Metal doped activated carbon
By combining activated carbon with electrical stabilizers and wettability enhancers and performing purge gas treatment to remove oxygen functional groups and form conductive metal-doped activated carbon, the problem of insufficient electrical properties of activated carbon in supercapacitors and lithium-sulfur batteries is solved. , achieving an energy storage system with high capacitance value and long life.
Patent Information
- Application Number
- CN202380023542.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-08-17
- Filing Date
- 2023-08-15
- Publication Date
- 2024-10-22
AI Technical Summary
Existing activated carbon has insufficient electrical properties in supercapacitors and lithium-sulfur batteries due to oxygen-containing functional groups, resulting in shortened electrode life and increased resistance, making it difficult to achieve high energy density and long-life energy storage systems.
By combining activated carbon with electrical stabilizers and wettability enhancers, and subjecting it to purge gas treatment at elevated temperatures, the oxygen functional groups in the activated carbon are removed to form conductive metal oxides or metal-doped activated carbon, improving its conductivity. and physical properties.
Significantly improves the conductivity and adsorption capacity of activated carbon, enhances the capacitance value of supercapacitors and the cycle stability of lithium-sulfur batteries, reduces resistance, and extends the service life of electrodes.
Smart Images

Figure CN118830101A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of U.S. Provisional Patent Application No. 63 / 398,816, filed on August 17, 2022, entitled “Metal-Doped Activated Carbon,” the entire contents of which are incorporated herein by reference for all purposes. Technical Field
[0003] Some embodiments relate to methods for preparing activated carbon having relatively high conductivity. Some embodiments relate to methods for preparing activated carbon having relatively low oxygen content. Some embodiments relate to methods for preparing activated carbon having relatively high ionic conductivity doped therein with metals. Some embodiments relate to activated carbon prepared by the methods described herein or activated carbon having relatively low internal resistance doped therein with metals. Some embodiments relate to supercapacitors or batteries having electrodes prepared from such materials. Background Art
[0004] Electrochemical energy storage devices use physical and chemical properties for electric charge. For example, supercapacitors use physical storage mechanisms to produce high power with long life. Batteries use redox reactions to store and release energy.
[0005] Electrodes for energy storage systems require high adsorption capacity due to good microporosity and low electrical resistance in supercapacitor and battery applications, including lithium-sulfur (LiS) battery applications. Typical activated carbons have high adsorption capacity but usually do not have suitable electrical properties. Typical activated carbons have oxygen-related functional groups chemically bound to the surface, which can lead to a shortened life of supercapacitors and lithium-sulfur batteries.
[0006] In order to address the shortcomings of its electrical properties, carbon materials such as activated carbon can provide useful materials for manufacturing electrodes. For example, carbon-based materials can be designed as highly porous materials so as to have a high surface area. The pore size in the material can be microporous, mainly to provide a high surface area. Carbon materials can also provide good adsorption (i.e., ions adhere to the surface of the material) and low resistance (i.e., effective electron and ion movement under high current). Carbon pore size can be described as micropores (with a pore width less than 2nm), mesopores (with a pore width between 2nm and 50nm) and macropores (with a pore width greater than 50nm).
[0007] Activated carbon has a high surface area (1,000 m 2 / g to 3000m 2 / g) and is used as an electrode material. Activated carbon is widely produced from many natural materials such as coal (lignite, bituminous coal and anthracite), peat, wood and coconut shell. Among these natural raw materials, coconut shell becomes a good activated carbon because it has primary micropores less than 2nm required for supercapacitor carbon.
[0008] The production of activated carbon mainly involves carbonization and activation with an oxidant or activator. Carbonization converts natural substances into charcoal (carbon) under a reducing atmosphere. The charcoal is partially oxidized to produce activated carbon. Activation can form a porous surface of the activated carbon, but this partial oxidation process cannot remove the oxygen-containing functional groups. When activated carbon is used as an electrode material for supercapacitors, the oxygen-containing functional groups will produce parasitic reactions on the supercapacitor, thereby reducing the initial capacitance and limiting the life span. The oxygen-containing functional groups also produce high resistance for supercapacitor and battery applications such as lithium-sulfur applications.
[0009] Examples of potential applications of activated carbon materials with improved electrical properties include supercapacitors and batteries, including metal sulfur, such as lithium-sulfur (LiS) batteries. Supercapacitors, known as electrochemical double layer capacitors (EDLCs), are high-capacity capacitors that can bridge the gap between electrolytic capacitors and rechargeable batteries. Supercapacitors can potentially store more power per unit volume or mass than electrolytic capacitors (e.g., typically 10 to 100 times more power), and can accept and deliver charge much faster than batteries because charging / discharging only involves the physical movement of ions, not chemical reactions. Supercapacitors can also allow for many more charge and discharge cycles than batteries, and can be used for power bursts, such as recovering and supplying electricity in hybrid vehicles during regenerative braking, or can be used for energy storage as part of a building or building component. Carbon is an ideal material for supercapacitors because it has a high surface area and a favorable cost.
[0010] An area of growing interest in rechargeable battery technology is the lithium-sulfur (Li-S) battery. A lithium-sulfur battery has a lithium metal anode and a sulfur cathode. Sulfur and lithium have a charge and discharge capacity of 1672 mA hg -1 or 1675mA hg -1 Therefore, the theoretical energy density of Li-S battery is 2500Wh kg -1 , which is one of the highest theoretical energy densities in rechargeable batteries. Therefore, lithium-sulfur batteries offer a promising electrical energy storage system for portable electronics and electric vehicles.
[0011] Lithium-sulfur (LiS) batteries work by reducing sulfur to lithium sulfide at the cathode:
[0012]
[0013] The reaction of sulfur reduction to lithium sulfide is complex and involves the formation of various polysulfides (Li2S x , where 8 < x < 1, such as Li2S8, Li2S6, Li2S4, and Li2S2).
[0014] In some cases of lithium-sulfur batteries, the anode can be pure lithium metal (Li° is oxidized to Li + during discharge), and in some cases, the cathode can be activated carbon containing sulfur (S° is reduced to S 2- (sulfide)) during discharge. An ion-permeable separator is provided between the anode and the cathode, and the electrolyte used in such systems is usually based on a mixture of organic solvents, such as cyclic ethers, such as 1,2-dimethoxyethane (DME) and 1,3-dioxolane (DOXL), which contain 1 mole of lithium bis(trifluoromethanesulfonyl)imide (LiN(SO2CF3)2) and 1% lithium nitrate, etc.).
[0015] The potential advantages of lithium-sulfur batteries include high energy density (theoretically 5 times that of lithium-ion, but actually 2 - 3 times that of lithium-ion), no need for supplementary charging during storage (while lithium-ion batteries may require 40% regular recharge to prevent capacity loss), the active materials are lighter compared to lithium-ions, and the materials used to manufacture lithium-sulfur batteries are more environmentally friendly and cheaper than lithium-ion batteries (because rare earth metals are not required).
[0016] However, the challenges faced by lithium-sulfur battery systems have not been fully resolved to enable their commercialization. For example, polysulfides (Li2S x , where x is an integer between 3 and 8) dissolve in the electrolyte and are further reduced to insoluble lithium sulfide (such as Li2S2 to Li2S) formed on the anode in the battery system. Such formation results in the loss of active materials, leading to a short life cycle (i.e., fewer discharge and charge cycles), which is not commercially viable.
[0017] Moreover, since sulfur is electron and ion-insulating, sulfur needs to be embedded in a conductive matrix to be used in lithium-sulfur batteries. Carbon is a potentially useful material for lithium-sulfur battery electrodes because it has a porous structure that supports the deposition of polysulfides and can help minimize the swelling of the electrodes during discharge. The cathode of a lithium-sulfur battery can be made of sulfur-impregnated activated carbon, which acts as the active material and reacts with lithium ions from the lithium metal on the anode side. The electrodes require high adsorption capacity due to micropores and low resistance to produce a high capacitance of a supercapacitor and store insoluble polysulfides on the anode side and reduce the formation of insoluble polysulfides, which can cause a short lifespan of the LiS battery.
[0018] Many forms of activated carbon also include a high percentage of oxygen, such as in the range of about 15%, typically in the form of oxygen-containing functional groups. Oxygen is an insulating material, and its presence in activated carbon increases the electrical resistance of the carbon product.
[0019] The adoption of a green economy and renewable energy sources, such as wind and solar, requires the adoption of better energy storage systems. Electricity generation from renewable energy sources cannot be controlled predictably, and in order for such energy sources to supply a significant proportion of electricity to the grid, reliable and significant energy storage systems are required to balance the irregular generation provided by renewable energy sources. Providing a meaningful energy storage system would allow electricity to be stored during periods of power generation, and allow power to be supplied to the grid during periods of reduced generation from renewable energy sources. However, such energy storage systems would have to be very large to achieve the desired stability of the grid.
[0020] One strategy for providing energy storage systems that can facilitate widespread generation of renewable energy is to incorporate such energy storage systems into buildings or building components. This strategy can allow large amounts of energy to be stored without creating a large amount of separate occupied space for the energy storage system. However, energy storage systems used as part of buildings or building components need to be robust and reliable (e.g., have a long life span covering many charge and discharge cycles), because replacing or repairing such systems may be difficult or disrupt other uses of the building. In addition, such energy storage systems should provide high energy density in order to maximize energy storage while minimizing the amount of space occupied by such energy storage systems.
[0021] There remains a need for technologies that improve the capabilities of supercapacitors and / or metal-sulfur (including lithium-sulfur) battery systems. The foregoing examples of the related art and limitations associated therewith are intended to be illustrative and not exclusive. Other limitations of the related art will become apparent to those skilled in the art upon reading the specification and studying the drawings. Summary of the invention
[0022] The following embodiments and aspects thereof are described and illustrated in conjunction with systems, tools and methods, which are intended to be exemplary and illustrative, but not limiting in scope. In various embodiments, one or more of the above-mentioned problems have been reduced or eliminated, while other embodiments are directed to other improvements.
[0023] In some aspects, a composition comprising activated carbon, an electrical stabilizer and / or a wettability enhancer is provided. In some aspects, a method of producing conductive activated carbon is provided, the method comprising combining the activated carbon with the electrical stabilizer and / or the wettability enhancer to form an activated carbon mixture, and exposing the activated carbon mixture to a purge gas at an elevated temperature.
[0024] In some aspects, the electrical stabilizer is a conductive metal. In some aspects, the electrical stabilizer is a transition metal. In some aspects, the electrical stabilizer is Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pb, Ag, La, Hf, Ta, W, Re, Os, Ir, Pt, Au or Ac. In some aspects, the electrical stabilizer is Ni or Cu. In some aspects, the electrical stabilizer is copper. In some aspects, the wettability enhancer is aluminum. In some aspects, the wettability enhancer is alumina or activated alumina.
[0025] In some aspects, the electrical stabilizer is a metal and the metal is present in an amount of about 0.5 wt % to about 4.0 wt % based on the elemental content of the metal. In some aspects, the wettability enhancer is a metal and is present in an amount of about 0.15 wt % to about 1.5 wt % based on the elemental content of the metal.
[0026] In some aspects, an electrode containing an activated carbon composition or activated carbon prepared by the methods described herein is provided. In some aspects, a supercapacitor or battery comprising such an electrode is provided.
[0027] In one aspect, a lithium-sulfur battery containing such an electrode is provided, wherein the electrode comprises activated carbon containing an electrical stabilizer at a concentration in the range of about 0.5 wt % to about 3.5 wt %, and / or wherein the electrode comprises activated carbon containing a wettability enhancer at a concentration in the range of about 0.1 wt % to about 0.2 wt %.
[0028] In one aspect, a supercapacitor containing such an electrode is provided, wherein the electrode comprises activated carbon containing an electrical stabilizer at a concentration in the range of about 1 wt % to about 3.5 wt %, and / or wherein the electrode comprises activated carbon containing a wettability enhancer at a concentration in the range of about 0.45 wt % to about 1.0 wt %.
[0029] In some aspects, there is provided a building or modular building component comprising an energy storage system comprising an ultracapacitor or battery as described herein.
[0030] In addition to the exemplary aspects and embodiments described above, further aspects and embodiments will become apparent by reference to the drawings and study of the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Exemplary embodiments are illustrated with reference to the accompanying drawings. The embodiments and drawings disclosed herein are intended to be considered illustrative rather than restrictive.
