Method for preparing hard carbon negative electrode material for sodium battery based on wood-plastic waste material

By pre-carbonizing, high-temperature carbonizing and washing the wood-plastic waste materials, the problem of unstable hard carbon performance caused by differences in biomass raw materials was solved, and efficient and low-cost preparation of hard carbon anode materials for sodium power was achieved, improving the material quality. Coulombic efficiency and reversible specific capacity.

CN118833801APending Publication Date: 2024-10-25ENERGY RES INST CO LTD HENAN ACADEMY OF SCI +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411217207.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Differences in biomass raw materials lead to unstable performance of hard carbon, affecting its reliability and efficiency in industrial applications.

Method used

Wood plastic waste materials are used for pre-carbonization and high-temperature carbonization, combined with acid washing and alkali washing steps, to optimize the process to obtain stable hard carbon anode materials for sodium electricity, and improve the uniformity and performance of the material through inert gas protection and ultrasonic dispersion.

Benefits of technology

It achieves efficient utilization of waste materials, reduces costs and energy consumption, improves the first Coulomb efficiency and reversible specific capacity of hard carbon anode materials, and solves the problem of unstable performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005021878330000061
    Figure BDA0005021878330000061
  • Figure HDA0005021878340000011
    Figure HDA0005021878340000011
  • Figure HDA0005021878340000012
    Figure HDA0005021878340000012
Patent Text Reader

Abstract

The invention belongs to the technical field of a hard carbon negative electrode material for a sodium battery, and particularly relates to a method for preparing a hard carbon negative electrode material for a sodium battery based on a wood-plastic waste material. The method comprises the following steps: carrying out pre-carbonization treatment on a wood-plastic waste material to obtain pre-carbon powder, carrying out high-temperature carbonization treatment to obtain carbon powder, sequentially carrying out acid washing, alkali washing and secondary acid washing on the carbon powder, treating to be neutral, and drying to obtain the hard carbon negative electrode material for the sodium battery. According to the preparation method of the hard carbon negative electrode material for the sodium battery based on the wood-plastic waste material, the waste material is fully utilized, the preparation method is optimized according to the condition of the raw material, and the preparation method is simple to operate, environment-friendly, low in energy consumption and suitable for industrial production. And meanwhile, the prepared hard carbon negative electrode material for the sodium battery has relatively high initial coulombic efficiency and reversible specific capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hard carbon negative electrode materials for sodium electricity, and in particular relates to a method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials. Background Art

[0002] Hard carbon is known as an amorphous carbon material that is difficult to graphitize. This type of carbon is also difficult to graphitize at high temperatures above 2500°C. Hard carbon has a larger interlayer spacing than graphite and a stronger sodium storage capacity, resulting in a higher reversible specific capacity. The volume expansion caused by the embedding of sodium ions is small, which effectively improves the safety performance of the battery. At the same time, it shows good structural stability during the charge and discharge process, which is conducive to extending the cycle life of the battery. The preparation precursors of hard carbon materials are diverse, including asphalt-based, phenolic resin-based and biomass-based. Using composite materials such as asphalt and coal tar as precursors, hard carbon materials are prepared through processes such as pyrolysis. This method has low cost, but the process technology and product capacity need to be improved. Using chemicals such as phenolic resin as precursors, the hard carbon products obtained have good uniformity and high purity, but the cost is high and industrialization is difficult. Biomass is the only renewable resource containing carbon. It has the advantages of wide sources, low prices and environmental friendliness, and has high economic benefits. However, the differences in biomass raw materials lead to unstable performance of hard carbon, which is one of the problems that need to be solved in the current industrial application process. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials, which can solve the problem of unstable hard carbon performance caused by differences in biomass raw materials. At the same time, the wood-plastic waste materials are fully utilized. The material obtained by the present invention obtains a very good first coulomb efficiency and rate performance.

[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0005] A method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials, comprising: pre-carbonizing the wood-plastic waste materials to obtain pre-carbon powder, then subjecting the pre-carbonizing materials to high-temperature carbonization to obtain carbon powder, sequentially subjecting the carbon powder to acid washing, alkali washing, and acid washing again, then subjecting the carbon powder to treatment to neutrality and drying to obtain the hard carbon negative electrode material for sodium electricity.

