release film according to one example of the present application is not particularly limited. As the base film, a base film that can be generally used to form a release film can be applied.

[0193] For example, as the base film, PET (poly(ethylene terephthalate)) film, PTFE (poly(tetrafluoroethylene)) film, PP (polypropylene) film, PE (polyethylene) film, polyimide film, polyamide film, COP (cyclic olefin polymer) film, polybutylene film, polybutadiene film, vinyl chloride copolymer film, polyurethane film, ethylene-vinyl acetate film, ethylene-propylene copolymer film, ethylene-ethyl acrylate copolymer film, ethylene-methyl acrylate copolymer film and / or polyimide film etc. can be used, but are not limited thereto.

[0194] In addition, the base film can be composed of a single layer, or can also be laminated by two or more layers, and in some cases, it can also include a functional layer, such as an antifouling layer or an antistatic layer. In addition, from the perspective of improving the adhesion of the base material, one or both sides of the base material can also be further surface treated, such as primer treatment.

[0195] The thickness of the base film is appropriately selected depending on the purpose, is not particularly limited, and it may be typically formed to a thickness of 5 μm to 500 μm, 5 μm to 250 μm, or 5 μm to 100 μm.

[0196] The release film of the present application can be manufactured in a known manner. In one example, the release film of the present application can be manufactured by applying a release composition according to an example of the present application to one side or both sides of the base material, and then curing it to form a release layer. Here, the application method of the release composition is not particularly limited, as long as it is commonly used in industry, including, for example, blade coating, roller coating or reverse coating, etc. In addition, the formation of the release layer can be carried out after fully removing the components causing bubbles, such as volatile components or reaction residues of the release composition. In addition, the method for curing the release composition is not particularly limited, and it can be cured by a suitable aging process, or in a suitable high temperature environment or light irradiation environment, as described above.

[0197] The thickness of the release layer included in the release film is not particularly limited, and may be, for example, 10 nm to 10 μm, 10 nm to 1 μm, or 10 nm to 100 nm.

[0198] Furthermore, the present application relates to a pressure-sensitive adhesive film.

[0199] The pressure-sensitive adhesive film according to one example of the present application may include the above release layer and a pressure-sensitive adhesive layer to which the release layer is attached. By including the release layer, the pressure-sensitive adhesive layer may be protected until it is used.

[0200] The release layer of the pressure-sensitive adhesive film according to one example of the present application is as described above.

[0201] The pressure-sensitive adhesive forming the pressure-sensitive adhesive layer of the pressure-sensitive adhesive film according to one example of the present application is not particularly limited.

[0202] For example, as the pressure-sensitive adhesive forming the pressure-sensitive adhesive layer, a pressure-sensitive adhesive using acrylic polymer, silicone-based polymer, polyester, polyurethane, polyamide, polyether, or fluorine-based or rubber-based polymer or the like as a base polymer can be appropriately selected and used.

[0203] Beneficial Effects

[0204] The present application provides a release composition, a release layer, a release film and a pressure-sensitive adhesive film.

[0205] The release composition of the present application has excellent curability and can thus be stably cured to form a release layer.

[0206] When a release layer has been formed, the present application can provide a release composition that allows a stable residual adhesion rate to be exhibited even if the release layer is repeatedly applied to a pressure-sensitive adhesive layer or the like.

[0207] The release layer of the present application can maintain the desired release characteristics even if it is kept at room temperature and high temperature for a long time. In addition, the release layer can stably maintain the balance between the high-speed peeling force and the low-speed peeling force. DETAILED DESCRIPTION

[0208] Hereinafter, the present application will be described in more detail through Examples and Comparative Examples, but the scope of the present application is not limited to the contents presented below.

[0209] 1. Release force measurement method

[0210] The sample is prepared by laminating the pressure-sensitive adhesive layer of a standard tape (TESA, TESA7475) having a pressure-sensitive adhesive layer on the surface of the release layer of the release film prepared with each release composition of the embodiment or comparative example. The pressure-sensitive adhesive layer of the standard tape is placed on the release layer and then attached by reciprocating the roller three times under a load of 2.5 kg. Subsequently, the sample is kept at room temperature (about 25°C) for 24 hours to measure the release peeling force, or kept at 60°C for 24 hours to measure the release peeling force. The release peeling force is measured using a physical property measuring device (Cheminstruments, AR-1000) when the standard tape is peeled off at a peeling angle of 180 degrees and a peeling rate of 0.3m / min (slow peeling force), or when the standard tape is peeled off at a peeling angle of 180 degrees and a peeling rate of 30m / min (high-speed peeling force). The peeling force is measured at room temperature (about 25°C).