[0032] Figure 1 An exemplary embodiment of a method of preparing doped activated carbon according to one embodiment is shown.
[0033] Figure 2 An example embodiment of a method of making an electrode for use in a supercapacitor is shown.
[0034] Figure 3 An example embodiment of a method of preparing an activated carbon cathode for a lithium-sulfur battery is shown.
[0035] Figure 4 An example embodiment of a method of assembling a cathode and a lithium metal anode for a lithium-sulfur battery is shown.
[0036] Figure 5 The 500 cycle performance of the LiS cell with the first baseline LAAC is shown.
[0037] Figure 6 The 500 cycle performance of the LiS cell with the second baseline LAAC is shown.
[0038] Figure 7 The first 50 cycles of the 500-cycle performance of the LiS cell with the first baseline LAAC are shown.
[0039] Figure 8 The first 50 cycles of the 500-cycle performance of the LiS cell with the second baseline LAAC are shown.
[0040] Fig. 9 The 500-cycle performance of LiS cells with the first metal-doped LAAC is shown.
[0041] Fig.10 The 500 cycle performance of LiS cells with a second metal-doped LAAC is shown.
[0042] Fig.11 The first 50 cycles of the 500-cycle performance of the LiS cell with the first metal-doped LAAC are shown.
[0043] Fig.12 The first 50 cycles of the 500-cycle performance of the LiS cell with the second metal-doped LAAC are shown. DETAILED DESCRIPTION
[0044] In the following description, specific details are set forth to provide a more thorough understanding to those skilled in the art. However, in order to avoid unnecessarily obscuring the present disclosure, well-known elements may not be shown or described in detail. Therefore, the specification and drawings are to be regarded as illustrative rather than restrictive.
[0045] In one exemplary embodiment, the inventors have developed new methods for producing carbons with desirable physical properties. Such carbons have potential utility, for example, in making electrodes for energy storage, such as for supercapacitors, metal-sulfur batteries, lithium-sulfur batteries, etc. The inventors have determined that doping activated carbon with metals that can act as wettability enhancers and electrical stabilizers can improve the conductivity and / or physical properties of the activated carbon, particularly after the activated carbon has been treated to reduce the number of functional groups present.
[0046] In a specific exemplary embodiment of the test, potassium hydroxide (KOH) was used as an exemplary oxidant, and lignin A (LA), lignin B (LB) and black liquor (BL, which contains lignin dissolved in an alkaline solution) were used to produce lignin-based activated carbon. The lignin-based activated carbon was treated using a purge gas (SG) process, which uses a reducing gas to remove oxygen-containing functional groups. YP50F (YPAC, derived from coconut shells) was selected as a comparative type of bio-based renewable source activated carbon.
[0047] It was observed that the metal-doped activated carbons tested in the examples showed significantly improved adsorption capacity and electrical properties, resulting in high capacitance values in the tested supercapacitor applications. The metal-doped activated carbons are suitable for electrode materials in supercapacitor and battery applications, such as metal-sulfur batteries, including lithium-sulfur batteries.
[0048] As used herein, a renewable activated carbon source refers to a carbon source that can naturally replenish itself (eg, derived from a bio-based source such as lignin or coconut), as opposed to non-renewable activated carbon sources (such as coal or oil byproducts).
[0049] As used herein, lignin refers to both lignin A, lignin B and black liquor. Lignin A and B are kraft lignins with low ash (<2% by mass) and high ash (<25% by mass), respectively. Pulp and paper biosolids (also referred to as "activated sludge") remaining after biogas digestion are another type of raw materials containing high levels of lignin. When preparing biogas, biodegradable biosolids are converted into biogas by digestion, leaving behind a non-degradable portion. The main component of the non-degradable portion is lignin. High lignin raw materials refer to materials containing a significant proportion of lignin (e.g., a lignin dry matter content between 65 wt. % and 98 wt. % or more, including any subranges therebetween, such as at least 65 wt. %, 70 wt. %, 75 wt. %, 80 wt. %, 85 wt. %, 90 wt. %, 95 wt. %, 96 wt. %, 97 wt. %, 98 wt. % or more than 98 wt. % lignin dry matter content), or black liquor obtained from a pulping process (which typically contains 10 wt. % to 15 wt. % lignin in its wet matter content, including any subranges therebetween), %, 31 wt%, 32 wt%, 33 wt%, 34 wt% or 35 wt% recoverable lignin in its dry matter content). In some embodiments, the high lignin feedstock has a recoverable lignin content between 65 wt % and 98 wt % or more on a dry weight basis, including any subranges therebetween, for example, at least 65 wt %, 70 wt %, 75 wt %, 80 wt %, 85 wt %, 90 wt %, 95 wt %, 96 wt %, 97 wt %, 98 wt %, or greater than 98 wt % recoverable lignin on a dry weight basis.
[0050] In one example embodiment, the activated carbon is ground and mixed with a dissolved salt of an electrical stabilizer and / or a dissolved salt of a wettability enhancer. The resulting preparation is dried, leaving the metal salt physically embedded in the activated carbon. The dried carbon is subjected to a purge gas treatment to remove oxygen from the material and convert the metal salt to its oxide form and / or elemental form, leaving the metal doped in the carbon. The electrical stabilizer can help improve the capacitance value by providing high capacitance at rapid discharge. The wettability enhancer can improve the interaction of the activated carbon with the solvent and the electrolyte.
[0051] More specifically and without being bound by theory, typical activated carbon contains a large number of oxygen-containing functional groups that have favorable interactions with polar solvents. Oxygen is chemically bound to the activated carbon and results in high resistance when used as an electrode material. Purge gas treatment using an oxygen-deficient gas or under reducing conditions as described herein can be used to reduce (and thereby remove) oxygen-based functional groups from the activated carbon, resulting in an increase in the carbon content of the activated carbon. Deoxygenated activated carbon becomes highly non-interactive with polar solvents, including polar solvents used as electrolytes in supercapacitors and lithium-sulfur batteries.
[0052] Most high-performance supercapacitors contain organic electrolytes. For example, the electrolyte may include a conductive salt (e.g., tetraethylammonium tetrafluoroborate or TEABF4) dissolved in an acetonitrile solvent (polar solvent). The activated carbon (i.e., high-purity carbon with a minimal amount of oxygen-based functional groups) produced by the purge gas method described herein does not interact with the polar solvent height. The wettability (interaction) between the electrolyte and the non-polar surface of the activated carbon is very poor. Poor wettability can produce a smaller TEABF4 ion mobility in an activated carbon-based electrode, resulting in a poor internal resistance (or ionic impedance or diffusion resistance different from resistance) of an activated carbon-based supercapacitor. Without being bound by theory, adding a wettability enhancer (such as doping aluminum or other suitable wettability enhancers in activated carbon) can improve the ion mobility of the electrolyte (e.g., by improving the ionic interaction between the electrode and the electrolyte).
[0053] Without being bound by theory, it is believed that the activated carbon doped with metal oxides, metals or metal complexes as described herein will provide high capacitance with low internal resistance for supercapacitors and minimize the migration of lithium polysulfides and subsequent deposition of insoluble lithium sulfides into the anode of lithium sulfur batteries. In addition, it has been observed that metal doping reduces the amount of solvent required when the activated carbon slurry is coated on aluminum foil to form an electrode for a supercapacitor and improves the coating characteristics of the activated carbon slurry on aluminum foil.
[0054] In some embodiments, the electrical stabilizer and / or wettability enhancer is non-flammable.
[0055] For example, the preparation of activated carbon using lignin or high lignin feedstocks is described in PCT application No. PCT / CA2022 / 050218 filed on February 15, 2022, the entire contents of which are incorporated herein by reference.
[0056] refer to Figure 1, an exemplary embodiment of a method 100 for preparing metal-doped activated carbon is shown. At 102, mixing is performed to combine one or more electrical stabilizers and / or wettability enhancers with activated carbon, as further described below. In some embodiments, the electrical stabilizer and / or wettability enhancer is provided as a solution, and the solution is mixed with the activated carbon and stirred for a period of time, such as 1 / 2 hour to 1 hour. In some aspects, a ball mill or other suitable device can be used to mix to combine the substances. In some aspects, micro-grinding can be performed at 102. In some aspects, after mixing, the combined substances are further ground using a planetary ball mill or other suitable device for a period of time, such as 1 / 2 hour to 1 hour. If necessary, the mixed and / or ground / micro-ground substances can be further processed at 102. At 104, the mixture is dried. At 106, the mixture is subjected to a purge gas treatment, for example as described in PCT / CA2022 / 050218.
[0057] In one exemplary embodiment, after drying at 104, at 106, the activated carbon is subjected to a purge gas treatment at an elevated temperature. In some embodiments, the purge gas process is performed using a reducing gas in combination with an inert gas. Examples of gases that can be used as reducing gases include hydrogen, ammonia, carbon monoxide, forming gas, synthesis gas, and the like. Forming gas is a mixture of hydrogen and nitrogen known in the art. Synthesis gas is a mixture of carbon monoxide and hydrogen known in the art. Examples of inert gases include nitrogen, helium, and argon.
[0058] In some embodiments, the gas used to perform the purge gas process comprises between about 80% to about 98% inert gas (including any value or sub-range therebetween, such as 82%, 84%, 86%, 88%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, or 97% inert gas) and between about 2% to about 20% reducing gas (including any value or sub-range therebetween, such as 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, or 18%). In some embodiments, the gas used to perform the purge gas process comprises between 90% to 96% inert gas and 4% to 10% reducing gas. In some embodiments, the purge gas contains 96% argon and 4% hydrogen.
[0059] In some embodiments, the activated carbon mixture is provided to the purge gas treatment as a solid thin layer, such as spread on a tray. In some embodiments, the activated carbon mixture remains stationary during the purge gas treatment.
[0060] In some embodiments, the purge gas is applied at a flow rate of about 0.25 L / min to 1 L / min in a 6" tube furnace at atmospheric pressure, including any values therebetween, such as 0.30 L / min, 0.35 L / min, 0.40 L / min, 0.45 L / min, 0.50 L / min, 0.55 L / min, 0.60 L / min, 0.65 L / min, 0.70 L / min, 0.75 L / min, 0.80 L / min, 0.85 L / min, 0.90 L / min, or 0.95 L / min. The flow rate at which the purge gas is applied can be adjusted by one skilled in the art depending on the type of apparatus used to perform the process. Step 106 can be performed in any suitable apparatus, such as a tube furnace, a rotary kiln, a fluidized bed reactor, or other suitable apparatus that can be used in various embodiments.
[0061] In some embodiments, the purge gas is sprayed onto or through the activated carbon material in step 106. In some embodiments, a sufficient amount of purge gas is supplied to the activated carbon material such that there is a molar excess of hydrogen relative to the number of oxygen functional groups in the activated carbon. In some embodiments, the superficial velocity of the purge gas relative to the surface of the activated carbon material is between about 0.25 cm / min and 7.0 cm / min, including any values therebetween, for example, 0.50 cm / min, 0.75 cm / min, 1.0 cm / min, 1.25 cm / min, 1.50 cm / min, 1.75 cm / min, 2.0 cm / min, 2.25 cm / min, 2.50 cm / min, 2.75 cm / min, 3.0 cm / min, 3.25 cm / min, 3.50 cm / min, 3.75 cm / min, 4.0 cm / min, 4.25 cm / min, 4.50 cm / min, 4.75 cm / min, 5.0 cm / min, 5.25 cm / min, 5.50 cm / min, 5.75 cm / min, 6.0 cm / min, 6.25 cm / min, 6.50 cm / min, or 6.75 cm / min.
[0062] In some embodiments, the purge gas process at 106 is performed at an elevated temperature, and the elevated temperature is a temperature in a range between about 750°C and about 950°C, including any values or sub-ranges therebetween, such as 775°C, 800°C, 825°C, 850°C, 875°C, 900°C, 925°C, or 950°C. In some embodiments, the purge gas treatment is carried out for a time period of between about 0.5 hours and about 9 hours, including any values or subranges therebetween, for example, 0.6 hours, 0.7 hours, 0.8 hours, 0.9 hours, 1.0 hours, 1.1 hours, 1.2 hours, 1.3 hours, 1.4 hours, 1.5 hours, 1.6 hours, 1.7 hours, 1.8 hours, 1.9 hours, 2.0 hours, 2.5 hours, 3.0 hours, 3.5 hours, 4.0 hours, 4.5 hours, 5.0 hours, 5.5 hours, 6.0 hours, 6.5 hours, 7.0 hours, 7.5 hours, 8.0 hours, or 8.5 hours.