[0006] Furthermore, the method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials of the present invention comprises the following steps:

[0007] 1) Cut the waste wood-plastic composite material into small sections of different lengths;

[0008] 2) placing the wood-plastic composite material of step 1) in a heating furnace protected by inert gas, performing pre-carbonization treatment at a certain heating rate at low temperature, cooling, and grinding to obtain pre-carbon powder;

[0009] 3) placing the pre-carbon powder in step 2) in an inert gas and heating it to a preset temperature in a heating furnace at a certain heating rate for high-temperature carbonization treatment, and obtaining carbon powder after cooling;

[0010] 4) The carbon powder obtained in step 3) is placed in acid solution and alkaline solution of different concentrations in turn, dispersed by ultrasonic, then stirred, washed to neutrality, filtered, and dried to obtain a hard carbon negative electrode material for sodium battery.

[0011] Preferably, the waste wood-plastic material is processed to a size less than 10 cm before being pre-carbonized.

[0012] The pre-carbonization treatment is carried out in an inert gas, with a heating rate of 5-10°C / min, a pre-carbonization treatment temperature of 200-700°C, and a duration of 60-120min.

[0013] The high-temperature carbonization treatment is carried out in an inert gas, with a heating rate of 2-6°C / min, a high-temperature carbonization treatment temperature of 1000-1600°C, and a duration of 60-180min.

[0014] The inert gas is nitrogen, argon or other gas that can provide an inert atmosphere.

[0015] The concentration of the acid or alkali solution used for pickling and alkali washing is 0.05-2 mol / L.

[0016] Furthermore, during acid washing and alkali washing, the high temperature carbon powder is placed in an acid or alkali solution, ultrasonically dispersed for 10-30 minutes, and then stirred for 12-24 hours.

[0017] The acid solution may be hydrochloric acid, nitric acid, sulfuric acid, hydrofluoric acid, etc., and the alkaline solution may be sodium hydroxide, potassium hydroxide, barium hydroxide, ammonium hydroxide, etc.

[0018] The drying is carried out at 120° C. for 60-240 minutes.

[0019] The hard carbon negative electrode material obtained by the present invention has a hard carbon particle size of 300-400 meshes, a crystal plane interlayer spacing d002 in the range of 0.3716-0.3823nm, and an ash content ratio of less than 20.66%.

[0020] The raw material waste wood-plastic material of the present invention refers to the waste raw materials formed in the preparation process of wood-plastic and the waste wood-plastic composite material generated in the use process. The components include wood powder, bamboo powder, PE, talcum powder, lubricant, compatibilizer and color powder.

[0021] The mass proportion of wood raw materials in the waste wood-plastic materials is 45-80%.

[0022] Preferably, the mass ratio of wood raw materials to plastic products in the wood-plastic waste material is 5-8:2-4, and the rest is one or more of talcum powder, lubricant, compatibilizer and color powder.

[0023] The wood raw material may be one or a mixture of wood powder, bamboo powder, straw of various crops, etc.

[0024] Since the raw materials used in the present invention are waste wood-plastic materials, the composition is relatively complex and variable. Under the premise that the hard carbon performance is unstable when only biomass is used as raw material, how to make full use of the waste raw materials and solve the problems caused by the difference in raw materials to obtain a hard carbon negative electrode material with relatively stable performance is the innovation of the present invention.

[0025] The present invention further provides a method for preparing a hard carbon negative electrode sheet for sodium power generation, comprising grinding and stirring a hard carbon negative electrode material, a conductive agent and an adhesive in a certain mass ratio to form an electrode slurry, coating the electrode slurry on a copper foil, and drying the slurry at 100-120°C for 5-6 hours to obtain a hard carbon negative electrode sheet for sodium power generation; cutting the sheet into 12 mm discs, and assembling the CR2032 button battery in a glove box with an oxygen content and a water content both lower than 0.1 ppm, combining the positive electrode, a diaphragm and an electrolyte.