[0211] 2. Change rate of peel strength at room temperature (A R1 )

[0212] For the release layer of the release film prepared with each release composition of the embodiment or comparative example, the aging change rate of the peeling force at room temperature (A R1 ) is measured according to the following formula 1.

[0213] [Formula 1]

[0214] A R1 =100×|A7-A1| / A1

[0215] In Formula 1, A1 is the release peel force measured after a specimen prepared by laminating a standard tape (TESA, TESA7475) to a release layer of a release film in the same manner as described in the release peel force measurement method is kept at room temperature (about 25° C.) for about 24 hours. The release peel force is measured when the standard tape is peeled off at a peel angle of 180 degrees and a peel rate of 0.3 m / min at room temperature (about 25° C.) using a physical property measuring device (Cheminstruments, AR-1000). A7 of Formula 1 is the release peel force measured after the specimen is kept at room temperature (about 25° C.) for 168 hours, and the release peel force is also measured when the standard tape is peeled off at a peel angle of 180 degrees and a peel rate of 0.3 m / min at room temperature (about 25° C.) using a physical property measuring device (Cheminstruments, AR-1000).

[0216] 3.60℃ peel strength aging change rate (A R2 )

[0217] For the release layer of the release film prepared with each release composition of the embodiment or comparative example, the aging change rate of the peeling force at 60°C (A R2 ) is measured according to the following formula 2.

[0218] [Formula 2]

[0219] A R2 =100×|A 60℃,7 -A 60℃,1 | / A 60℃,1

[0220] In formula 2, A 60℃,1 is the release peel force measured after a test specimen prepared by laminating a standard adhesive tape (TESA, TESA7475) to the release layer of a release film in the same manner as described in the release peel force measurement method is kept at 60° C. for 24 hours, and A of Formula 2 60℃,7 It is the release peel force measured after a test specimen prepared by laminating a standard adhesive tape (TESA, TESA7475) to the release layer of a release film in the same manner as described in the release peel force measurement method is kept at 60° C. for 168 hours. The release peel force is measured when the standard adhesive tape is peeled off at a peel angle of 180 degrees and a peel rate of 0.3 m / min at room temperature (about 25° C.) using a physical property measuring device (Cheminstruments, AR-1000).

[0221] 4. Peel force aging change rate at room temperature -60℃ (A R3 )

[0222] For the release layer of the release film prepared with each release composition of the embodiment or comparative example, the peeling force aging change rate (A R3 ) is measured according to the following formula 3.

[0223] [Formula 3]

[0224] A R3 =100×|A 60℃,7 -A1| / A1

[0225] In Formula 3, A1 is the release peel force measured after a specimen prepared by laminating a standard adhesive tape (TESA, TESA7475) to the release layer of a release film in the same manner as described in the release peel force measurement method is kept at room temperature (about 25° C.) for about 24 hours, and A 60℃,7The release peel force is measured after the sample is kept at 60° C. for 168 hours. The release peel force is measured when a standard tape is peeled off at a peel angle of 180 degrees and a peel rate of 0.3 m / min at room temperature (about 25° C.) using a physical property measuring device (Cheminstruments, AR-1000).

[0226] 5. Peel force ratio depending on peel rate (A R4 )

[0227] For the release layer of the release film prepared with each release composition of the embodiment or comparative example, the peeling force ratio (A R4 ) is measured according to the following formula 4.

[0228] [Formula 4]

[0229] A R4 =100×A H / A L

[0230] In formula 4, A H The release peel force is measured after a specimen prepared by laminating a standard adhesive tape (TESA, TESA7475) to a release layer of a release film in the same manner as described in the release peel force measurement method is kept at 60°C for 24 hours. The release peel force is measured when the standard adhesive tape is peeled off at a peeling angle of 180 degrees and a peeling rate of 30 m / min at room temperature (about 25°C) using a physical property measuring device (Cheminstruments, AR-1000). In addition, A of Formula 4 L The release peel force is measured after keeping the sample at 60° C. for 24 hours, which is the release peel force measured when the tape is peeled off at a peel angle of 180 degrees and a peel rate of 0.3 m / min at room temperature (about 25° C.) using a physical property measuring device (Cheminstruments, AR-1000).