[0063] In some embodiments, at 102, a suitable activated carbon source is combined with an electrical stabilizer and / or a wettability enhancer. The activated carbon can be ground to a relatively small particle size. In some embodiments, the activated carbon is ground to a size in the range of about 1 μm to about 10 μm, including any value or sub-range therebetween, such as 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, or 9 μm. In one embodiment, the activated carbon is ground to a size in the range of about 1 μm to about 10 μm, with an average size of 6 μm.
[0064] Any suitable form of activated carbon can be used in various embodiments. Suitable activated carbon sources include carbonized biomass, including coconut, nut shells, lignin or high lignin feedstocks, coal, peat, wood, etc., which can be converted into activated carbon in any desired manner.
[0065] In some embodiments, the electrical stabilizer is a conductive metal. In some embodiments, the electrical stabilizer is a transition metal. In some embodiments, the electrical stabilizer is Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pb, Ag, La, Hf, Ta, W, Re, Os, Ir, Pt, Au or Ac. In some embodiments, the electrical stabilizer is Cu. In some embodiments, the electrical stabilizer is Ti, V, Ni, Cr, Co, Cu, Fe, Zn, Mn or Mo. In some embodiments, the electrical stabilizer is a conductive metal. In some embodiments, the electrical stabilizer is a metal having a non-Faraday reaction in a supercapacitor. In some embodiments, the electrical stabilizer is copper (Cu) or nickel (Ni), which is commonly used as a current collector for supercapacitors. In some embodiments, the electrical stabilizer is Cu. In some embodiments in which the electrical stabilizer is Fe, the Fe level in the electrode manufactured using activated carbon is less than 50ppm.
[0066] In some embodiments, the wettability enhancer is aluminum. In some embodiments, the wettability enhancer is an aluminum oxide, such as AlO (aluminum (II) oxide) or Al2O3 (aluminum (III) oxide, i.e., alumina), activated alumina (γ-Al2O3), or any other compound that can provide a better interaction between polar and non-polar substances.
[0067] In some embodiments, the electrical stabilizer and / or wettability enhancer is supplied at 102 as a solution of a metal salt, such as a salt of a metal with chloride, hydroxide, nitrate, sulfate, etc., such as copper nitrate, copper sulfate, aluminum nitrate, aluminum sulfate, etc. In some embodiments, at 102, the metal salt is provided as an aqueous solution or a solution with any acceptable solvent, such as water, methanol, ethanol, and / or any other polar solvent. In an example embodiment, the electrical stabilizer is copper, and the copper is supplied as copper sulfate, such as CuSO4.5H2O. In an example embodiment, the wettability enhancer is aluminum, and the aluminum is supplied as aluminum nitrate, such as Al(NO3)3.9H2O.
[0068] In some embodiments, the amount of electrical stabilizer combined with activated carbon in the final product is in the range of about 0.5 wt % to about 4.0 wt % elemental content, including any value or sub-range therebetween, for example, 0.6 wt %, 0.7 wt %, 0.8 wt %, 0.9 wt %, 1.0 wt %, 1.1 wt %, 1.2 wt %, 1.3 wt %, 1.4 wt %, 1.5 wt %, 1.6 wt %, 1.7 wt %, 1.8 wt %, 1.9 wt %, 2.0 wt %, 2.1 wt %, 2.2 wt %, 2.3 wt %, 2.4 wt %, 2.5 wt %, 2.6 wt %, 2.7 wt %, 2.8 wt %, 2.9 wt %, 3.0 wt %, 3.1 wt %, 3.2 wt %, 3.3 wt %, 3.4 wt %, 3.5 wt %, 3.6 wt %, 3.7 wt %, 3.8 wt %, 3.9 wt %, 4.1 wt %, 4.2 wt %, 4.3 wt %, 4.4 1.8 wt%, 1.9 wt%, 2.0 wt%, 2.1 wt%, 2.2 wt%, 2.3 wt%, 2.4 wt%, 2.5 wt%, 2.6 wt%, 2.7 wt%, 2.8 wt%, 2.9 wt%, 3.0 wt%, 3.1 wt%, 3.2 wt%, 3.3 wt%, 3.4 wt%, 3.5 wt%, 3.6 wt%, 3.7 wt%, 3.8 wt% or 3.9 wt%. In some embodiments, the amount of electrical stabilizer combined with the activated carbon is in the range of about 1 wt % to about 3.5 wt % elemental content based on the elemental content of the metal, including any values or sub-ranges therebetween, for example, 1.0 wt %, 1.1 wt %, 1.2 wt %, 1.3 wt %, 1.4 wt %, 1.5 wt %, 1.6 wt %, 1.7 wt %, 1.8 wt %, 1.9 wt %, 2.0 wt %, 2.1 wt %, 2.2 wt %, 2.3 wt %, 2.4 wt %, 2.5 wt %, 2.6 wt %, 2.7 wt %, 2.8 wt %, 2.9 wt %, 3.0 wt %, 3.1 wt %, 3.2 wt %, 3.3 wt %, 3.4 wt % or 3.5 wt %. In some embodiments, the amount of electrical stabilizer combined with the activated carbon is less than about 4.0 weight percent, including, for example, less than about 3.9 weight percent, 3.8 weight percent, 3.7 weight percent, 3.6 weight percent, 3.5 weight percent, 3.4 weight percent, 3.3 weight percent, 3.2 weight percent, 3.1 weight percent, 3.0 weight percent, 2.9 weight percent, 2.8 weight percent, 2.7 weight percent, 2.6 weight percent, 2.5 weight percent, 2.4 weight percent, 2.3 weight percent, 2.2 weight percent, 2.1 weight percent, 2.0 weight percent, 1.9 weight percent, 1.8 weight percent, 1.7 weight percent, 1.6 weight percent, 1.5 weight percent, 1.4 weight percent, 1.3 weight percent, 1.2 weight percent, 1.1 weight percent, 1.0 weight percent, 0.9 weight percent, 0.8 weight percent, 0.7 weight percent, 0.6 weight percent, or 0.5 weight percent, based on the elemental content of the metal.
[0069] In some embodiments, the amount of wettability enhancer supplied at 102 is in the range of about 0.15 wt % to about 1.50 wt %, including any values or sub-ranges therebetween, such as 0.20 wt %, 0.25 wt %, 0.30 wt %, 0.35 wt %, 0.40 wt %, 0.45 wt %, 0.50 wt %, 0.55 wt %, 0.60 wt %, 0.65 wt %, 0.70 wt %, 0.75 wt %, 0.80 wt %, 0.85 wt %, 0.90 wt %, 0.95 wt %, 1.0 wt %, 1.05 wt %, 1.10 wt %, 1.15 wt %, 1.20 wt %, 1.25 wt %, 1.30 wt %, 1.35 wt %, 1.40 wt %, or 1.45 wt %, based on the elemental content of the metal in the final product. In some embodiments, the amount of wettability enhancer supplied at 102 is in the range of about 0.45 wt % to about 1.00 wt %, based on the elemental content of the metal, including any values or sub-ranges therebetween, such as 0.45 wt %, 0.50 wt %, 0.55 wt %, 0.60 wt %, 0.65 wt %, 0.70 wt %, 0.75 wt %, 0.80 wt %, 0.85 wt %, 0.90 wt %, 0.95 wt %, or 1.0 wt %.
[0070] In some embodiments of producing activated carbon from lignin, the electrical stabilizer is present in an amount between about 2.75 wt % and 3.25 wt %, including any values therebetween, such as 2.80 wt %, 2.85 wt %, 2.90 wt %, 2.95 wt %, 3.0 wt %, 3.05 wt %, 3.10 wt %, 3.15 wt %, or 3.20 wt %, and the wettability enhancer is present in an amount between about 0.50 wt % and 1.25 wt %, including any values therebetween, such as 0.55 wt %, 0.60 wt %, 0.65 wt %, 0.70 wt %, 0.75 wt %, 0.80 wt %, 0.85 wt %, 0.90 wt %, 0.95 wt %, 1.0 wt %, 1.05 wt %, 1.10 wt %, 1.15 wt %, or 1.20 wt %.
[0071] In some embodiments of producing activated carbon from coconut shells, the electrical stabilizer is present in an amount between about 2.75 wt% and 3.25 wt%, including any values therebetween, such as 2.80 wt%, 2.85 wt%, 2.90 wt%, 2.95 wt%, 3.0 wt%, 3.05 wt%, 3.10 wt%, 3.15 wt%, or 3.20 wt%, and the wettability enhancer is present in an amount between about 0.25 wt% and 1.00 wt%, including any values therebetween, such as 0.30 wt%, 0.35 wt%, 0.40 wt%, 0.45 wt%, 0.50 wt%, 0.55 wt%, 0.60 wt%, 0.65 wt%, 0.70 wt%, 0.75 wt%, 0.80 wt%, 0.85 wt%, 0.90 wt%, or 0.95 wt%.
[0072] In some embodiments, any other desired additives or components may be added at 102 in a similar manner as described for electrical stabilizers and wettability enhancers. For example, in some embodiments, conductivity enhancing additives such as graphene, graphite, etc. are added at 102 or after the purge gas treatment is completed at 106.
[0073] In some embodiments, after the activated carbon has been combined with the metal salt, the resulting mixture is dried at 104. Any suitable drying conditions may be used to perform step 104, including ambient conditions. In some embodiments, which are merely examples, the drying is performed at about 70°C, for example, at a temperature between about 60°C and 80°C, in a convection oven for a period of about 48 hours. In some embodiments, the drying is performed at atmospheric pressure. In some embodiments, the drying is performed under vacuum, for example, at a pressure in the range of about 10 mmHg to about 760 mmHg, including any value therebetween, for example, 20 mmHg, 50 mmHg, 100 mmHg, 150 mmHg, 200 mmHg, 250 mmHg, 300 mmHg, 350 mmHg, 400 mmHg, 450 mmHg, 500 mmHg, 550 mmHg, 600 mmHg, 650 mmHg, 700 mmHg, or 750 mmHg. After drying, at 106, the mixture is subjected to a purge gas at an elevated temperature.
[0074] In one exemplary embodiment, aluminum doping of activated carbon is performed with aluminum as a wettability enhancer. Aluminum salts such as aluminum nitrate are converted into a thin layer of aluminum oxide on the surface of the activated carbon. Typical activated carbon as an electrode material is highly non-interactive with polar solvents containing organic electrolytes for supercapacitors and lithium-sulfur batteries. Without being bound by theory, it is believed that the activated carbon doped with aluminum oxide as described herein has interaction and adsorption properties with polar substances, resulting in improved capacitance at fast discharge rates. The aluminum oxide content in the doped activated carbon (which can be expressed as elemental aluminum content, such as the elemental content of the metal in the composition by weight) can be optimized to provide a thin and conductive aluminum oxide layer.
[0075] More specifically and further, without being bound by theory, it is believed that the final product of Al-O treated with a purge gas from aluminum (e.g., provided as aluminum nitrate) is present as activated alumina, and activated alumina is known to be highly effective for the adsorption of sulfur compounds and is hydrophilic. Activated alumina is also known to be highly effective for the adsorption of fluoride. In the following examples, the electrolyte used in the supercapacitor contains fluoroborate ions (BF - 4), which may explain the observed properties of these electrodes. The results described in the Examples herein indicate that Al-doped and Al- and Cu-doped activated carbons formed by purge gas treatment can minimize the formation of lithium polysulfides in the anode side of lithium-sulfur battery applications while providing improved capacitance.
[0076] Further, without being bound by theory, it is believed that the copper doped in the activated carbon exists in the form of pure copper metal without any adsorption and hydrophilic properties. Copper doping can provide improved conductivity to the activated carbon. However, electrodes with copper doped at too high a concentration may reduce the capacitance of the supercapacitor because the copper may block the micropores on and in the activated carbon. Therefore, moderate levels of electrical stabilizers such as copper may be beneficial.