[0026] Compared with the prior art, the advantages of the present invention are:

[0027] The invention discloses a method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials. The raw materials fully utilize the waste materials, and the preparation method is optimized according to the conditions of the raw materials. The method is simple to operate, environmentally friendly, and has low energy consumption. At the same time, the prepared hard carbon negative electrode material for sodium electricity has a high first coulombic efficiency and reversible specific capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 TG graphs of the hard carbon materials obtained in Example 1 and Comparative Examples 1-2;

[0029] Figure 2 The XRD test results of the hard carbon materials obtained in Examples 2 and 3 are shown;

[0030] Figure 3 The charge and discharge curves of the hard carbon materials obtained in Examples 1-3 and Comparative Examples 1-2 are shown. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is described below with specific embodiments, but the protection scope of the present invention is not limited thereto:

[0032] Example 1

[0033] The hard carbon precursor wood-plastic waste material (the content of wood powder + bamboo powder is 60%) is placed in a muffle furnace in a nitrogen atmosphere, the temperature of the muffle furnace is increased to 500°C at 5°C / min, kept warm for 90 minutes, taken out after cooling, and ground to obtain pre-carbon powder; the pre-carbon powder is placed in a muffle furnace in a nitrogen atmosphere, the temperature is increased to 1600°C at 5°C / min, kept warm for 90 minutes, and taken out after cooling; the obtained sample is placed in a 0.5mol / L hydrochloric acid solution, ultrasonically dispersed, and stirred and washed overnight; after washing with clean water until neutral, 0.5mol / L sodium hydroxide solution is added, ultrasonically dispersed, and stirred and washed overnight; after washing with clean water until neutral, 0.5mol / L hydrochloric acid solution is added, ultrasonically dispersed, and stirred and washed overnight, after washing with clean water until neutral, drying is performed to obtain a hard carbon material, recorded as MS-500-1600-acid and alkali washing.

[0034] Example 2

[0035] The pre-carbonization process is consistent with that in Example 1;

[0036] The pre-carbon powder was further calcined at 1400° C. The remaining operations were consistent with those in Example 1. The obtained hard carbon material was recorded as MS-500-1400-acid-base washing.

[0037] Example 3

[0038] The pre-carbonization process is consistent with that in Example 1;

[0039] The pre-carbon powder was further calcined at 1200° C. The remaining operations were consistent with those in Example 1. The obtained hard carbon material was recorded as MS-500-1200-acid-base washing.

[0040] Comparative Example 1

[0041] The same hard carbon precursor wood-plastic waste material as in Example 1 was placed in a muffle furnace in a nitrogen atmosphere, the temperature of the muffle furnace was raised to 500° C. at 5° C. / min, kept at that temperature for 90 min, taken out after cooling, and ground to obtain pre-carbon powder;

[0042] The pre-carbon powder was placed in a muffle furnace in a nitrogen atmosphere, heated to 1600°C at 5°C / min, kept at this temperature for 90 minutes, and taken out after cooling to obtain a hard carbon material, which was recorded as MS-500-1600.

[0043] Comparative Example 2

[0044] The hard carbon precursor wood plastic was placed in a muffle furnace in a nitrogen atmosphere, heated to 1600°C at 5°C / min, kept warm for 90 minutes, and taken out after cooling to obtain a hard carbon material, which was recorded as MS-1600.

[0045] Comparative Example 3

[0046] The hard carbon precursor wood-plastic waste material is placed in a muffle furnace in a nitrogen atmosphere, the temperature of the muffle furnace is increased to 500°C at 5°C / min, kept warm for 90 minutes, taken out after cooling, and ground; the obtained sample is placed in a 0.5mol / L hydrochloric acid solution, ultrasonically dispersed, stirred and washed overnight; after washing with clean water until neutral, 0.5mol / L sodium hydroxide solution is added, ultrasonically dispersed, and stirred and washed overnight; after washing with clean water until neutral, 0.5mol / L hydrochloric acid solution is added, ultrasonically dispersed, stirred and washed overnight, washed with clean water until neutral, and dried to obtain pre-carbon powder; the pre-carbon powder is placed in a muffle furnace in a nitrogen atmosphere, the temperature is increased to 1400°C at 5°C / min, kept warm for 90 minutes, taken out after cooling, and a hard carbon material is obtained, which is recorded as MS-500-acid-base washing-1400.

