Method for overcoming slag pit defect on surface of casting blank

By improving the slag adhesion condition of the sector-shaped second-stage rollers, the problem of slag pit defects on the surface of the slab is solved, the occurrence rate of defects is significantly reduced, and the quality of the slab and production efficiency are improved.

CN118832129APending Publication Date: 2024-10-25SGIS SONGSHAN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411201710.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Slag pit defects on the surface of the cast slab are difficult to detect and deal with in a timely manner, resulting in increased production costs, reduced product quality, and extended delivery times.

Method used

By improving the slag adhesion situation of the sector-shaped second-section rollers, including improving water quality, eliminating the inner arc roller, adding an external cooling water system, and standardizing roller maintenance and offline requirements, the defects of slag pits on the surface of the slab are solved.

Benefits of technology

Significantly reduced the incidence of slag pit defects on the slab surface from 30% to 3%, improved the quality of the slab, and reduced production costs and delivery time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118832129A_ABST
    Figure CN118832129A_ABST
Patent Text Reader

Abstract

The invention discloses a method for overcoming the defect of slag pits on the surface of a casting blank. The invention provides a method for solving the casting blank surface slag pit defect. The method comprises the step of solving the casting blank surface slag pit defect by improving bonded slag of a fan-shaped two-section roller. According to the method, the reason for causing the casting blank surface slag pit defect is that slag adheres to the surface of a fan-shaped two-section roller of a secondary cooling chamber, the slag adheres to the surface of the roller, poor cooling and the quality of the roller are greatly related, part of the roller adheres to the slag continuously, part of the roller adheres to the slag discontinuously, and part of the roller does not adhere to the slag; therefore, the defect of slag pits on the surface of the casting blank is overcome by improving the slag sticking condition of the fan-shaped two-section roller.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to a method for solving slag pit defects on the surface of a casting blank. Background Art

[0002] The quality of the continuous casting billet surface determines whether the billet needs finishing before hot processing. It is a key factor affecting metal yield and cost. In addition, hot delivery, hot loading or direct rolling of continuous casting billets requires the billet surface quality to be zero defect. Figure 1 As shown in the figure, Figure a shows the slag pit defect on the surface of the billet before peeling, and Figures b1 and b2 show the slag pit defect on the surface of the billet after peeling). The "slag pit" defect on the billet surface is a defect that is difficult to detect through conventional manual inspection. After the billet is produced from the casting machine, its surface is no different from that of a normal billet. The billet must be peeled before it can be inspected and found. Its macroscopic morphology is irregular, irregular pits of varying sizes and depths of 1 to 3 mm distributed on the upper and lower surfaces of the billet after peeling. The depth of some defects even exceeds 5 mm. After the billet is rolled into round steel, defects such as scarring, "cracks", and folding will form. Because defects cannot be discovered and handled in time, batch defects are usually formed.

[0003] The current processing methods mainly have the following problems:

[0004] (1) After the ingot is cooled, it is peeled and inspected, and then the ingot that can be saved by grinding and finishing is ground, which increases the production cost of the steel ingot.

[0005] (2) After the ingots are peeled and inspected, those ingots that cannot be repaired and saved are picked out and declared scrap on site.

[0006] (3) After the ingot is rolled into round steel, magnetic leakage detection is carried out to check the surface quality of the round steel, which increases the detection cost and prolongs the delivery time. Summary of the invention

[0007] The purpose of the present invention is to overcome the defects of the prior art and provide a method for solving the slag pit defects on the surface of the casting.

[0008] The present invention solves the technical problem by adopting the following technical solutions.

[0009] The invention provides a method for solving the slag pit defect on the surface of the ingot, which comprises: solving the slag pit defect on the surface of the ingot by improving the slag sticking of the fan-shaped two-stage roller.