[0077] In an exemplary embodiment, copper doping of activated carbon is performed using copper as an electrical stabilizer. Copper salts such as copper sulfate can be converted into metallic (i.e., elemental) copper to reduce the internal resistance of the supercapacitor while minimizing the blocking of the micropores of the activated carbon by elemental copper. The copper content of the doped activated carbon can be expressed as elemental copper content, such as the elemental content of copper in the composition by weight.
[0078] In one exemplary embodiment, aluminum and copper doping of activated carbon is performed, wherein the aluminum acts as a wettability enhancer and the copper acts as an electrical stabilizer.
[0079] In some embodiments, the resulting activated carbon product has a carbon content of at least about 95%, including between about 90% and about 99%, including any values therebetween, such as 96%, 97%, or 98%.
[0080] In some embodiments, the resulting activated carbon product has a carbon content of at least 2500 m / s as measured using nitrogen adsorption. 2 / g BET surface area, including at least 2600m 2 / g, 2700m 2 / g、2800m 2 / g、2900m 2 / g、3000m 2 / g、3100m 2 / g、3200m 2 / g or 3300m 2 / g. In some embodiments, the resulting activated carbon product has a pore volume of at least 0.8cc / g measured using nitrogen adsorption, including at least 0.85cc / g, 0.90cc / g, 0.95cc / g, 1.00cc / g, 1.05cc / g, 1.10cc / g, 1.15cc / g, or 1.20cc / g. In some embodiments, the resulting activated carbon product has an iodine value of at least 2500mg / g, including at least 2550mg / g, 2600mg / g, 2650mg / g, 2700mg / g, 2750mg / g, 2800mg / g, 2850mg / g, 2900mg / g, 2950mg / g, 3000mg / g, 3050mg / g, 3100mg / g, 3150mg / g, or 3200mg / g. In some embodiments, the resulting activated carbon product has an average particle size of less than 15 μm without micronization, including, for example, less than 14 μm, 13 μm, 12 μm, 11 μm, or 10 μm without micronization, or an average particle size of less than 7 μm with micronization, including, for example, less than 6 μm or less than 7 μm with micronization. In some embodiments, the resulting activated carbon product has a bulk density of 0.25 g / cc or more, including, for example, 0.26 g / cc, 0.27 g / cc, 0.28 g / cc, 0.29 g / cc, 0.30 g / cc, 0.31 g / cc, 0.32 g / cc, 0.33 g / cc, 0.34 g / cc, or 0.35 g / cc or more.
[0081] In some embodiments, the activated carbon products described herein are incorporated into electrodes. Figure 2An example embodiment of a method 200 for making an electrode using activated carbon is shown. At 202, an activated carbon slurry is prepared in a suitable solvent (e.g., N-methylpyrrolidone, NMP) using activated carbon and a binder (e.g., PVF, polyvinylidene fluoride). Optionally, a conductivity enhancer such as graphite is added. At 204, the slurry is homogenized in any suitable manner, such as by ultrasonic treatment. At 206, the resulting slurry is coated on a suitable foil, such as aluminum foil, in any suitable manner (e.g., using a coating machine).
[0082] At 208, the electrode is cut from the coated foil, and at 210, the electrode is hot compressed using any suitable device, such as a Carver laboratory press, for example by first heating the electrode to a suitable temperature, such as 200° C., and then compressing the electrode, for example, at 100 MPa. At 212, the electrode is pre-treated, for example by placing it overnight at 150° C. in a vacuum. At 214, the electrode is assembled in an inert atmosphere, such as an argon-filled glove box, for example, using an airtight button cell (e.g., a CR2032 button cell with Swagelok). Two electrodes can be placed in the cell, with a suitable separator placed between them, and an electrolyte (1.5 M tetraethylammonium tetrafluoroborate (TEABF4) dissolved in acetonitrile) can be added.
[0083] Other methods of making electrodes are known to those skilled in the art and can be used in other embodiments, and the foregoing description provides guidance as to one exemplary method of making electrodes and is not limiting.
[0084] refer to Figure 3 , an example embodiment of a method 300 for preparing an activated carbon cathode for a lithium-sulfur battery is shown. At 302, the activated carbon is mixed with aluminum, for example in the form of aluminum nitrate (Al(NO3)3·9H2O) and copper, for example in the form of copper sulfate (CuSO4·5H2O). At 304, the combined material is dried, and at 306, the material is subjected to a purge gas treatment as described above. Finally, at 308, the activated carbon is impregnated with sulfur, for example using liquid ammonia as described in PCT Publication No. WO 2021 / 0248245, the entire contents of which are incorporated herein by reference, but any suitable method of impregnating the activated carbon may be used and other methods are known to those skilled in the art.
[0085] Figure 4 An example embodiment of a method 400 of making a cathode for a lithium-sulfur battery is shown. Figure 4The method shown is exemplary only, and a person skilled in the art can make the cathode of a lithium-sulfur battery in any suitable manner. At 402, a carbon-sulfur composite slurry is prepared in a suitable solvent (e.g., N-methyl-2-pyrrolidone) using a binder (e.g., polyvinylidene fluoride) and a conductive agent (e.g., graphite). The mixture is homogenized at 404 (e.g., by ultrasonic treatment) and then coated on an aluminum foil at 406, for example, using a doctor blade coater. At 408, the coated foil is dried and the coated foil is shaped as needed (e.g., cut into a desired shape) to form a cathode at 410, and the cathode is compressed in any suitable manner (e.g., using a Carver laboratory press) at 412. The cathode is combined with a lithium metal anode and then assembled at 414, and an electrolyte (e.g., 1M bis(trifluoromethanesulfonyl)imide lithium (LiN(SO2CF3)2) and 1% lithium nitrate in 1,2-dimethoxyethane (DME) and 1,3-dioxolane (DOXL)) is added.
[0086] In some embodiments, a lithium-sulfur battery having an electrode incorporated with activated carbon is provided, wherein the electrode comprises activated carbon, the activated carbon comprising an electrical stabilizer at a concentration in the range of about 0.5 wt % to about 3.5 wt %, and / or wherein the electrode comprises activated carbon, the activated carbon comprising a wettability enhancer at a concentration in the range of about 0.1 wt % to about 0.2 wt %.
[0087] In some embodiments, a supercapacitor having an electrode incorporated with activated carbon is provided, wherein the electrode comprises activated carbon comprising an electrical stabilizer at a concentration in the range of about 1 wt % to about 3.5 wt %, and / or wherein the electrode comprises activated carbon comprising a wettability enhancer at a concentration in the range of about 0.45 wt % to about 1.0 wt %.
[0088] In some embodiments, electrodes made from activated carbon materials as described herein are incorporated into solid-state lithium batteries (e.g., lithium-sulfur batteries). In some embodiments, activated carbon materials described herein are incorporated into capacitors or supercapacitors.
[0089] In some embodiments, electrodes made from activated carbon materials as described herein are incorporated into structures and / or components of building structures for energy storage. In some embodiments, energy storage systems incorporating activated carbon prepared as described herein can provide higher energy density than materials made from conventional activated carbon, can provide lower risk of heat buildup within building components or building structures than materials made from conventional activated carbon, can provide a greater number of charge and discharge cycles than materials made from conventional activated carbon, and / or can provide a faster charge rate than materials made from conventional activated carbon.
[0090] In some embodiments, energy storage systems made using activated carbon as described herein are embedded in modular building components, such as panels that can be used as interior or exterior cladding, floors, roofs, countertops, stairs or stairwells, cabinets, or other building components of a building. In some embodiments, modular building components incorporate at least one supercapacitor or at least one battery having electrodes made from activated carbon materials as described herein.
[0091] In some embodiments, the energy storage system is permanently incorporated into the modular building component, such as being integrally cast into the modular building component when the modular building component is manufactured, or being permanently fixed therein. In some embodiments, the energy storage system can be removably incorporated into the modular building component, such as being inserted into a compartment within the modular building component that is accessible via an access door, access panel, or other removable or removable covering structure.
[0092] In some embodiments, an energy storage system made using activated carbon as described herein is installed within a building structure during its construction or erection. The energy storage system may be incorporated into any desired portion of a building structure during construction, such as a portion of a building structure that will minimally interfere with ordinary use of the building structure, such as a wall, floor, ceiling, or interior components thereof.
[0093] Providing a removably coupled energy storage system allows the system to be removed for repair or replacement in the event of a failure or once the energy storage system has reached the end of its useful useful life. In embodiments where the energy storage system is permanently installed, if a particular energy storage system fails or reaches the end of its useful useful life, use of that particular energy storage system can be discontinued and / or that particular energy storage system can be disconnected from other energy storage systems while the physical energy storage unit remains in place within the building structure.
[0094] In some embodiments, an energy storage system or modular building components including the energy storage system are installed in a warehouse or other building structure that is relatively large in size and does not typically have a large concentration of people (e.g., as in the case of an office building or a residential building structure).
[0095] The individual energy storage systems integrated into the modular building components or directly into the building can be interconnected with each other and to the main power grid in any manner. For example, appropriate connectors and cables can be incorporated into the modular building components or into the building structure to allow the individual energy storage systems to be interconnected.
[0096] Depending on the particular circumstances in which the energy storage system is deployed, the thermal characteristics of the portion of the building or modular building component in which the energy storage system is incorporated may be selected. For example, in embodiments in which the energy storage system is deployed in modular building panels that also function as insulation, the material of the modular building panels or building components may be selected to be thermally insulating. In alternative embodiments, the material of the modular building panels or building components may be selected to be thermally conductive to allow heat to transfer away from the energy storage system included therein.
[0097] In embodiments in which a surface of a portion of a building or modular building components incorporating an energy storage system will be exposed to external elements, at least the surface of the portion of the building or modular building components exposed to the external elements should be weatherproof (i.e., capable of withstanding rain, snow, wind, sun, and other weather conditions to which it may be exposed).
[0098] In embodiments where the energy storage system is incorporated into modular building components, the modular building components may be provided with any suitable surface configurations, connectors, and / or fasteners to allow the modular building components to be assembled into a building structure. Any of a variety of available modular building systems may be used for this purpose. In some embodiments, the connectors or fasteners incorporated into the modular building components may also serve as electrical connectors to connect the included energy storage system to the main electrical system of the building structure.
[0099] Example
[0100] Certain embodiments are further described with reference to the following examples, which are intended to be illustrative and not limiting in scope.
[0101] Example 1 - Evaluation of Metal Doping of Activated Carbon
[0102] Aluminum (Al) as a wettability enhancer and / or copper (Cu) as an electrical stabilizer were added to commercially available activated carbon (YP50F, Calgon Carbon Corporation, denoted as YPAC). The resulting Al and Cu doped YPAC was treated with a purge gas (containing 10% hydrogen and 90% nitrogen) at 800°C to 900°C for 3 to 6 hours. Supercapacitors fabricated with these Al and Cu doped electrodes were tested.
[0103] For these studies, activated carbon YP50F obtained from Calgon Carbon Corporation and indicated in this specification as YPAC was used. Figure 1Methods for describing the properties. In this study, supercapacitors with the following compositions were fabricated and tested. (1) Al-doped activated carbon: Aluminum salts (aluminum nitrate in this study) were converted into conductive Al-O, with a thin layer on the resulting activated carbon. Without being bound, it is believed that the Al-O doped activated carbon will have ionic interactions and adsorption properties with polar substances, resulting in improved capacitance at fast discharge rates. The optimal Al-O content in the doped activated carbon (expressed as elemental Al content by weight in this example) was determined to find a thin and conductive Al-O layer. (2) Cu-doped activated carbon: Copper salts (copper sulfate in this study) were converted into metallic (elemental) copper. Without being bound, it is believed that this improves the internal resistance of the supercapacitor while minimizing the blocking of the micropores of YPAC by elemental copper. In this study, the optimal copper content in the doped activated carbon (expressed as elemental Cu content by weight in this example) was determined. (3) Al-Cu composite doping of activated carbon: The combination of Al and Cu doping can provide improved properties for supercapacitors over those provided by either Al or Cu doping alone.
[0104] Materials and methods
[0105] Al, Cu and Al-Cu composite doping tests were performed using YP50F, Calgon Carbon Corporation (denoted as YPAC). Original YP50F (denoted as YPAC) is a commercial activated carbon widely used in activated carbon-based supercapacitor applications because it has high surface area, low ash content and low electrical resistance. The inventors treated YPAC with a purge gas (without metal doping) to remove oxygen chemically bound to the YPAC. Untreated YPAC and purge gas treated YPAC (denoted as YPAC+SG) were used as baselines (baseline 1 and baseline 2, respectively) for comparison tests with metal-doped and purge gas treated YPAC.
