Production process of sub-nano high-purity ceramic powder

By optimizing the raw material pretreatment and sintering process, combined with ultra-fine grinding and chemical reactions, the problems of particle size control, purity and specific surface area in traditional ceramic powder production are solved, and high-efficiency, low-energy consumption production of sub-nanometer high-purity ceramic powder is achieved. , suitable for high-performance ceramics and electronic materials.

CN118834072APending Publication Date: 2024-10-25HENAN JIANGDI NEW MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410840927.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Traditional ceramic powder production technology is difficult to effectively control particle size distribution, achieve high purity, achieve high specific surface area and reduce energy consumption, and the process complexity is high, which limits the use of ceramic powder in high-performance applications.

Method used

By optimizing the raw material pretreatment, sintering process and grinding process, high-purity quartz, carbon and salt are selected as the main raw materials, high-purity alumina or magnesium oxide is added as secondary dopants, ultrasonic cleaning and microwave-assisted chemical vapor deposition are carried out, and high temperature is used Sintering and ultra-fine grinding, combined with chemical reactions and cleaning steps, form sub-nanometer high-purity ceramic powder.

Benefits of technology

Ceramic powder with extremely fine particle size and high specific surface area is achieved, which improves chemical and physical activity, reduces energy consumption and production costs, simplifies the process flow, and is suitable for high-performance ceramics, electronics and biomedical materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118834072A_ABST
    Figure CN118834072A_ABST
Patent Text Reader

Abstract

The invention discloses a sub-nano high-purity ceramic powder production process, and particularly relates to the technical field of sub-nano high-purity ceramic powder production, and the sub-nano high-purity ceramic powder production process comprises the steps of S1, raw material selection and pretreatment, S2, high-temperature sintering and crystal synthesis, S3, ultrafine grinding and doping, S4, chemical reaction and cleaning, and S5, drying and packaging. The ceramic powder disclosed by the invention has extremely fine particle size, high specific surface area and relatively high purity, can show relatively high chemical and physical activity, and has a good effect when being applied to the fields of semiconductor material substrates, invisible material coatings and semiconductor material crystal supports.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sub-nanometer high-purity ceramic powder production, and more specifically, to a sub-nanometer high-purity ceramic powder production process. Background Art

[0002] Ceramic materials are widely used in electronics, aviation, biomedicine and other fields due to their excellent mechanical properties, high temperature resistance and corrosion resistance. Especially in the production of high-performance ceramic products, the performance requirements of raw material powders are extremely high, including parameters such as particle size, purity and specific surface area.

[0003] Traditional ceramic powder production technology mainly relies on solid phase reaction method, wet chemical method, etc. These methods have some limitations in producing sub-nanometer high-purity ceramic powder;

[0004] 1. Particle size control: Traditional processes often have difficulty in effectively controlling the particle size distribution of powders, especially at the sub-nanometer level, which limits the use of powders in high-performance applications;

[0005] 2. Purity problem: During the production process, due to the limitations of raw materials and processes, it is difficult to achieve extremely high purity requirements, which affects the performance and application range of the final product;

[0006] 3. Specific surface area limitation: Traditional production methods usually have difficulty in achieving high specific surface area while maintaining high purity, which is a disadvantage for applications requiring high surface activity;

[0007] 4. Energy consumption and efficiency: Some traditional processes require high temperature and long time sintering, resulting in high energy consumption, low production efficiency, and possible environmental pollution;

[0008] 5. Process complexity: Some methods for producing sub-nano ceramic powders involve complex process steps, which increases production costs and reduces the market competitiveness of the products.

[0009] In view of the above problems, the present invention provides a production process for sub-nanometer high-purity ceramic powder, which effectively overcomes the shortcomings of the prior art by optimizing raw material pretreatment, sintering process and grinding process. Summary of the invention

[0010] In order to overcome the above-mentioned defects of the prior art, the present invention provides a sub-nanometer high-purity ceramic powder production process to solve the problems raised in the above-mentioned background technology.