[0231] 6. Residual Adhesion Rate (A d ) Measurement method

[0232] For the release layer of the release film prepared with each release composition prepared in the examples or comparative examples, the residual adhesion rate (A d ) is measured according to the following formula 5.

[0233] [Formula 5]

[0234] A d =100×A f / A i

[0235] In Formula 5, Ai The release peel force is the release peel force measured after a specimen prepared by laminating a standard adhesive tape (TESA, TESA7475) to a release layer of a release film in the same manner as described in the release peel force measurement method is kept at room temperature (about 25° C.) for about 24 hours, and is the release peel force measured when the standard adhesive tape is peeled off at a peel angle of 180 degrees and a peel rate of 0.3 m / min at room temperature (about 25° C.) using a physical property measuring device (Cheminstruments, AR-1000). In addition, A of Formula 5 f In order to measure the release force by laminating a standard adhesive tape (TESA, TESA7475) to the test strip in the same manner as described in the release force measurement method. i The release peel force of a sample prepared by using the same release layer of the subsequent release film is measured after being kept at room temperature (about 25°C) for about 24 hours, which is the release peel force measured when a standard tape is peeled off at room temperature (about 25°C) at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min using a physical property measuring device (Cheminstruments, AR-1000).

[0236] 7. Method for evaluating the curability of release compositions

[0237] For the release layer of the release film produced using the release composition of the example or comparative example, the curability of the release composition was evaluated using a rub-off evaluation method, which is an evaluation method for observing changes after rubbing the surface of the release layer three times with a constant load while wearing latex gloves.

[0238] Curability was evaluated based on the following criteria.

[0239] <Curability Evaluation Criteria>

[0240] PASS: When there is no change in the release layer after the abrasion evaluation

[0241] NG: When the release layer peeled off or the base film became blurred after the rubbing evaluation.

[0242] 8. Evaluation of weight average molecular weight

[0243] The weight average molecular weight (Mw) and the polydispersity index (PDI) were measured using GPC (gel permeation chromatography).The unit of the weight average molecular weight (Mw) and the number average molecular weight (Mn) mentioned in this specification is g / mol.

[0244] Place the sample (sample to be analyzed) in a 20 mL vial, dilute it to a concentration of approximately 20 mg / mL with THF (tetrahydrofuran), and filter the calibration standard sample and the sample to be analyzed through a syringe filter (pore size: 0.2 μm), then measure the molecular weight characteristics. As the analysis procedure, use ChemStation from Agilent technologies, compare the elution time of the sample with the calibration curve to obtain the number average molecular weight (Mn) and the weight average molecular weight (Mw), and then use the value (Mw / Mn) obtained by dividing the weight average molecular weight (Mw) by the number average molecular weight (Mn) as the polydispersity index.

[0245] <GPC Measurement Conditions>

[0246] Instrument: 1200 series from Agilent technologies

[0247] Column: Use TL Mix.A&B from Agilent technologies

[0248] Solvent: THF

[0249] Column temperature: 40 °C

[0250] Sample concentration: 20 mg / mL, 10 μl injection

[0251] Use MP: 364000, 91450, 17970, 4910, 1300 as the standard sample

[0252] Preparation Example 1.

[0253] Prepare the polyorganosiloxane of the following formula A.

[0254] [Formula A]

[0255]

[0256] In formula A, x is a number around approximately 1,000, y is a number around approximately 60, and z is a number around approximately 60.

[0257] As the monomers for forming the polyorganosiloxane, octamethylcyclotetrasiloxane (M), 1,3,5,7 - tetramethyl - 1,3,5,7 - tetravinylcyclotetrasiloxane (V), and octaphenylcyclotetrasiloxane (P) are mixed at a weight ratio of 170:10:10 (M:V:P) (primary mixture). Further add P4 - tert - butyl - phosphazene (C) and chlorodimethylvinylsilane (S) to the mixture (secondary mixture). The addition is carried out at a weight ratio of approximately 6250:2.5:1 (primary mixture:C:S).

[0258] The secondary mixture was polymerized at a temperature of about 60° C. for 12 hours to prepare a polyorganosiloxane component of the above formula A. The polyorganosiloxane component had a weight average molecular weight of about 600,000 g / mol and a polydispersity index of about 1.85.

[0259] Preparation Example 2.

[0260] The polyorganosiloxane of the following formula B was prepared.