[0106] To prepare metal-doped activated carbon, aluminum nitrate (Al(NO3)3·9H2O) and copper sulfate (CuSO4·5H2O) were dissolved in RO (reverse osmosis) water to add Al and Cu to YPAC, respectively. The prepared solutions contained 0.075% to 2.5% weight / weight of elemental Al (or 0.14% to 4.85% of aluminum nitrate hydrate) and 1% to 9.2% weight / weight of elemental Cu (or 0.53% to 5.36% of copper sulfate hydrate) per liter, respectively. Specifically, the following salt solutions were prepared for doping: 0.14% Al(NO3)3·9H2O (98%) for 0.075%; 0.28% Al(NO3)3·9H2O (98%) for 0.15% Al; 0.57% Al(NO3)3·9H2O (98%) for 0.3% Al; 0.85% Al(NO3)3·9H2O (98%) for 0.45% Al; 1.44% Al(NO3)3·9H2O (98%) for 0.75% Al. l; 1.91% Al(NO3)3·9H2O (98%), for 1% Al; 4.85% Al(NO3)3·9H2O (98%), for 2.5%; 0.53% CuSO4·5H2O (99%), for 1% Cu; 1.92% CuSO4·5H2O (99%), for 3.5% Cu; 2.71% CuSO4·5H2O (99%), for 4.9% Cu; 5.36% CuSO4·5H2O (99%), for 9.2% Cu.
[0107] Under constant stirring conditions, 6 g of YPAC was soaked in 45 mL of the prepared solution at room temperature for 1 hour to add the desired Al and Cu content to YPAC, respectively. The soaked YPAC solution was placed in an oven at 70 ° C for drying to remove water (until there is no observable mass change). Using the same method as Al addition, YPAC (6 g) was prepared using Al (45 mL) and Cu (45 mL) salt solutions for Al-Cu composite doped YPAC. Various samples were prepared as follows:
[0108] Baseline 1: YPAC as received (Baseline 1, not treated with purge gas).
[0109] • Baseline 2: As-prepared YPAC (undoped with metal) using purge gas treatment.
[0110] Al-doped activated carbon: Al salt (aluminum nitrate) was added to YPAC to prepare 0.075%, 0.15%, 0.3%, 0.45%, 1% and 2.5% Al (based on the weight content of elemental Al) in YPAC, respectively. Al source (converted to Al2O3 after purge gas treatment)
[0111] Used as a polarizing agent (i.e., wettability enhancer) to improve the ionic interactions of the resulting activated carbon.
[0112] Cu-doped activated carbon: Copper sulfate was added to YPAC to prepare 1 wt%, 3.5 wt%, and 4.87 wt% Cu in YPAC, respectively. The Cu source (converted to metallic copper after purge gas treatment) was used as a conductive agent to further stabilize the electrode.
[0113] Al-Cu composite doped activated carbon: Aluminum nitrate and copper sulfate were added to YPAC to prepare 0.45 wt% Al-3.51 wt% Cu and 0.75 wt% Al-3.51 wt% Cu in YPAC, respectively. These concentrations were chosen based on the best results of the tested supercapacitors made with Al-doped and Cu-doped YPAC.
[0114] The dried YPAC+Al, YPAC+Cu and YPAC+Al-Cu products were treated with a purge gas flow rate of 1 L / min, wherein the dried YPAC+Al, YPAC+Cu and YPAC+Al-Cu composites were flushed with a gas mixture containing 90% nitrogen and 10% hydrogen at 800° C. to 900° C. for 3 to 6 hours. The diameter of the 6-inch (15.24 cm) and surface area of 182 cm 2 In a furnace of 1 L / min, a flow rate of 1 L / min produces a flow velocity of about 5.5 cm / min through the treated product. During this period, the treated product is exposed to a molar excess of hydrogen relative to the estimated oxygen content of the activated carbon (about 11%). Without being bound, it is believed that this purge gas treatment removes oxygen groups chemically bound to the activated carbon and converts conductive Al, Cu and Al-Cu salts into conductive Al-O, Cu and Al-Cu complexes in the activated carbon, respectively. For example, thermal decomposition of Al(NO3)3 to Al2O3 and thermal decomposition of CuSO4 to metallic Cu may occur. The former reaction may involve partial reaction with the supplied reducing gas. In addition, without being bound by theory, it is believed that the reducing gas prevents the copper from converting back to copper oxide during the process. After drying and purge gas treatment of the activated carbon product, one (1) mole of Al(NO3)3·9H2O and CuSO4·5H2O become 0.5 mole of Al2O3 (or 1 mole of Al expressed as elemental Al) and 1 mole of metallic Cu in the activated carbon, respectively.
[0115] Figure 2The manufacturing method of the electrode used in the supercapacitor tested in this embodiment is shown. Using 80% activated carbon, 10% graphite and 10% binder (polyvinylidene fluoride) and N-methylpyrrolidone (NMP) as a solvent (for standard activated carbon, the mass ratio is 1 solid: 2.5NMP, or for doped activated carbon, it is 1 solid: 2NMP), activated carbon slurry is prepared by high-energy ultrasonic treatment. The activated carbon slurry is coated on aluminum foil using a coating machine. The coated aluminum foil is dried overnight in a vacuum oven at 80°C. The dried aluminum foil is cut into a circle with a diameter of 15.0mm. The resulting electrode is rolled at 200°C for 2 minutes and immediately compressed at 100MPa. The compressed electrode is pretreated overnight at 150°C in a vacuum oven, and then the electrode is placed in an Ar-filled glove box for supercapacitor assembly. Electrodes are assembled in an Ar-filled glove box using airtight button cells (CR2032). Two identical electrodes are placed in a battery. A separator (Celgard, 25 μm) was placed between the two electrodes. The electrolyte (100 μL) used for the cell assembly contained 1.5 M tetraethylammonium tetrafluoroborate dissolved in acetonitrile.
[0116] It was observed that when electrodes were made using metal-doped activated carbon, approximately 20% less solvent was required to prepare a slurry suitable for coating on aluminum foil used to make electrodes, compared to an activated carbon control that more closely mirrors the properties of a standard activated carbon, and it was further observed that the metal-doped activated carbon slurry exhibited better physical properties when coated on aluminum foil. Specifically, it was observed that the metal-doped activated carbon coating on aluminum foil was more robust than activated carbon alone, as assessed using a finger squeeze test.
[0117] Current charge and discharge (GCD) tests were performed to determine the specific capacitance of the supercapacitor (tests were performed from slow charge and discharge (CD) of 0.5A / g to fast charge and discharge (CD) of 5A / g). GCD measurements used potentials ranging from 0V to 2.3V at various current densities ranging from 0.5A / g to 5A / g. Capacitance retention (%) and internal resistance (mOhm) were calculated according to the following formulas:
[0118]
[0119] The IR drop values were measured at current densities of 0.5 A / g to 5 A / g. The internal resistance (milliohm) was calculated based on the correction between the IR drop and the current density.
[0120] result
[0121] Al-doped activated carbon
[0122] Initial performance results of supercapacitors (SCs) with baseline and Al-doped and purge-gas treated YPAC in Table 1 were tested at slow and fast discharge rates with current densities of 0.5 A / g and 5 A / g, respectively. Table 1 shows the performance of SCs with the following baseline and Al-doped YPAC (+SG treatment):
[0123] YPAC (Baseline 1): As is
[0124] YPAC+3hSG (Baseline 2): YPAC as is treated with SG at 800°C for 3 hours
[0125] YPAC+Al-doping+3hSG: YPAC was doped with 0.075%, 0.15%, 0.3%, 0.45%, 0.75% and 1% Al (using aluminum nitrate), respectively, and then treated with SG at 800°C for 3 hours.
[0126] For each YPAC-based SC group, four SC cells (CR2032) were prepared. Three best cells were selected from each Al-doped and SG-treated group for comparison with the baseline. The cells noted in Table 1 were not used for comparison to determine the optimal Al doping content. As shown in Table 1, Baseline 1 and Baseline 2 SCs achieved 80F / g to 84F / g at a current density of 0.5A / g (slow discharge) and 8F / g to 20F / g at a current density of 5A / g (fast discharge), while the Al-doped and SG-treated YPAC groups (#36, #34, and #21) achieved 81F / g to 92F / g at 0.5A / g and 41F / g to 71F / g at 5A / g. The YPAC used in these YPAC groups (#36, #43, and #21) was doped with 0.45 wt% to 1 wt% Al in elemental form, indicating the optimal range of Al dopant content under these specific test conditions. The baseline SC has an internal resistance ranging from 44 mOhm to 94 mOhm. The Al-doped and SG-treated YPAC group has an internal resistance ranging from 23 mOhm to 62 mOhm, resulting in higher capacitance retention than the baseline.
[0127] Table 1. Initial properties of SCs treated with Al doping and SG using 0.075% to 2.5% Al .
[0128]
[0129]
[0130]
[0131] Table 2 shows the performance results of the best supercapacitors (SCs) in the Al-doped group compared to the baseline 1 and 2 SCs. Each SC was cycled 300 times at 0.5 A / g and 300 times at 5 A / g. The performance of the Al-doped YPAC SCs (80 F / g to 86 F / g at 0.5 A / g, 30 F / g to 51 F / g at 5 A / g, 30 milliohms to 79 milliohms) is better than the baseline SCs (79 F / g to 82 F / g at 1 A / g, and 19 F / g to 34 F / g at 5 A / g, and 56 milliohms to 74 milliohms).
[0132] Table 2. Optimal SCs treated with Al from 0.45% to 1% Al and treated with SG for 600 cycles (at 0.5 A / g Long-term cycling performance after 300 cycles and 300 cycles at 5 A / g
[0133]
[0134] Cu-doped activated carbon
[0135] Table 3 shows the initial performance results of Cu doped and purge gas treated supercapacitors (SCs) compared to baseline SCs. Table 3 summarizes the performance results of SCs with the following baselines and Al doped YPAC (+SG treatment):
[0136] YPAC (Baseline 1): As is
[0137] YPAC+3hSG (Baseline 2): YPAC as is treated with SG at 800°C for 3 hours
[0138] YPAC+Cu doping+3hSG: YPAC was doped with 1.0%, 3.51%, 4.87% and 9.2% Cu, respectively, and then treated with SG at 800°C for 3 hours.
[0139] Table 3 shows that cells with optimal Cu dopant content in YPAC (1% to 3.5% Cu, #22 and #32) perform better than the baseline SC (79 F / g to 82 F / g at 0.5 A / g and 19 F / g to 34 F / g at 5 A / g, and 56 mOhm to 74 mOhm).
[0140] Table 3. Initial properties of SCs treated with Cu doping and SG using 1% to 9.2% Cu .
[0141]
[0142]
[0143] Table 4 shows the long cycle performance results of the best supercapacitors (SCs) in the Cu doped group compared to the baseline 1 and 2 SCs. Each SC was cycled 300 times at 0.5 A / g and 300 times at 5 A / g. The Cu doped YPAC SCs performed better than the baseline SCs as follows:
[0144] Cu doped and SG treated groups (#22 and #32): 78F / g to 78F / g at 0.5A / g, 42F / g to 51F / g at 5A / g, 31mOhm to 46mOhm
[0145] Baseline SC: 79F / g to 82F / g at 0.5A / g, and 19F / g to 34F / g at 5A / g, and 56mOhm to 74mOhm
[0146] Table 4. Best SCs treated with Cu from 1% to 4.87% Al and treated with SG for 600 cycles (at 0.5 A / g Long-term cycling performance after 300 cycles and 300 cycles at 5 A / g
[0147]
[0148] Al-Cu composite doping of activated carbon
[0149] Al and Cu doping each have advantages. Without being bound by theory, low Al doping provides better interaction and adsorption characteristics with polar substances for the electrode. High Cu doping provides improved electrode conductivity for SC applications. Table 5 shows the purge gas treatment for converting the Al-Cu mixture into a conductive Al-Cu composite. First, a volume of 45 mL each was added to a crucible, and the prepared crucible (90 mL in total) was placed in an oven at 70 ° C until all water was removed. The dried solid mixture was treated with a purge gas at 800 ° C to 900 ° C for 3 to 6 hours. These tests were performed only with a mixture solution (without activated carbon) to determine the optimal temperature and holding time before the activated carbon metal doping.