[0010] The present invention has the following beneficial effects:

[0011] The present invention provides a method for solving the slag pit defect on the surface of the ingot, and the method for solving the slag pit defect on the surface of the ingot includes: solving the slag pit defect on the surface of the ingot by improving the slag sticking on the fan-shaped second-stage roller. In the present invention, the cause of the slag pit defect on the surface of the ingot is found out through on-site full-process tracking that the slag sticking on the surface of the fan-shaped second-stage roller in the second cooling chamber is the slag sticking on the surface of the roller. The slag sticking on the surface of the roller is greatly correlated with poor cooling and roller quality. Some rollers have continuous slag sticking, some have intermittent slag sticking, and some have no slag sticking. Therefore, the slag pit defect on the surface of the ingot is solved by improving the slag sticking on the surface of the fan-shaped second-stage roller. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0013] Figure 1 The slag pit defect on the surface of the ingot. Figure a shows the slag pit defect on the surface of the ingot before peeling, and Figures b1 and b2 show the slag pit defect on the surface of the ingot after peeling.

[0014] Figure 2 Figure 1 is a physical picture of the "slag" of the slag pit defect of the casting billet. Figures a and b are physical pictures of the "slag" of the slag pit defect of the casting billet in different states.

[0015] Figure 3 This is a schematic diagram of slag sticking to the fan-shaped two-stage roller;

[0016] Figure 4 is a schematic diagram of a fan-shaped two-section stick, a is a schematic diagram of a fan-shaped two-section stick before optimization, and b is a schematic diagram of a fan-shaped two-section stick before optimization. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out under normal conditions. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0018] A method for solving slag pit defects on the surface of a casting billet provided by an embodiment of the present invention is described in detail below.

[0019] The invention provides a method for solving the slag pit defect on the surface of the ingot, which comprises: solving the slag pit defect on the surface of the ingot by improving the slag sticking of the fan-shaped two-stage roller.

[0020] In an optional embodiment, the following steps are included: first, a composition analysis is performed on the "slag" at the location of the slag pit defect on the surface of the ingot, and the composition of the "slag" is determined to be a mixture of protective slag and iron oxide, and the "slag pit" defect on the surface of the ingot is determined to be related to the pressure of "iron oxide scale" on the surface of the ingot, and through comparative analysis, it is found that the "slag pit" defect has no direct relationship with the protective slag and steel type, but is related to the casting machine, and then the cause of the slag pit defect on the surface of the ingot is found out through on-site full-process tracking, and the slag pit defect on the surface of the ingot is solved by improving the slag sticking of the fan-shaped second-stage roller.

[0021] In an optional embodiment, the slag sticking to the second-stage sector roller is reduced by improving the water quality and ensuring the heat transfer effect of the cooling water.

[0022] In an optional embodiment, the method for improving water quality includes: regulating the turbidity, Ca content, and oil content of the continuous casting secondary cooling water, requiring the water turbidity to be ≤20mg / L, Ca ≤210mg / L, and oil ≤2mg / L. By regulating and improving the water quality, the cooling heat transfer is effectively solved. The slag sticking to the fan-shaped second-stage roller is reduced.

[0023] In an optional embodiment, the second-segment sector-shaped inner arc roller is optimized to reduce slag sticking to the second-segment sector-shaped roller.

[0024] In an optional embodiment, optimizing the fan-shaped two-stage inner arc roller includes: eliminating the fan-shaped two-stage inner arc roller to "cures" the roller slag sticking. Through comparative tests, it is found that eliminating the inner arc roller has no effect on the internal quality of the casting, and eliminating the fan-shaped two-stage inner arc roller can "cures" the roller slag sticking.

[0025] In an optional embodiment, the second-stage fan-shaped outer arc roller is modified to add external cooling water to reduce the amount of residue sticking to the second-stage fan-shaped roller.

[0026] In an optional embodiment, the modification of the fan-shaped second-stage outer arc roller to add external cooling water includes: adding an external cooling water system to the fan-shaped second-stage outer arc roller, and during production, cooling water is sprayed to the outer arc roller through the external cooling water system, and the cooling water cools the outer arc roller to reduce the roller temperature and improve roller slag sticking, and at the same time, washes the slag stuck on the roller to prevent the slag from sticking to the casting. Adding an external cooling water system to the fan-shaped second-stage outer arc roller, the cooling water can cool the outer arc roller to reduce the roller temperature, improve roller slag sticking, and at the same time, wash the slag stuck on the roller to prevent the slag from sticking to the casting.