[0261] [Formula B]

[0262]

[0263] In Formula B, x is a number of about 1,000 or so, y is a number of about 60 or so, and z is a number of about 7 to 8 or so.

[0264] The preparation of the polyorganosiloxane component of the above formula B is carried out in the same manner as the polyorganosiloxane component of the formula A, but when preparing the polyorganosiloxane component of the formula B, the weight ratio of octamethylcyclotetrasiloxane (M), 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane (V) and octaphenylcyclotetrasiloxane (P) is set to 130:9:1 (M:V:P) when preparing the primary mixture. The weight average molecular weight of the polyorganosiloxane component is about 600,000 g / mol, and the polydispersity index is about 1.85.

[0265] Preparation Example 3.

[0266] The polyorganosiloxane of the following formula C was prepared.

[0267] [Formula C]

[0268]

[0269] In Formula C, x is a number of about 1,000, y is a number of about 11, and z is a number of about 70.

[0270] The polyorganosiloxane component of the above formula C was prepared in the same manner as in Preparation Example 1. However, when preparing the polyorganosiloxane component of formula C, the weight ratio of octamethylcyclotetrasiloxane (M), 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane (V) and octaphenylcyclotetrasiloxane (P) in the primary mixture was adjusted to about 145:1:10 (M:V:P). The weight average molecular weight of the polyorganosiloxane component of formula C was about 600,000 g / mol, and the polydispersity index was about 1.85.

[0271] Example 1.

[0272] The polyorganosiloxane of the following formula E (KS-847H, Shinetsu Silicone) (weight average molecular weight of about 350,000 g / mol), the polyorganosiloxane of the following formula F (X-92-122, Shinetsu Silicone) (weight average molecular weight of about 10,000 g / mol), the platinum catalyst (PL-50L, Shinetsu Silicone) (C) and the polyorganosiloxane component (A) of Preparation Example 1 were mixed at a weight ratio of 5:0.1:0.15:0.5 (E:F:C:A) and dispersed in a solvent to prepare a release composition. As the solvent (S), a solvent obtained by mixing THF (tetrahydrofuran), MEK (methyl ethyl ketone), toluene (T) and n-heptane (H) at a weight ratio of 50:30:10:10 (THF:MEK:T:H) was used.

[0273] [Formula E]

[0274]

[0275] In Formula E, m is a number of about 1,500 or so, and n is a number of about 12 to 13 or so.

[0276] [Formula F]

[0277]

[0278] In Formula F, a is a number of approximately 34 to 36, and b is a number of approximately 34 to 36.

[0279] Example 2.

[0280] The polyorganosiloxane of the above formula E (KS-847H, Shinetsu Silicone) (weight average molecular weight of about 350,000 g / mol), the polyorganosiloxane of the above formula F (X-92-122, Shinetsu Silicone) (weight average molecular weight of about 10,000 g / mol), the platinum catalyst (PL-50L, Shinetsu Silicone) (C) and the polyorganosiloxane component (A) of the above Preparation Example 1 were mixed at a weight ratio of 5:0.1:0.15:2.5 (E:F:C:A) and dispersed in a solvent to prepare a release composition. As the solvent (S), the same solvent as in Example 1 was used.

[0281] Example 3.

[0282] The polyorganosiloxane of the above formula E (KS-847H, Shinetsu Silicone) (weight average molecular weight of about 350,000 g / mol), the polyorganosiloxane of the above formula F (X-92-122, Shinetsu Silicone) (weight average molecular weight of about 10,000 g / mol), the platinum catalyst (PL-50L, Shinetsu Silicone) (C) and the polyorganosiloxane component (A) of the above Preparation Example 1 were mixed at a weight ratio of 5:0.1:0.15:12.5 (E:F:C:A) and dispersed in a solvent to prepare a release composition. As the solvent (S), the same solvent as in Example 1 was used.

[0283] Example 4.

[0284] Instead of the polyorganosiloxane component of Preparation Example 1, the polyorganosiloxane component (B) of Preparation Example 2 was used. The polyorganosiloxane of the above formula E (KS-847H, Shinetsu Silicone) (weight average molecular weight of about 350,000 g / mol), the polyorganosiloxane of the above formula F (X-92-122, Shinetsu Silicone) (weight average molecular weight of about 10,000 g / mol), the platinum catalyst (PL-50L, Shinetsu Silicone) (C) and the polyorganosiloxane component (B) of the above Preparation Example 2 were mixed in a weight ratio of 5:0.1:0.15:0.5 (E:F:C:B) and dispersed in a solvent to prepare a release composition. As the solvent (S), the same solvent as in Example 1 was used.