[0011] To achieve the above object, the present invention provides the following technical solution: a sub-nanometer high-purity ceramic powder production process, the production process specifically comprising the following steps:

[0012] S1. Raw material selection and pretreatment: high-purity quartz, high-purity carbon and high-purity salt with a purity of 99.99% are selected as the main raw materials, and high-purity alumina or high-purity magnesium oxide is introduced as a secondary dopant. The raw materials are ultrasonically cleaned to remove dust and attachments on the surface of the raw materials, as well as some trace impurities, and microwave-assisted chemical vapor deposition treatment is performed to form a thin protective film on the surface of the raw materials;

[0013] S2, high temperature sintering and crystal synthesis, high purity quartz, high purity carbon and high purity salt are mixed in proportion, high purity alumina or high purity magnesium oxide secondary dopant is added to mix evenly, the mixed raw materials are placed in a high temperature sintering furnace, boric acid or lithium carbonate is added as a sintering aid, and sintered at 2000-2500°C in an oxygen-free environment to form green silicon carbide crystals;

[0014] S3, ultrafine grinding and doping, using a planetary ball mill as grinding equipment, using zirconium oxide and high-purity silicon carbide as grinding media to grind green silicon carbide crystals for 300-400 hours, while introducing boron and phosphorus as trace and multi-element dopants:

[0015] S4, chemical reaction and cleaning, put the ground slurry into the reactor, add sulfuric acid, nitric acid and hydrofluoric acid below 20PPM in turn, heat to 200℃, react for 24h, then put into the stirring tank and use cleaning agent to wash the acid to pH7;

[0016] Put the washed slurry into the reactor, add 20PPM hydrochloric acid, react for 24 hours, put it into the stirring tank, and wash it with 6PPM ultrapure water to pH 4-5;

[0017] S5, drying and packaging, the slurry is placed in a low-temperature drying oven at 80-100°C for drying, and then crushed and packaged.

[0018] Preferably, in S2, the mixing ratio of high-purity quartz, high-purity carbon and high-purity salt is 1:1:0.5, and high-purity alumina or high-purity magnesium oxide accounts for 0.5%-2% of the total raw materials.

[0019] Preferably, in S2, the sintering agent accounts for 0.5-1% of the total raw materials, and during the sintering process, a mixed atmosphere of argon and hydrogen is continuously introduced, wherein the volume ratio of hydrogen is 5%-10%.

[0020] Preferably, in S3, the added amount of boron and phosphorus is 0.1%-0.5% of the total raw materials.

[0021] Preferably, in S4, the chemical reaction is carried out in three stages;

[0022] In the first stage, sulfuric acid is used to react to remove specific impurities in the raw materials or to pre-treat the raw materials;

[0023] In the second stage, nitric acid is used to react, and nitric acid uses its strong oxidizing property to further purify the raw materials;

[0024] In the third stage, hydrofluoric acid is used to react and optimize the purity and internal structure of the raw materials;

[0025] The cleaning agent is a mixture of ethanol and water in a ratio of 0.5:1.

[0026] Preferably, the median particle size of the sub-nanometer high-purity ceramic powder is D500.3-0.5um, D90≧0.15um, D10≦0.7um, D100≦1um, and the specific surface area is 13m 2 / g-20m 2 / g.

[0027] Preferably, the sub-nanometer high-purity ceramic powder is used for semiconductor material substrates, stealth material coatings and semiconductor material crystal holders.