[0150] Tests 1 and 2 show treatment of the mixture with a purge gas at 800°C for 3 hours and 6 hours. The resulting product of Test 1 (3 hours at 800°C) is not conductive, while the product of Test 2 becomes conductive after SG treatment at 800°C for 6 hours. The resulting product of Test 3 (3 hours at 900°C) is conductive. The product of Test 3 has a relative resistivity of 323% based on MTI graphite. The product of Test 4 achieves greater conductivity after purge gas treatment at 900°C for 6 hours and has a relative resistivity of 180%.
[0151] Table 5. Electrical conductivity of Al-Cu composites after purge gas treatment .
[0152]
[0153] The mass balance of the mixture solution is examined in Table 6. Table 6 compares the collected mass of the product of Run 4 with the theoretical mass based on the initial mass of aluminum nitrate and copper sulfate, which are completely converted to the Al-Cu complex (without being bound by theory, it is believed to be Al2O3 uniformly mixed with elemental copper). Table 6 shows that the calculated mass of the product is consistent with the collected mass of the product of Run 4.
[0154] Table 6. Mass balance of Al-Cu composites after purge gas treatment .
[0155]
[0156] Table 7 summarizes the initial performance results of Al and Cu doped and purge gas treated supercapacitors (SCs) compared to baseline SCs. Table 7 shows the initial performance results generated by the following experiments:
[0157] YPAC (Baseline 1, #17): As is.
[0158] YPAC+3hSG (Baseline 2, #20): As-received YPAC was treated with SG at 800°C for 3 hours.
[0159] YPAC+0.45%Al+3.51%Cu doping+3hSG900 (#38-1): YPAC was doped with 0.45%Al and 3.51%Cu, and then treated with SG at 900°C for 3 hours.
[0160] YPAC+0.45%Al+3.51%Cu doping+6hSG900 (#42): YPAC was doped with 0.45%Al and 3.51%Cu, respectively, and then treated with SG at 900°C for 6 hours.
[0161] YPAC+0.75%Al+3.51%Cu doping+6hSG900 (#46): YPAC was doped with 0.75%Al and 3.51%Cu, respectively, and then treated with SG at 900°C for 6 hours.
[0162] Groups #42 and #46 achieved the following results that were superior to Baselines 1 and 2.
[0163] • Groups doped with Al and Cu and treated with SG (#42 and #46): 87 F / g to 92 F / g at 0.5 A / g, 37 F / g to 64 F / g at 5 A / g, 29 mOhm to 51 mOhm.
[0164] • Baseline SC: 79 to 82 F / g at 0.5 A / g, and 19 to 34 F / g and 56 to 74 mOhms at 5 A / g.
[0165] Group #38-1 produced similar results to Baseline 2, indicating that the 3-hour purge gas treatment time was not long enough for Al-Cu doping in YPAC under the tested conditions.
[0166] Table 7. Initial properties of SCs with Al-Cu doping and purge gas treatment .
[0167]
[0168]
[0169] Remark:
[0170] 1. The #42-1 cell was not charged during the initial test, and after two days of rest, it showed 97 F / g at 0.5 A / g and 57 F / g at 5 A / g.
[0171] 2. The #46-4 battery was unstable during the initial test. After standing for 1 week, it became stable, reaching 111 F / g at 0.5 A / g and 64 F / g at 5 A / g (internal resistance of 51 mΩ).
[0172] Table 8 shows the long cycle performance results of the best SCs in the Al and Cu doped groups compared to the baseline 1 and 2 SCs. The following results were obtained for each SC group after 300 cycles at 1 A / g and 300 cycles at 10 A / g. The Al and Cu doped YPAC SCs performed better than the baseline SCs as follows:
[0173] • Groups doped with Al and Cu and treated with purge gas (#42-2 and #46-2): 86 F / g to 90 F / g at 0.5 A / g, 53 F / g to 57 F / g at 5 A / g, 36 mOhm to 38 mOhm.
[0174] • Baseline SC: 79 to 82 F / g at 0.5 A / g, and 19 to 34 F / g and 56 to 74 mOhms at 5 A / g.
[0175] Table 8. Optimal supercapacitors treated with Al and Cu doping and purge gas using optimal Al and Cu contents at 600 Long-term cycling performance after 300 cycles (300 cycles at 0.5 A / g and 300 cycles at 5 A / g) .
[0176]
[0177] In summary, the following performance data are demonstrated by the foregoing examples:
[0178] The supercapacitor based on Baseline 2 achieved similar performance to Baseline 1 at a slow discharge of 0.5 A / g (low ampere load), while the supercapacitor based on Baseline 2 performed significantly better than Baseline 1 at a fast discharge of 5 A / g (high ampere load).
[0179] SC based on YPAC+Al+SG achieves better performance than baselines 1 and 2.
[0180] The YPAC+Cu+SG based SC exhibits better performance than baselines 1 and 2 at a fast discharge of 10 A / g.
[0181] • The YPAC+Al+Cu+SG based SC achieved the best results among the compared SCs.
[0182] The optimum content of the Al-Cu mixture in YPAC is any concentration within the optimum range of 0.45% to 1% Al and 1% to 3.5% Cu by mass.
[0183] Table 9 summarizes the results of various experimental samples to demonstrate how treatment with purge gas and embedding of aluminum and copper improves the capacitance of the capacitors tested. The metal-doped activated carbon was found to produce capacitors with 2.9 times the area and volume capacitance of capacitors made with conventional activated carbon.
[0184] Table 9. Area and volume capacitance of selected experimental examples .
[0185]
[0186] In summary, the above examples show that purge gas treatment together with Al and Cu doping improves the performance of supercapacitors made of activated carbon (YPAC). Without being bound, it is believed that purge gas treatment with Al doping (Al2O3 doping) and Cu doping can improve ionic interactions and provide improved resistance characteristics for supercapacitors based on activated carbon with high capacitance and high stability. Low Al doping improves the wettability of the electrode by providing an electrode with improved hydrophilicity and adsorption characteristics. High Cu doping provides improved electrode conductivity for supercapacitor applications. Without being bound by theory, the electrolyte used to test supercapacitors in these examples contains a conductive salt tetraethylammonium tetrafluoroborate TEABF4 dissolved in acetonitrile, and acetonitrile is a hydrophilic solvent. The activated carbon produced by purge gas treatment has a high degree of hydrophobicity due to the removal of oxygen-based functional groups. Therefore, due to the hydrophobic surface of activated carbon, the wettability (i.e., hydrophilicity) of the electrode is poor. It is believed that this poor wettability can cause the ion mobility of TEABF4 in the activated carbon electrode, resulting in a poor internal resistance of the supercapacitor based on activated carbon. Doping with aluminum, which is believed to be converted into the form of Al2O3 or AlO, can improve the wettability of the electrolyte with the activated carbon electrode surface, thereby improving the performance of the supercapacitor.
[0187] Without limitation, embodiments may include the following:
[0188] An activated carbon product doped with aluminum and treated at elevated temperature using a purge gas process, wherein the concentration of elemental aluminum in the activated carbon is in the range of 0.45 wt. % to 1 wt. % (e.g. in the form of Al2O3).
[0189] An activated carbon product doped with copper and treated with a purge gas process at elevated temperature, wherein the elemental copper concentration is in the range of 1 wt% to 3.5 wt%.
[0190] An activated carbon product doped with aluminum and copper and treated with a purge gas process at elevated temperature, wherein the elemental concentrations of aluminum and copper are between 0.45 wt% and 1 wt% and less than 3.5 wt%, respectively (or wherein the elemental concentration of copper is between 1 wt% and 3.5 wt%).
[0191] When used as an electrode material, coating activated carbon doped with a wettability enhancer on aluminum foil for electrode fabrication requires 20% less solvent than typical activated carbon.
[0192] Example 2 - Supercapacitors prepared using metal-doped and SG-treated LAAC
[0193] Activated carbon made from lignin-A ("LAAC") (micronized) was treated with a purge gas treatment and used as a baseline for supercapacitor performance testing in comparison with supercapacitors with metal doped + SG treated LAAC. Based on the optimal dopant content using YP50AC, LAAC was doped with an Al source ranging from 0.45% to 1.5% Al and 3% Cu, followed by a purge gas (SG) treatment.
[0194] Supercapacitors were assembled using baseline LAAC and metal doped + SG treated LAAC. Four (4) cells were assembled per group and tested at a low ampere load of 0.5A / g and a high ampere load of 5A / g. The initial capacitance and internal resistance of each cell were tested. Based on high capacitance and low internal resistance, the best cell in each group was selected for 600 cycle testing.
[0195] Table 10 shows the properties of SG-LAAC (micronized). The average size of the ground LAAC was 5.8 μm. The ground LAAC was used for metal doping and SG treatment. The ground LAAC had a carbon content of 97.5% and an ash content of 0.29%. The iodine value of the ground LAAC was 3,050 mg / g, which was slightly reduced before grinding. The correlation between the iodine value measured from the previous activated carbon sample and the BET surface area value (based on nitrogen adsorption) (y = 0.9374x + 47.781, R 2 = 0.9416) and the BET surface area of the ground LAAC was calculated to be 2,900 m 2 / g. The relative resistance of the milled LAAC is within the typical value (225%).
[0196] Table 10. Properties of SG-LAAC (micronized) for metal doping and SG treatment .
[0197]
[0198] Note: The surface area (m2) was calculated using the correlation between the iodine value and the BET surface area value. 2 / g).
[0199] Table 11 summarizes the initial capacitance and initial internal resistance of the supercapacitors (SCs). Group #111 is a baseline SC with SG-treated LAAC. Groups #112, #113, #124, #122, and #123 are SCs with metal-doped and SG-treated LAACs, which are compared to the baseline SC. Based on internal resistance and capacitance, the worst cells in each group were excluded to select the best cells.
[0200] At low amperometric loading (0.5 A / g), the baseline SC (LAAC with SG treatment) achieved the best performance (144 F / g to 155 F / g) compared to SCs with doped and SG treated LAAC (groups #112, #113, #124, #122 and #123, 127 F / g to 155 F / g), while at high amperometric loading, the performance of groups #113 and #124 SCs was consistently better than the baseline SCs (106 F / g to 123 F / g). Groups #113 and #124 SCs had LAAC-based electrodes doped with 0.75 wt% Al+3 wt% Cu and 1 wt% Al+3 wt% Cu, respectively. These doped LAACs were treated with SG prior to SC assembly.
[0201] The initial internal resistance values of the SC groups with metal doped and SG treated LAAC were tested (28mΩ-g to 62mΩ-g) lower than (or better than) the baseline SC (43mΩ-g to 62mΩ-g), except for group #112 (30mΩ-g to 92mΩ-g). These low internal resistance values of the doped and SG treated SC groups are the reason for achieving higher capacitance values than the baseline SC at high ampere loads.
[0202] These results also suggest that the doped Al and Cu sources can partially block the surface of the SG-treated LAAC, resulting in slightly lower capacitance than the baseline SC at low ampere loads. Based on the consistent results of capacitance and internal resistance, the best cells from the baseline group and other groups were selected for 600 cycle testing, with the exception of group #112, which performed inconsistently and had poor internal resistance.
[0203] Table 11. Initial performance of SG-treated LAAC compared with doped and SG-treated LAAC .
[0204]
[0205]
[0206]
[0207] Table 12 shows the capacitance and internal resistance of the best SC selected from the baseline group and other groups except group #112, and then tested after 300 cycles at low ampere load and 300 cycles at high ampere load. At low ampere, the baseline SC (150F / g) performs better than the other groups (117F / g to 126F / g), while at high ampere load, the baseline SC achieves a lower capacitance (97F / g) than groups #113 and #124 (109F / g to 113F / g).
[0208] The internal resistance of the SCs of groups #112, #113, and #124 ranged from 28 mΩ-g to 33 mΩ-g, which was much lower than the baseline SC (78 mΩ-g). The internal resistance of the SCs of groups #112, #113, and #124 had little change after 600 cycles, while the internal resistance of the baseline SC became worse, indicating that the baseline SC was unstable under high ampere loads.