[0285] Example 5.

[0286] The polyorganosiloxane of the above formula E (KS-847H, Shinetsu Silicone) (weight average molecular weight of about 350,000 g / mol), the polyorganosiloxane of the above formula F (X-92-122, Shinetsu Silicone) (weight average molecular weight of about 10,000 g / mol), the platinum catalyst (PL-50L, Shinetsu Silicone) (C) and the polyorganosiloxane component (B) of the above Preparation Example 2 were mixed at a weight ratio of 5:0.1:0.15:2.5 (E:F:C:B) and dispersed in a solvent to prepare a release composition. As the solvent (S), the same solvent as in Example 1 was used.

[0287] Example 6.

[0288] The polyorganosiloxane of the above formula E (KS-847H, Shinetsu Silicone) (weight average molecular weight of about 350,000 g / mol), the polyorganosiloxane of the above formula F (X-92-122, Shinetsu Silicone) (weight average molecular weight of about 10,000 g / mol), the platinum catalyst (PL-50L, Shinetsu Silicone) (C) and the polyorganosiloxane component (B) of the above Preparation Example 2 were mixed at a weight ratio of 5:0.1:0.15:10 (E:F:C:B) and dispersed in a solvent to prepare a release composition. As the solvent (S), the same solvent as in Example 1 was used.

[0289] Example 7.

[0290] The polyorganosiloxane of the above formula E (KS-847H, Shinetsu Silicone) (weight average molecular weight of about 350,000 g / mol), the polyorganosiloxane of the above formula F (X-92-122, Shinetsu Silicone) (weight average molecular weight of about 10,000 g / mol), the platinum catalyst (PL-50L, Shinetsu Silicone) (C) and the polyorganosiloxane component (B) of the above Preparation Example 2 were mixed at a weight ratio of 5:0.1:0.15:12.5 (E:F:C:B) and dispersed in a solvent to prepare a release composition. As the solvent (S), the same solvent as in Example 1 was used.

[0291] Example 8.

[0292] The polyorganosiloxane of the above formula E (KS-847H, Shinetsu Silicone) (weight average molecular weight of about 350,000 g / mol), the polyorganosiloxane of the above formula F (X-92-122, Shinetsu Silicone) (weight average molecular weight of about 10,000 g / mol), the platinum catalyst (PL-50L, Shinetsu Silicone) (C) and the polyorganosiloxane component (B) of the above Preparation Example 2 were mixed at a weight ratio of 5:0.1:0.15:20 (E:F:C:B) and dispersed in a solvent to prepare a release composition. As the solvent (S), the same solvent as in Example 1 was used.

[0293] Example 9.

[0294] Instead of the polyorganosiloxane component of Preparation Example 1, the polyorganosiloxane component (D) of Preparation Example 3 was used. The polyorganosiloxane of the above formula E (KS-847H, Shinetsu Silicone) (weight average molecular weight of about 350,000 g / mol), the polyorganosiloxane of the above formula F (X-92-122, Shinetsu Silicone) (weight average molecular weight of about 10,000 g / mol), the platinum catalyst (PL-50L, Shinetsu Silicone) (C) and the polyorganosiloxane component (D) of the above Preparation Example 3 were mixed in a weight ratio of 5:0.1:0.15:2.5 (E:F:C:D) and dispersed in a solvent to prepare a release composition. As the solvent (S), the same solvent as in Example 1 was used.

[0295] Example 10.

[0296] The polyorganosiloxane of the above formula E (KS-847H, Shinetsu Silicone) (weight average molecular weight of about 350,000 g / mol), the polyorganosiloxane of the above formula F (X-92-122, Shinetsu Silicone) (weight average molecular weight of about 10,000 g / mol), the platinum catalyst (PL-50L, Shinetsu Silicone) (C) and the polyorganosiloxane component (D) of the above Preparation Example 3 were mixed at a weight ratio of 5:0.1:0.15:12.5 (E:F:C:D) and dispersed in a solvent to prepare a release composition. As the solvent (S), the same solvent as in Example 1 was used.

[0297] Comparative Example 1.