[0047] Comparative Example 4

[0048] The hard carbon precursor wood-plastic waste material is placed in a muffle furnace in a nitrogen atmosphere, the temperature of the muffle furnace is raised to 500°C at 5°C / min, kept at this temperature for 90 minutes, taken out after cooling, and ground to obtain pre-carbon powder;

[0049] The pre-carbon powder was placed in a muffle furnace in a nitrogen atmosphere, heated to 1400°C at 5°C / min, kept at that temperature for 90 minutes, and taken out after cooling to obtain a hard carbon material, which was recorded as MS-500-1400.

[0050] Comparative Example 5

[0051] The hard carbon precursor wood plastic was placed in a muffle furnace in a nitrogen atmosphere, heated to 1400°C at 5°C / min, kept at this temperature for 90 min, and taken out after cooling to obtain a hard carbon material, which was recorded as MS-1400.

[0052] The hard carbon negative electrode material, conductive agent Super B and adhesive PVDF of the embodiment and the comparative example are ground, stirred and mixed in a mass ratio of 8:1:1 to form an electrode slurry, which is coated on a copper foil and dried at 100-120°C for 5-6h to obtain a hard carbon negative electrode plate for sodium electricity; the plate is cut into 12mm discs, and in a glove box with an oxygen content and a water content of less than 0.1ppm, a positive electrode, a diaphragm and an electrolyte are combined to assemble a CR2032 button battery. If the proportion of hard carbon negative electrode material in hard carbon negative electrode material, conductive agent Super B and adhesive PVDF is increased, the corresponding reversible specific capacity and the first coulomb efficiency will be improved.

[0053] The following Table 1 lists the basic reaction conditions and measurement results used in Examples 1-3 and Comparative Examples 1-5.

[0054] Table 1

[0055]

Claims

1. A method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials, characterized in that: The wood-plastic waste material is pre-carbonized to obtain pre-carbon powder, and then subjected to high-temperature carbonization to obtain carbon powder. The carbon powder is sequentially acid-washed, alkaline-washed, and acid-washed again, and then treated to neutrality and dried to obtain a hard carbon negative electrode material for sodium electricity.

2. The method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials according to claim 1, characterized in that: The pre-carbonization treatment is carried out in an inert gas, with a heating rate of 5-10°C / min, a pre-carbonization treatment temperature of 200-700°C, and a duration of 60-120min.

3. The method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials according to claim 1, characterized in that: The high-temperature carbonization treatment is carried out in an inert gas, with a heating rate of 2-6°C / min, a high-temperature carbonization treatment temperature of 1000-1600°C, and a duration of 60-180min.

4. The method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials according to claim 2 or 3, characterized in that: The inert gas is nitrogen or argon.

5. The method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials according to claim 1, characterized in that: The concentration of the acid or alkali solution used for pickling and alkali washing is 0.05-2 mol / L.

6. The method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials according to claim 5, characterized in that: During acid washing and alkali washing, the high temperature carbon powder is placed in an acid or alkali solution, ultrasonically dispersed for 10-30 minutes, and then stirred for 12-24 hours.

7. The method for preparing a sodium-based hard carbon negative electrode material based on wood-plastic waste materials according to claim 1, characterized in that: The drying is carried out at 120° C. for 60-240 minutes.

8. The method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials according to claim 1, characterized in that: The wood-plastic waste materials are processed to a size less than 10 cm and then pre-carbonized.

9. The method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials according to claim 8, characterized in that: The mass proportion of wood raw materials in the wood-plastic waste material is 45-80%.

10. The method for preparing a hard carbon negative electrode material for sodium electricity based on wood-plastic waste materials according to claim 9, characterized in that: The mass ratio of wood raw materials to plastic products in the wood-plastic waste materials is 5-8:2-4.

Citation Information

Patent Citations

  • Method for recycling polyvinyl chloride wood-plastic composites waste

    CN104211041A

  • Flaky sodium battery negative electrode carbon electrode material and preparation method thereof

    CN106450317A

  • Porous carbon nanomaterial and preparation method thereof

    CN113277509A

  • Sodium-ion battery carbon negative electrode material prepared based on waste wood chips and preparation method thereof

    CN113651307A

  • Biomass / resin composite derived hard carbon material as well as preparation method and application thereof

    CN117623272A