[0028] Technical effects and advantages of the present invention:

[0029] 1. The production process of the present invention can produce sub-nano ceramic powder with extremely fine particle size and high specific surface area, which can show higher chemical and physical activity, and can provide better mechanical strength and reaction efficiency in the fields of high-performance ceramics, electronic components and biomedical materials. At the same time, by adopting the steps of raw material pretreatment and sintering, the purity of the ceramic powder is greatly improved, so that the ceramic powder has a good application effect in semiconductor production and high-end electronic products, and can significantly improve the reliability and performance of the final product;

[0030] 2. The sintering process of the present invention optimizes energy consumption and reduces energy consumption by precisely controlling the sintering temperature and atmosphere while maintaining high product quality. This not only reduces production costs, but also meets current sustainable development and environmental protection requirements. At the same time, the process flow is simple, reduces unnecessary processes, and improves production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is the overall flow chart of the present invention. DETAILED DESCRIPTION

[0032] Embodiment 1,

[0033] This embodiment provides a sub-nanometer high-purity ceramic powder production process, which specifically includes the following steps:

[0034] S1. Raw material selection and pretreatment: high-purity quartz, high-purity carbon and high-purity salt with a purity of 99.99% are selected as the main raw materials, and high-purity alumina or high-purity magnesium oxide is introduced as a secondary dopant. The raw materials are ultrasonically cleaned to remove dust and attachments on the surface of the raw materials, as well as some trace impurities, and microwave-assisted chemical vapor deposition treatment is performed to form a thin protective film on the surface of the raw materials;

[0035] In this step, high-purity quartz is used as a silicon source to ensure that there is no impurity contamination, high-purity carbon is used as a carbon source to ensure the purity of the reaction, and high-purity salt is used as a main dopant to improve the performance of the product. According to specific needs, high-purity aluminum oxide or high-purity magnesium oxide can be selected as a secondary dopant, which can adjust the performance of the ceramic powder at the molecular level, such as improving its mechanical strength, improving thermal conductivity or optimizing electrical properties, thereby improving the thermal conductivity and electrical insulation properties of the product;

[0036] Ultrasonic cleaning is used to remove dust, attachments and some trace impurities on the surface of the raw materials to avoid defects during high-temperature sintering and affect the performance of the final product;

[0037] Microwave-assisted chemical vapor deposition forms a thin protective film on the surface of the raw material, which can prevent the raw material from being contaminated again during subsequent processing and may also help prevent excessive oxidation or impurity diffusion during high-temperature sintering.

[0038] S2, high temperature sintering and crystal synthesis, high purity quartz, high purity carbon and high purity salt are mixed in a ratio of 1:1:0.5, 1.2% of the total raw materials are added as a secondary dopant of high purity aluminum oxide or high purity magnesium oxide to mix evenly, the mixed raw materials are placed in a high temperature sintering furnace, 0.8% of the total raw materials are added as boric acid or lithium carbonate as a sintering aid, and sintered at 2200°C in an oxygen-free environment to form green silicon carbide crystals, and during the sintering process, a mixed atmosphere of argon and hydrogen is continuously introduced, wherein the volume ratio of hydrogen is 8%;

[0039] Specifically, in this step, on the basis of S1, during the process of mixing high-purity quartz, high-purity carbon, high-purity salt and secondary dopants and sintering, boric acid or lithium carbonate is introduced as a sintering aid, which helps to lower the melting point during high-temperature sintering and promote the growth of green silicon carbide crystals, thereby improving the density and mechanical properties of the sintered body. In addition, the introduction of a mixed atmosphere of argon and hydrogen helps prevent the raw materials from reacting with oxygen at high temperatures. At the same time, hydrogen may help remove impurities or promote crystal growth.

[0040] S3, ultrafine grinding and doping, using a planetary ball mill as the grinding equipment, using zirconium oxide and high-purity silicon carbide as grinding media to grind the green silicon carbide crystal for 350 hours, and at the same time introducing 0.2% of the total raw material boron and phosphorus as trace and multi-element dopants;

[0041] Specifically, in this step, the planetary ball mill can grind the above-mentioned original material to nanometer-scale particle size, and zirconium oxide and high-purity silicon carbide are selected as grinding media, which have high hardness and good wear resistance, and can effectively grind green silicon carbide crystals with higher hardness, while reducing the wear of the grinding medium itself and avoiding the introduction of unnecessary impurities. Finally, boron and phosphorus are introduced as trace and multi-element dopants to adjust the electrical properties, mechanical properties or other physical and chemical properties of the ceramic powder to meet specific application requirements.