[0298] The polyorganosiloxane of the above formula E (KS-847H, Shinetsu Silicone) (weight average molecular weight of about 350,000 g / mol), the polyorganosiloxane of the above formula F (X-92-122, Shinetsu Silicone) (weight average molecular weight of about 10,000 g / mol) and the platinum catalyst (PL-50L, Shinetsu Silicone) (C) were mixed at a weight ratio of 5:0.1:0.15 (E:F:C) and dispersed in a solvent to prepare a release composition. As the solvent (S), the same solvent as in Example 1 was used.

[0299] A release film was prepared using each release composition of the above examples or comparative examples. The release film was prepared by applying the release composition of the examples or comparative examples to one side of a base film using a Meyer bar, and then curing the applied release composition by keeping it at 150° C. for 3 minutes to form a release layer.

[0300] The thickness of the release layer is about 200 nm to 300 nm, and a PET (polyethylene terephthalate) film having a thickness of about 50 μm is used as the base film.

[0301] The results of the test data measured in the Examples and Comparative Examples are summarized in the following Tables 1 and 2. The unit of the release peel force in the following Tables 1 and 2 is gf / inch.

[0302] [Table 1]

[0303]

[0304] [Table 2]

[0305]

[0306] In Table 1, A1, A7 and A R1 As defined in Formula 1, A 60℃,1 , A 60℃,7 and A R2 As defined in Equation 2, and A R3 As defined in Equation 3. In Table 2, A H , A L and A R4 as defined in Equation 4, and the residual adhesion rate as defined in Equation 5.

Claims

1. A release composition comprising a polyorganosiloxane having a siloxane unit of the following formula 1, a siloxane unit of the following formula 2, and a siloxane unit of the following formula 3: [Formula 1] (R 1 2SiO 2 / 2 ) [Formula 2] (R 1 R 2 SiO 2 / 2 ) [Formula 3] (R 3 2SiO 2 / 2 ) in, R 1 is an alkyl group, R 2 is alkenyl, and R 3 It is an aromatic group. 2 . The release composition according to claim 1 , wherein a ratio of the total mole number of the siloxane units of Formulae 1 to 3 relative to the total mole number of all siloxane units of the polyorganosiloxane is 85 mol % or more. 3 . The release composition according to claim 1 , wherein a ratio of the number of moles of the siloxane unit of Formula 1 to the number of moles of the siloxane unit of Formula 2 is in the range of 0.5 to 2,000. 4 . The release composition according to claim 1 , wherein a ratio of the number of moles of the siloxane unit of Formula 1 to the number of moles of the siloxane unit of Formula 3 is in the range of 0.5 to 2,000.

5. The release composition according to claim 1, wherein the polyorganosiloxane further comprises one or more siloxane units selected from the group consisting of the siloxane units of the following formula 4 and the siloxane units of the following formula 5: [Formula 4] (R 1 3SiO 1 / 2 ) [Formula 5] (R 2 R 1 2SiO 1 / 2 ) in, R 1 is an alkyl group and R 2 It is an alkenyl group.

6. The release composition according to claim 1, wherein the polyorganosiloxane has an average unit of the following formula 6: [Formula 6] R 1 a R 2 b R 3 c R 4 d SiO (4-a-b-c-d) / 2 in, R 1 is an alkyl group, R 2 is alkenyl, R 3 is an aryl group, R 4 is an alkoxy group, a hydroxyl group or a monovalent hydrocarbon group, a is a number in the range of 0.6 to 2, b is a number in the range of 0.001 to 0.7, c is a number in the range of 0.001 to 1.4, and d is a number in the range of 0 to 0.

5. 7 . The release composition according to claim 1 , wherein a ratio of the total mole number of trifunctional siloxane units and tetrafunctional siloxane units based on the mole number of all siloxane units included in the polyorganosiloxane is 10 mol % or less. 8 . The release composition according to claim 1 , wherein the weight average molecular weight of the polyorganosiloxane is in the range of 20,000 g / mol to 2,000,000 g / mol. 9 . The release composition according to claim 8 , wherein the polydispersity index of the polyorganosiloxane is in the range of 1 to 5. 10 . The release composition according to claim 1 , further comprising a curable silicone resin component. 11 . The release composition according to claim 10 , wherein the polyorganosiloxane is included in a ratio of 1 part by weight to 500 parts by weight relative to 100 parts by weight of the curable silicone resin component.