[0027] In an optional embodiment, the slag sticking to the second-stage sector roller is reduced by standardizing the maintenance and offline requirements of the second-stage sector roller.

[0028] In an optional embodiment, the standard requirements for the maintenance and offline of the sector-shaped two-stage roller include: requiring the online roller to be free of cracks, surfacing marks, and roller surface roughness Ra 2.0. By standardizing the roller maintenance and offline requirements, the online roller must be free of cracks, surfacing marks, and roller surface roughness Ra 2.0. Improving the roller surface quality can improve the "slag" hanging on the roller surface.

[0029] The present invention will be further described below in conjunction with the embodiments.

[0030] The embodiment of the present invention provides a method for solving regular depression defects on the surface of a casting, comprising the following steps:

[0031] The "slag" of the slag pit defect of the casting billet is as follows Figure 2 As shown in the figure, Figure a and Figure b are the physical pictures of the "slag" of the slag pit defects in different states of the ingot. The composition analysis of the "slag" at the regular pit defect position on the surface of the ingot is shown in the following table:

[0032] Element Weight % Atomic% CK 11.54 25.02 OK 28.03 45.61 Na K 1.06 1.20 Al K 0.33 0.32 S K 0.41 0.38 K 0.23 0.17 Ca K 0.36 0.23 Mn 0.37 0.18 Fe K 57.67 26.89 Totals 100.00

[0033] According to the table above, the composition of "slag" is a mixture of protective slag and iron oxide. It can be basically determined that the "slag pit" defect on the surface of the ingot is related to the pressure of "iron oxide scale" on the surface of the ingot. And through comparative analysis, the "slag pit" defect has no direct relationship with the protective slag and steel type, but should be related to the casting machine. Therefore, the cause of the slag pit defect on the surface of the ingot is found through on-site full-process tracking: the surface of the second-stage roller of the second cooling chamber is sticky slag (such as Figure 3 As shown in the figure, the slag sticking on the roller surface is closely related to poor cooling and roller quality. Some rollers have continuous slag sticking, some have intermittent slag sticking, and some have no slag sticking. Therefore, improving the slag sticking on the fan-shaped second-stage roller is the fundamental source of solving the slag pit defects on the surface of the ingot.

[0034] The technical solution provided by the embodiment of the present invention is: to optimize and improve from four aspects: first, to improve the water quality and ensure the heat transfer effect of cooling water; second, to optimize the fan-shaped two-stage roller and cancel the inner arc roller; third, to modify the fan-shaped two-stage outer arc roller and add external cooling water; fourth, to standardize the roller maintenance and offline requirements. Specifically:

[0035] (1) Improve water quality. Standardize the turbidity, Ca, and oil content of the secondary cooling water for continuous casting. The turbidity of the water is required to be ≤20mg / L, Ca≤210mg / L, and oil≤2mg / L. By standardizing and improving the water quality, the cooling and heat transfer problems can be effectively solved.

[0036] (2) Optimize the fan-shaped two-stage roller and cancel the inner arc roller. Through comparative tests, canceling the inner arc roller has no effect on the internal quality of the ingot. The cancellation of the fan-shaped two-stage inner arc roller "cures" the roller slag sticking. Figure 4 As shown in Figure a and Figure b, the inner arc roller is eliminated in Figure b.

[0037] (3) The fan-shaped two-stage outer arc roller is modified to add external cooling water, and an external cooling water pipeline is added to the fan-shaped two-stage outer arc roller (such as Figure 4 As shown in Figure b, an external cooling water pipeline is added under the fan-shaped second-stage outer arc roller). During production, cooling water is sprayed to the outer arc roller through the external cooling water system. The cooling water cools the outer arc roller to reduce the roller temperature and improve the roller slag sticking. At the same time, it has a flushing effect on the slag stuck on the roller to prevent the slag from sticking to the casting.

[0038] (4) Fourth, standardize the roller maintenance and offline requirements. The online rollers must be free of cracks, surfacing marks, and roller surface roughness Ra 2.0. Improving the roller surface quality can improve the "slag" hanging on the roller surface.