[0209] Since groups #113 and #124 consistently produced better capacitance (109 F / g to 113 F / g or 12% to 16% higher) and lower internal resistance than the baseline SC, the optimal metal dopant levels for this particular activated carbon under the conditions tested appear to be 0.75% Al + 3% Cu and 1% Al + 3% Cu for LAAC. This optimal level is slightly higher than the optimal dopant levels determined for YP50AC (0.45% Al + 3% Cu and 0.75% Al + 3% Cu).
[0210] It was also noted that the SG-treated LAAC had low resistance (225%) and ultra-high surface area (2,900 m 2 / g), which is 434% and 1,876m higher than YP50AC (SG treated YP50AC 2 Without being bound by theory, electrode enhancement with metal doping may improve the properties of YP50AC better than LAAC, which already has relatively low resistance and high surface area (or high ion adsorption capacity), sufficient for supercapacitor (SC) applications at low ampere loads.
[0211] Table 12. 600 cycle performance of SG-treated LAAC compared with doped and SG-treated LAAC .
[0212]
[0213] Based on this study, the following findings were obtained:
[0214] Under the tested conditions, the optimal Al and Cu dopant contents of LAAC were determined to be 0.75%Al+3%Cu and 1%Al+3%Cu, which are slightly higher than the dopant contents of YP50AC (0.45%Al+3%Cu and 0.75%Al+3%Cu).
[0215] Under high ampere loading, the SC with optimal Al-Cu doping and SG-treated LAAC was demonstrated to have 12% to 16% higher capacitance than the baseline SC (SC with SG-treated LAAC), which is significant for high ampere SC (5 A / g).
[0216] The optimal Al-Cu doped and SG treated LAAC electrodes do not improve the capacitance at low ampere loading (0.5 A / g).
[0217] Without being bound by theory, it is believed that electrode enhancement with doping can improve YP50AC better than LAAC because LAAC already has low resistance and high surface area (or high ion adsorption capacity) sufficient for SC applications (under low amperage loads).
[0218] Example 3 - LiSB with metal doping, SG treatment and S impregnation LAAC
[0219] LiS batteries use sulfur as the active material in the cathode, and during the discharge mode, the sulfur is reduced to polysulfide intermediates. These polysulfides are polar and highly soluble in the electrolyte, leaking from the cathode to the anode (known as the shuttle effect). The diffused polysulfides are further reduced to lower-order sulfides and deposited as passivated solids, which is irreversible. Therefore, LiS batteries cannot provide the theoretical energy density. This study uses highly ion-adsorbing AC with micropores (width <2nm) and metal doping technology to capture polysulfides in the cathode to overcome the shuttle effect.
[0220] The main purpose of this study was to optimize the content of Al-Cu mixture in the cathode of LiS batteries containing non-conductive sulfur. In order to improve the interaction of lignin-based activated carbon cathode with polar-based electrolyte in LiSB system, while minimizing the conductivity loss caused by sulfur impregnation after doping and SG treatment, the Al-Cu mixture content of LAAC doping is lower than the optimal Al-Cu mixture content for supercapacitors for LiSB. Without being bound by theory, it is believed that sulfur impregnation of activated carbon to produce the cathode of LiS battery may further increase the resistance of the cathode. Sulfur is electrically insulating, and the micropore space of activated carbon is occupied by impregnated sulfur.
[0221] Al-Cu mixture doping was performed using lignin-based activated carbon or LAAC. LAAC was produced using lignin A obtained from a lignin recovery plant in Alberta, Canada, which has high surface area, low ash content, and low electrical resistivity. Figure 3 The procedure shown was to dope the activated carbon with metals and dry it at a temperature between 60°C and 80°C.
[0222] For this example, LAAC was doped with an Al doping range of 0-0.45% Al and 3% Cu. To dope the desired content of Al-Cu mixture, LAAC (6 g) was also added to 45 mL of aluminum nitrate (0.28% Al(NO3)3·9H2O (98%) for 0.15% wt / wt Al; 0.57% Al(NO3)3·9H2O (98%) for 0.3% wt / wt Al; and 0.85% Al(NO3)3·9H2O (98%) for 0.45% wt / wt Al) and 45 mL of copper sulfate (1.63% CuSO4·5H2O (99%) for 3% wt / wt Cu) solutions, respectively. The soaked LAAC solution was placed in an oven at 70°C to remove water until no further mass change was observed. The following metal-doped LAAC samples were prepared for SG treatment:
[0223] Baseline: LAAC treated with SG
[0224] Al-Cu mixture doping: Aluminum nitrate and copper sulfate are added to LAAC to prepare an Al-Cu mixture with the following content:
[0225] ο0.15%Al+3%Cu(wt / wt)
[0226] ο0.3%Al+3%Cu(wt / wt)
[0227] ο0.45%Al+3%Cu(wt / wt)
[0228] The dried LAAC and Al-Cu doped LAAC products were treated with a purge gas containing 90% nitrogen and 10% hydrogen. The purge gas was flushed through the dried LAAC and Al-Cu doped LAAC products in a 6-inch tube at a temperature of 900°C at a flow rate of 100 mL / min for 6 hours. This purge gas treatment removes oxygen groups chemically bonded to the activated carbon and converts the Al-Cu salts into a conductive Al-Cu mixture in the activated carbon. Through this treatment, one (1) mole of Al(NO3)3·9H2O and CuSO4·5H2O becomes 0.5 mole of Al2O3 (or 1 mole of Al expressed as elemental Al) and 1 mole of metallic Cu, respectively.
[0229] The sulfur impregnation method involves dissolving granular S° (elemental sulfur) in liquid ammonia (LNH3) at ammonia vapor pressure (about 110 psig at room temperature), for example as described in PCT Publication No. WO 2021 / 248245. The carbon is then simply immersed in the solution and the S° dissolved in the LNH3 is adsorbed onto the LAAC. The S-impregnated activated carbon can then be collected after the sample is removed from the pressurized environment and the LHN3 evaporates at room temperature (RT). The sulfur is left behind after evaporation, and the impregnated carbon is ready for use as a cathode material for a LiS battery. The following cathode materials were prepared:
[0230] Baseline: LAAC treated with SG, containing 63.12% sulfur
[0231] 0.15% Al and 3.0% Cu doped and SG treated LAAC, containing 71.0% wt / wt sulfur
[0232] 0.3% Al and 3.0% Cu doped and SG treated LAAC, containing 67.3% wt / wt sulfur
[0233] 0.45% Al and 3.0% Cu doped and SG treated LAAC, containing 65.97% wt / wt sulfur
[0234] LiSB Assembly
[0235] In the method for manufacturing the cathode of LiSB (according to Figure 4 The example method shown), S-impregnated activated carbon, polyvinylidene fluoride (PVDF) (binder) and graphite (as a conductive agent) were suspended in a slurry using N-methyl-2-pyrrolidone (NMP) in a mass ratio of 60:20:20, respectively. The carbon-sulfur (CS) composite slurry was homogenized for 20 minutes using ultrasonic treatment and then coated onto an Al foil using a doctor blade coater. The Al foil, now thinly coated with the CS composite material, was dried at 60°C and vacuum for 24 hours to remove the NMP. A 15 mm diameter disc was punched out as the cathode. A 15 mm diameter lithium disc was punched out from a lithium strip (40 mm wide and 0.6 mm thick) in an argon-filled glove box for use as the anode material, and the electrode was assembled using CR 2032 (swagelock type button cell) in an argon-filled glove box. An electrolyte (containing 1 M lithium bis(trifluoromethanesulfonyl)imide (LiN(SO2CF3)2) and 1% lithium nitrate in 1,2-dimethoxyethane (DME) and 1,3-dioxolane (DOXL)) was added to each cell, with the electrolyte volume ranging from 40 μL to 115 μL per mg of sulfur in the cathode.
[0236] LiSB Performance Test
[0237] Constant current charge and discharge (GCD) was tested to determine the specific capacity (mAh / g) of Li-S batteries with lignin-based cathodes. GCD measurements used potentials ranging from 1.7V to 3.0V (100% DoD, depth of discharge) at a current density of 1.0 coulomb (C) / g or 1,675mA / g. The LiS batteries were also cycled 500 times using the GCD method to test cyclability. The capacity and capacity retention were calculated using the following formula:
[0238] Capacitance from GCD (mAh / g) = Applied current (A) × Discharge time (seconds) / 60 × 60 × Mass of sulfur in cathode (g)
[0239] Capacity retention rate (%) = Capacity at the number of cycles tested with 100% DoD / Initial capacity at the first cycle tested with 100% DoD
[0240] Characteristics of SG-treated LAAC for sulfur impregnation
[0241] The main chemical and adsorption properties (iodine value and surface area) of LAAC are shown in Table 13. SG treated LAAC had a carbon content of 98.1%, an iodine value of 3,140 mg / g and a surface area of 3,203 m2 / g with an average pore diameter of 1.13 nm and an average particle size of 14.3 μm.
[0242] Table 13. Comparison of LAAC characteristics .
[0243]
[0244] LiSBs were assembled using the following sulfur-impregnated LAAC-based cathode materials:
[0245] Battery LC21-27-5: 0% Al + 0% Cu + SG + 63.12% S (baseline)
[0246] Battery LC21-25-9: 0.15% Al + 3.0% Cu + SG + 71.0% S
[0247] Battery LC21-23-16: 0.3% Al + 3.0% Cu + SG + 67.30% S
[0248] Battery LC21-26-7: 0.45% Al + 3.0% Cu + SG + 65.97% S
[0249] These batteries (CR 2032, 15mm diameter) have the following components:
[0250] Cathode: 60(AC-S):20(graphite):20(PVDF) coated on aluminum foil
[0251] • Electrolyte: 1 M lithium bis(trifluoromethanesulfonyl)imide (LiN(SO2CF3)2) and 1% lithium nitrate in 1,2-dimethoxyethane (DME) and 1,3-dioxolane (DOXL).
[0252] Electrolyte dosage: 40 μL to 52 μL per 1 mg of active sulfur in the cathode
[0253] ·Separator: Celgard 25 micron membrane
[0254] Anode: 0.2mm lithium metal
[0255] Performance of LiSB with sulfur-impregnated LAAC cathode
[0256] Table 14 shows the performance results of LiSB with baseline LAAC and doped and SG treated LAAC containing 63% to 71% sulfur content. All cells were cycled 500 times at 1 C / g using 100% depth of discharge (1.7 V to 3.0 V).
[0257] The second cycle capacity of LiSB with baseline cathode (LC21-27-5) is 590 mAh / g, which is about 5% lower than the first cycle capacity (622 mAh / g). The capacity of baseline LiSB continues to decline until the 500th cycle. The capacity retention rate of LC21-27-5 after 500 cycles is 55.9% (based on the first cycle capacity). Interestingly, the second cycle capacity of LiSB with 0.15% Al+3% Cu+SG cathode (LC 21-25-9) is 665 mAh / g, which is a 10% increase over the first cycle capacity (594 mAh / g). The capacity retention rate (%) of LC 21-25-9 is calculated based on the second capacity. The 500 cycle capacity retention rate of LC21-25-9 is 74.4%, which is a significant improvement compared with the baseline LiSB.
[0258] LiSB with other metal-doped and SG-treated cathodes (0.3% Al + 3% Cu + SG for LC21-23-16 and 0.45% Al + 3% Cu + SG for LC21-26-7) have initial capacities of 601 mAh / g and 570 mAh / g, respectively. Both batteries have worse capacity retention than the baseline battery (36.1% and 33.7%, respectively).
[0259] Table 14. LiS cells with sulfur-impregnated LAAC at 1 C / g and 100% DoD for 500 Cycle test.
[0260]
[0261]
[0262] Two optimal LiSBs with baseline (LC21-27-8) and 0.15%+3%Cu+SG (LC21-25-10) were tested to confirm the effect of doping+SG treatment on the improvement of capacity retention of LiSB. The LiSB with baseline cathode was tested with a 1st cycle capacity of 696 mAh / g and a capacity retention of 55.7% (388 mAh / g) after the 500th cycle, while the LiSB with 0.15%+3%Cu+SG cathode (LC21-25-10) achieved 1st cycle capacity and 2nd cycle capacity of 462 mAh / g and 578 mAh / g, respectively. Based on the 2nd capacity value, the 500 cycle capacity retention of LC21-25-10 was 70.5% (407 mAh / g). As observed in Table 14, the 2nd cycle capacity of LC21-25-10 in Table 15 also increased over the initial capacity value. This increase in capacity after the 1st capacity is shown in Figures 5 to 12 as discussed further below.