12. The release composition according to claim 10, wherein the curable silicone resin component comprises a polyorganosiloxane having an average unit of the following formula 7 and a polyorganosiloxane having an average unit of the following formula 8: [Formula 7] P 2 c Q 2 d SiO (4-c-d) / 2 in, P 2 is alkenyl, Q 2 is an alkoxy group, a hydroxyl group or a monovalent hydrocarbon group, c is a number in the range of 0.0001 to 0.1, and d is a number in the range of 1 to 4: [Formula 8] H e Q 3 f SiO (4-e-f) / 2 Among them, Q 3 is an alkoxy group, a hydroxyl group or a monovalent hydrocarbon group, e is a number in the range of 0.01 to 0.9, and f is a number in the range of 1 to 4.

13. The release composition according to claim 12, wherein the polyorganosiloxane of Formula 7 comprises one or more siloxane units selected from the group consisting of the siloxane units of the following Formula 9 and the siloxane units of the following Formula 10: [Formula 9] For 3 2SiO 1 / 2 [Formula 10] ViR 3 SiO 2 / 2 in, Vi is alkenyl, and R 3 It is a hydroxyl group, an alkoxy group or a monovalent hydrocarbon group.

14. The release composition according to claim 12, wherein the polyorganosiloxane of Formula 8 comprises a siloxane unit of the following Formula 11: [Formula 11] HR 4 SiO 2 / 2 in, R 4 It is a hydroxyl group, an alkoxy group or a monovalent hydrocarbon group.

15. The release composition according to claim 12, wherein the weight average molecular weight of the polyorganosiloxane having the average unit of Formula 7 is in the range of 100,000 g / mol to 1,000,000 g / mol, and the weight average molecular weight of the polyorganosiloxane having the average unit of Formula 8 is in the range of 1,000 g / mol to 50,000 g / mol. 16 . A release layer comprising the release composition according to claim 1 or a cured product thereof.

17. The release layer according to claim 16, satisfying at least one or more of the following formulas 1 to 5: [Formula 1] 18≥A R1 =100×(|A7-A1|) / A1 in, A1 is a release peel force measured when the pressure-sensitive adhesive layer is kept attached to the release layer for 24 hours at 25° C. and then the pressure-sensitive adhesive layer is peeled off from the release layer at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min at 25° C., and A7 is a release peel force measured when the pressure-sensitive adhesive layer is kept attached to the release layer for 168 hours at 25° C. and then the pressure-sensitive adhesive layer is peeled off from the release layer at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min at 25° C.; [Formula 2] 20≥A R2 =100×|A 60℃,7 -A 60℃,1 | / A 60℃,1 Among them, A 60℃,1 A is the release peeling force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 60° C. for 24 hours and then peeled from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min, and A 60℃,7 The release peel force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 60° C. for 168 hours and then the pressure-sensitive adhesive layer is peeled off from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min; [Formula 3] 30≥A R3 =100×|A 60℃,7 -A1| / A1 wherein A1 is the release peeling force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 25° C. for 24 hours and then the pressure-sensitive adhesive layer is peeled off from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min, and A 60℃,7 The release peel force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 60° C. for 168 hours and then the pressure-sensitive adhesive layer is peeled off from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min; [Formula 4] 150≤A R4 =100×A H / A L Among them, A H A is the release peeling force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 60° C. for 24 hours and then peeled from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 30 m / min, and A L The release peel force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 60° C. for 24 hours and then the pressure-sensitive adhesive layer is peeled off from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min; [Formula 5] 80≤A d =100×A f / A i Among them, A i A is the release peeling force measured when the pressure-sensitive adhesive layer is kept attached to the release layer at 25° C. for 24 hours and then the pressure-sensitive adhesive layer is peeled off from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min, and A f For measuring A i Thereafter, the state of the pressure-sensitive adhesive layer attached to the release layer is maintained again at 25° C. for 24 hours and then the release force is measured when the pressure-sensitive adhesive layer is peeled from the release layer at 25° C. at a peeling angle of 180 degrees and a peeling rate of 0.3 m / min. 18 . A release film comprising a base film and the release layer according to claim 16 , wherein the release layer is on one side or both sides of the base film. 19 . A pressure-sensitive adhesive film comprising the release layer according to claim 16 ; and a pressure-sensitive adhesive layer attached to the release layer.

Citation Information

Patent Citations

  • Silicone emulsion composition

    CN112912443A

  • Silicone emulsion releasing composition and releasing substrate using the same

    EP2112191A1