[0039] Example 1

[0040] A method for solving regular depression defects on the surface of a casting blank comprises the following steps:

[0041] (1) Improve water quality. Standardize the turbidity, Ca, and oil content of the secondary cooling water for continuous casting. The turbidity is 15mg / L, Ca is 120mg / L, and oil is 0.5mg / L. By standardizing and improving water quality, cooling and heat transfer are effectively solved.

[0042] (2) Optimize the fan-shaped two-stage roller and eliminate the inner arc roller. Comparative tests show that eliminating the inner arc roller has no effect on the internal quality of the ingot. Eliminating the fan-shaped two-stage inner arc roller can "cure" the roller slag sticking.

[0043] (3) The fan-shaped two-stage outer arc roller is modified to add external cooling water. An external cooling water system is added to the fan-shaped two-stage outer arc roller. During production, cooling water is sprayed to the outer arc roller through the external cooling water system. The cooling water cools the outer arc roller to reduce the roller temperature and improve the roller slag sticking. At the same time, it has a flushing effect on the slag stuck on the roller to prevent the slag from sticking to the casting.

[0044] (4) Standardize roller maintenance and offline requirements. The online rollers must be free of cracks, surfacing marks, and roller surface roughness Ra2.0. Improving the roller surface quality can improve the "slag" hanging on the roller surface.

[0045] After adopting the technical solution provided by the embodiment of the present invention, the "slag pit" defect of the casting machine ingot is significantly reduced, and the defect incidence rate is reduced from 30% before the improvement to 3%, and the "slag pit" defect of the casting ingot is fundamentally improved.

[0046] Comparative Example 1 (Original Scheme)

[0047] (1) The turbidity, Ca and oil content of the secondary cooling water of continuous casting are not standardized. The turbidity of the water is 40mg / L, Ca is 250mg / L, and the oil is 2.5mg / L. Oil and Ca in the cooling water will significantly reduce the heat transfer effect of the cooling water. Poor heat transfer effect leads to high roller temperature and easy slag sticking. At the same time, the roller strength deteriorates and cracks easily occur. The rough surface and other problems aggravate the slag sticking.

[0048] (2) The fan-shaped two-stage roller has no external cooling. Without external roller cooling, the roller has poor cooling effect, and the roller is prone to sticking slag when the temperature is high. At the same time, the roller strength deteriorates, and cracks and surface roughness are prone to occur, which aggravates the sticking of slag.

[0049] (3) Roller maintenance and offline requirements are not standardized. The online rollers have cracks, surfacing marks, and roller surface roughness greater than Ra 5.0. The roller roughness is high, and the roller surface is uneven, which is conducive to slag sticking to the roller.

[0050] In this comparative example, the rollers were seriously slag-sticked. Through peeling inspection, the casting machine's ingot "slag pit" defects were serious, and the defect incidence rate reached 35%.

[0051] Comparative Example 2

[0052] The steps are similar to those in Example 1, except that the turbidity, Ca, and oil content of the secondary cooling water of continuous casting are not standardized, and the turbidity of the water is 35 mg / L, Ca is 150 mg / L, and the oil is 1.0 mg / L. The heat transfer of the secondary cooling water is the same as before the improvement, but the external cooling and roller optimization reduce the probability of slag sticking to the roller. The results of the peeling inspection showed that the "slag pit" defects of the casting machine were serious, and the defect incidence rate reached 20%.

[0053] Comparative Example 3

[0054] The steps are similar to those in Example 1, except that the roller maintenance and offline requirements are not standardized, the online rollers have cracks, surfacing marks, and the roller surface roughness is Ra 3.0. The roller roughness is high, and the roller surface is uneven, which increases the probability of roller sticking slag. The results of the peeling inspection showed that the "slag pit" defect of the casting machine was serious, and the defect incidence rate reached 15%.

[0055] Comparative Example 4

[0056] The steps are similar to those in Example 1, except that no external cooling water system is added to the fan-shaped second-stage roller. Water quality specifications and roller optimization have a good effect on roller slag sticking, but the water volume in the fan-shaped second stage is small and there is more slag here, so the effect is not particularly obvious. Results Through peeling inspection, the "slag pit" defect of the casting machine is serious, and the defect incidence rate is 20%.