[0263] Table 15. LiS cells with baseline cathodes and cathodes with optimal doping and SG treatment at 1C / g and LiSB Comparison of 500 cycles test at 100% DoD .
[0264]
[0265] Figures 5 to 8 The 500 cycle performance of LiS cells (LC21-27-5 and LC21-27-8) with baseline LAAC is shown, and Figures 9 to 12 The 500 cycle performance of LiS cells (LC21-25-9 and LC21-25-10) with 0.15%Al+3%Cu+SG LAAC is shown. Figure 7 , Figure 8 , Fig.11 and Fig.12 Each shows an enlarged view of the capacity retention rate of only the first 50 cycles. That is, Figure 7 Shows Figure 5 The enlarged graph of the capacity retention rate of only the first 50 cycles, Figure 8 Shows Figure 6 The enlarged graph of the capacity retention rate of only the first 50 cycles, Fig.11 Shows Fig. 9 A zoomed-in graph of the capacity retention for only the first 50 cycles, and Fig.12 Shows Fig.10 A zoomed-in view of the capacity retention for only the first 50 cycles. Figures 5 to 8It is shown that the capacity and capacity retention of LiS cells with the baseline (SG-treated LAAC, non-metal-doped) slightly increase in the first 50 cycles (maximum increase of 4.3% for LC21-27-5 and gradually decrease for LC21-27-8) and continue to decrease between the 100th and 500th cycles. Figures 7 and 8 The capacity retention of the baseline LiSB over the first 50 cycles is shown.
[0266] Figures 9 to 12 It is shown that the capacity and capacity retention of the LiS batteries (LC21-25-9 and LC21-25-10) with 0.15% Al + 3% Cu + SG increase significantly over 50 cycles (for LC21-25-9, the maximum capacity increase is 8.2% based on the 2nd cycle, and for LC21-25-10, the maximum capacity increase is 10.8% based on the 2nd cycle), and then gradually decrease between the 100th and 500th cycles. Figure 11 to Figure 12 The capacity retention of LiS cells with 0.15% Al and 3% Cu+SG over the first 50 cycles is shown.
[0267] The test results of LiS cells fabricated with 0.15%Al+3%Cu+SG cathodes indicate that lithium polysulfides (polar) generated (reduced) by active sulfur in the cathode during the discharge mode of LiSB interact effectively in the doped and SG-treated LAAC and are better captured in the cathode than in the baseline LiS cell (SG-treated LAAC cathode).
[0268] In summary, the comparative results of LiS cells with baseline and LiS cells with metal doping and SG-LAAC show that the capacity and capacity retention of LiSB are significantly improved when LAAC is doped with 0.15% Al and 3% Cu and treated with purge gas.
[0269] Although a number of exemplary aspects and embodiments have been discussed above, those skilled in the art will recognize certain modifications, permutations, additions and sub-combinations thereof. It is therefore intended that the following appended claims and claims introduced thereafter be interpreted as including all such modifications, permutations, additions and sub-combinations consistent with the broadest interpretation of the entire specification.
[0270] References
[0271] The following references are related to the subject matter described herein. Each of the following references is incorporated herein by reference in its entirety.
[0272] · Quach, Nguyen Khanh Nguyen et al. (2017) The Influence of the Activation Temperature on the Structural Properties of the Activated Carbon Xerogels and Their Electrochemical Performance, Advances in Materials Science and Engineering, 2017, 8308612, doi.org / 10.1155 / 2017 / 8308612。
Claims
1. A composition comprising activated carbon, an electrical stabilizer and a wettability enhancer.
2. A composition comprising activated carbon, an electrical stabilizer and / or a wettability enhancer.
3. A method for producing activated carbon, the method comprising: combining the activated carbon with an electrical stabilizer and a wettability enhancer to form an activated carbon mixture; as well as The activated carbon mixture is exposed to a purge gas at an elevated temperature.
4. A method for producing activated carbon, the method comprising: combining the activated carbon with an electrical stabilizer and / or a wettability enhancer to form an activated carbon mixture; as well as The activated carbon mixture is exposed to a purge gas at an elevated temperature.
5. The method of any one of claims 3 or 4 or any other claim herein, wherein the purge gas comprises a combination of an inert gas and a reducing gas.
6. A method according to any one of claims 3 to 5 or any other claim herein, wherein the inert gas comprises nitrogen, argon or helium; and wherein the reducing gas comprises hydrogen, ammonia, carbon monoxide, forming gas or synthesis gas.
7. The method of any one of claims 3 to 6 or any other claim herein, wherein the purge gas comprises between about 80% and about 98% of the inert gas and about 2% to about 20% of the reducing gas.
8. The method of any one of claims 3 to 7 or any other claim herein, wherein the first elevated temperature is between about 750°C and about 950°C.
9. The method of any one of claims 3 to 8 or any other claim herein, wherein during the step of exposing the activated carbon to the purge gas, the purge gas is supplied at a flow rate between 0.25 L / min and 1.0 L / min.
10. The method of any one of claims 3 to 9 or any other claim herein, wherein during the step of exposing the activated carbon to the purge gas, the purge gas is sprayed onto or through the activated carbon.
11. The method of claim 10 or any other claim herein, wherein the sweep gas is sprayed onto or through the activated carbon at a superficial velocity of between 0.25 cm / min and 7.0 cm / min relative to the surface of the activated carbon.
12. The method of any one of claims 3 to 11 or any other claim herein, wherein the step of exposing the activated carbon to the purge gas is performed at atmospheric pressure.
13. The method of any one of claims 3 to 12 or any other claim herein, wherein the step of exposing the activated carbon to the purge gas is performed for a period of between 0.5 hours and 9 hours.
14. The method of any one of claims 3 to 13 or any other claim herein, comprising drying the activated carbon mixture prior to the step of exposing the activated carbon mixture to the purge gas.
15. The method of any one of claims 3 to 14 or any other claim herein, comprising micronizing the activated carbon prior to the step of exposing the activated carbon mixture to the purge gas.
16. A composition prepared by the method of any one of claims 3 to 15 or any other claim herein.
17. The composition or method of any one of claims 1 to 16 or any other claim herein, wherein the electrical stabilizer comprises a conductive metal.
18. The composition or method of any one of claims 1 to 17 or any other claim herein, wherein the electrical stabilizer comprises a transition metal.
19. The composition or method of any one of claims 1 to 18 or any other claim herein, wherein the electrical stabilizer comprises Sc, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pb, Ag, La, Hf, Ta, W, Re, Os, Ir, Pt, Au, or Ac.
20. The composition or method of any one of claims 1 to 19 or any other claim herein, wherein the electrical stabilizer comprises copper.
21. The composition or method of any one of claims 1 to 20 or any other claim herein, wherein the wettability enhancer comprises aluminum.
22. The composition or method of any one of claims 1 to 21 or any other claim herein, wherein the wettability enhancer comprises alumina or activated alumina (γ-Al2O3).
23. The composition or method of any one of claims 1 to 22 or any other claim herein, wherein the wettability enhancing agent comprises a compound that provides enhanced interaction between polar and non-polar substances.
24. The composition or method of any one of claims 1 to 23 or any other claim herein, wherein the electrical stabilizer is present in an amount of about 0.5 wt % to about 4.0 wt % based on the elemental content of the electrical stabilizer, optionally about 1 wt % to about 3.5 wt % based on the elemental content of the electrical stabilizer.
25. The composition or method of any one of claims 1 to 24 or any other claim herein, wherein the wettability enhancer is present in an amount from about 0.15 wt % to about 1.5 wt % based on the elemental content of the wettability enhancer, optionally from about 0.45 wt % to about 1.0 wt % based on the elemental content of the wettability enhancer.
26. The composition or method of any one of claims 1 to 25 or any other claim herein, wherein the activated carbon is produced from lignin, wherein the electrical stabilizer is present in an amount between about 2.75 wt% and 3.25 wt%, and wherein the wettability enhancer is present in an amount between about 0.50 wt% and 1.25 wt%.
27. The composition or method of any one of claims 1 to 25 or any other claim herein, wherein the activated carbon is produced from coconut shells, wherein the electrical stabilizer is present in an amount between about 2.75 wt% and 3.25 wt%, and wherein the wettability enhancer is present in an amount between about 0.25 wt% and 1.0 wt%.
28. The composition or method of any one of claims 1 to 27 or any other claim herein, wherein the electrical stabilizer and the wettability enhancer are non-flammable.
29. A composition according to any one of claims 1 to 2 or 16 to 28 or any other claim herein, or a composition produced by a method according to any one of claims 3 to 28 or any other claim herein, wherein: The activated carbon is produced from lignin or high-lignin raw materials and has at least 2500 m 2 / g BET surface area; The activated carbon has a pore volume of at least 1 cc / g, which is primarily micropores; The activated carbon is produced from lignin or high lignin feedstock and has an average particle size of less than about 15 μm without micronization or less than about 7 μm with micronization; and / or The activated carbon has a bulk density of at least about 0.25 g / cc.
30. An apparatus for performing a method according to any one of claims 3 to 28 or any other claim herein.
31. An activated carbon prepared by the method according to any one of claims 3 to 28 or any other claim herein.
32. An electrode comprising the composition of any one of claims 1 to 2 or 16 to 29 or a composition prepared by the method of any one of claims 3 to 28 or any other claim herein.
33. A supercapacitor or battery comprising an electrode according to claim 32 or any other claim herein.
34. A lithium-sulfur battery comprising an electrode according to claim 32 or any other claim herein, wherein the electrode comprises activated carbon comprising the electrical stabilizer at a concentration in the range of about 0.5 wt % to about 3.5 wt %, and / or wherein the electrode comprises activated carbon comprising the wettability enhancer at a concentration in the range of about 0.1 wt % to about 0.2 wt %.
35. An ultracapacitor comprising an electrode according to claim 32 or any other claim herein, wherein the electrode comprises activated carbon comprising the electrical stabilizer at a concentration ranging from about 1 wt % to about 3.5 wt %, and / or wherein the electrode comprises activated carbon comprising the wettability enhancer at a concentration ranging from about 0.45 wt % to about 1.0 wt %.
36. A building or modular building component comprising an energy storage system comprising a supercapacitor or battery comprising an electrode according to claim 32 or any other claim herein.
37. A building or modular building component comprising an energy storage system comprising activated carbon according to claim 31 or any other claim herein.
38. A building or modular building component according to any one of claims 36 to 37 or any other claim herein, wherein the modular building component or portion of the building incorporating the energy storage system is thermally insulated.
39. A building or modular building component according to any one of claims 36 to 38 or any other claim herein, wherein the modular building component or portion of the building incorporating the energy storage system is thermally conductive.
40. A building or modular building component according to any one of claims 36 to 39 or any other claim herein, wherein the modular building component or portion of the building incorporating the energy storage system is weatherproof.
41. A modular building component according to any one of claims 36 to 40 or any other claim herein, wherein the modular building component comprises an interior or exterior cladding panel, a floor panel, a roof panel, a countertop, a staircase or a cabinet.
42. A building as claimed in any one of claims 36 to 40 or any other claim herein wherein the energy storage system is incorporated into walls, floors, ceilings and / or internal components of the building.
43. A modular building component or a building according to any one of claims 36 to 42 or any other claim herein wherein the energy storage system is permanently incorporated into the modular building component or the building.
44. A modular building component or a building according to any one of claims 36 to 43 or any other claim herein, wherein the energy storage system is removably incorporated into the modular building component or the building, optionally by being included in a compartment accessible via an access door, access panel or removable covering structure.
45. A building or modular building component according to any one of claims 36 to 44 or any other claim herein, comprising a connector for coupling the energy storage system to an electrical system of the building or a building comprising the modular building component.
46. A building according to any one of claims 36 to 40 or 42 to 45 or any other claim herein, or a building comprising modular building components according to any one of claims 36 to 45 or any other claim herein, wherein the building is a warehouse.
Citation Information
Patent Citations
Sulphur cathodes, sulphur cathode materials, and apparatus and methods for making same
WO2021248245A1