[0057] It can be seen from the above content that the present invention provides a method for solving the slag pit defect on the surface of the casting billet, including the following aspects:

[0058] (1) Improve water quality. Standardize the turbidity, Ca, and oil content of the secondary cooling water for continuous casting. The turbidity of the water is required to be ≤20mg / L, Ca≤210mg / L, and oil≤2mg / L. By standardizing and improving the water quality, the cooling and heat transfer problems can be effectively solved.

[0059] (2) Optimize the fan-shaped two-stage roller and eliminate the inner arc roller. Comparative tests show that eliminating the inner arc roller has no effect on the internal quality of the ingot. Eliminating the fan-shaped two-stage inner arc roller can "cure" the slag sticking to the inner arc roller.

[0060] (3) The fan-shaped two-stage outer arc roller is modified to add external cooling water. The cooling water cools the outer arc roller to reduce the roller temperature and improve the roller slag sticking. At the same time, it plays a role in flushing the slag stuck on the roller to prevent the slag from sticking to the ingot.

[0061] (4) Fourth, standardize the roller maintenance and offline requirements. The online rollers must be free of cracks, surfacing marks, and roller surface roughness Ra 2.0. Improving the roller surface quality can improve the "slag" hanging on the roller surface.

[0062] Through the improvements in the above aspects, the "slag pit" defects of the casting machine's ingots have been significantly reduced, and the "slag pit" defects of the ingots have been fundamentally improved.

[0063] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for solving the slag pit defect on the surface of the casting billet, characterized in that: It includes: The slag pit defect on the surface of the ingot is solved by improving the slag sticking to the fan-shaped second-stage roller.

2. The method according to claim 1, characterized in that The following steps are involved: Firstly, the composition of the "slag" at the slag pit defect position on the ingot surface was analyzed, and it was determined that the composition of the "slag" was a mixture of protective slag and iron oxide. It was determined that the "slag pit" defect on the ingot surface was related to the pressure of "iron oxide scale" on the ingot surface. Moreover, through comparative analysis, it was found that the "slag pit" defect had no direct relationship with the protective slag and steel type, but was related to the casting machine. Then, the cause of the slag pit defect on the ingot surface was found out through on-site full-process tracking, and the slag pit defect on the ingot surface was solved by improving the slag sticking on the fan-shaped second-stage roller.

3. The method according to claim 1 or 2, characterized in that: By improving the water quality and ensuring the heat transfer effect of cooling water, the residue sticking to the fan-shaped second-stage roller can be reduced.

4. The method according to claim 3, characterized in that Methods to improve water quality include: standardizing the turbidity, Ca content, and oil content of the secondary cooling water of continuous casting, requiring the water turbidity to be ≤20mg / L, Ca ≤210mg / L, and oil ≤2mg / L.

5. The method according to claim 1 or 2, characterized in that: The slag sticking to the second-stage fan-shaped roller can be reduced by optimizing the second-stage fan-shaped roller's inner arc.

6. The method according to claim 5, characterized in that Optimizing the fan-shaped two-stage inner arc roller includes: eliminating the fan-shaped two-stage inner arc roller and "curing" the roller slag sticking.

7. The method according to claim 1, characterized in that By modifying the second-stage fan-shaped outer arc roller and adding external cooling water, the residue sticking to the second-stage fan-shaped roller can be reduced.

8. The method according to claim 7, characterized in that The modification of the fan-shaped second-stage outer arc roller to add external cooling water includes: adding an external cooling water system at the fan-shaped second-stage outer arc roller. During production, cooling water is sprayed to the outer arc roller through the external cooling water system. The cooling water cools the outer arc roller to reduce the roller temperature and improve the roller slag sticking. At the same time, the slag sticking on the roller is washed to prevent the slag from sticking to the casting.

9. The method according to claim 1, characterized in that: By standardizing the maintenance and offline requirements of the second-stage fan-shaped roller, the residue sticking to the second-stage fan-shaped roller can be reduced.

10. The method according to claim 9, characterized in that Standardized maintenance and offline requirements for sector-shaped two-stage rollers include: requiring the online rollers to be free of cracks, surfacing marks, and roller surface roughness Ra 2.0.