[0042] S4, chemical reaction and cleaning, the ground slurry is placed in a reactor, sulfuric acid below 20PPM is added for preliminary reaction, nitric acid is added for reaction, and finally hydrofluoric acid is added for reaction, wherein the temperature is 200°C, the reaction time is 24h, and the slurry is placed in a stirring tank and washed with a mixed cleaning agent of ethanol and water in a ratio of 0.5:1 to a pH of 7;

[0043] Put the washed slurry into the reactor, add 20PPM hydrochloric acid, react for 24 hours, put it into the stirring tank, and wash it with 6PPM ultrapure water to pH 4-5;

[0044] Specifically, in this step, the ground raw material undergoes a three-stage reaction operation, wherein the first stage uses sulfuric acid for a preliminary reaction to remove specific impurities in the raw material or pre-treat the raw material, the second stage uses nitric acid for a reaction to further purify the raw material using its strong oxidizing property, and the third stage uses hydrofluoric acid for a reaction to optimize the purity and internal structure of the raw material;

[0045] Finally, pickling and washing steps are adopted to make the pH value of the raw material 4-5 to ensure the stability and safety of the product in subsequent processing and use.

[0046] S5, drying and packaging, the slurry is placed in a low-temperature drying box at 95°C for drying, and then crushed and packaged to obtain sub-nanometer high-purity ceramic powder. Vacuum low-temperature drying technology is used to reduce the material performance degradation that may be caused by high temperature.

[0047] Finally, the obtained sub-nanometer high-purity ceramic powder has a median particle size of D50 of 0.3um, D90 of 0.2um, D10 of 0.5um, D100 of 0.8um, and a specific surface area of ​​15m 2 / g, suitable for semiconductor material substrates, invisible material coatings and semiconductor material crystal trays.

[0048] Embodiment 2,

[0049] This embodiment provides a sub-nanometer high-purity ceramic powder production process, which specifically includes the following steps:

[0050] S1. Raw material selection and pretreatment: high-purity quartz, high-purity carbon and high-purity salt with a purity of 99.99% are selected as the main raw materials, and high-purity alumina or high-purity magnesium oxide is introduced as a secondary dopant. The raw materials are ultrasonically cleaned to remove dust and attachments on the surface of the raw materials, as well as some trace impurities, and microwave-assisted chemical vapor deposition treatment is performed to form a thin protective film on the surface of the raw materials;

[0051] S2, high temperature sintering and crystal synthesis, high purity quartz, high purity carbon and high purity salt are mixed in a ratio of 1:1:0.5, 0.8% of the total raw materials are added as a secondary dopant of high purity aluminum oxide or high purity magnesium oxide to mix evenly, the mixed raw materials are placed in a high temperature sintering furnace, 0.5% of the total raw materials are added as boric acid or lithium carbonate as a sintering aid, and sintered at 2400°C in an oxygen-free environment to form green silicon carbide crystals, and during the sintering process, a mixed atmosphere of argon and hydrogen is continuously introduced, wherein the volume ratio of hydrogen is 5%;

[0052] S3, ultrafine grinding and doping, using a planetary ball mill as the grinding equipment, using zirconium oxide and high-purity silicon carbide as grinding media to grind the green silicon carbide crystal for 380 hours, and at the same time introducing 0.3% of the total raw material boron and phosphorus as trace and multi-element dopants;

[0053] S4, chemical reaction and cleaning, the ground slurry is placed in a reactor, sulfuric acid below 20PPM is added for preliminary reaction, nitric acid is added for reaction, and finally hydrofluoric acid is added for reaction, wherein the temperature is 200°C, the reaction time is 24h, and the slurry is placed in a stirring tank and washed with a mixed cleaning agent of ethanol and water in a ratio of 0.5:1 to a pH of 7;

[0054] Put the washed slurry into the reactor, add 20PPM hydrochloric acid, react for 24 hours, put it into the stirring tank, and wash it with 6PPM ultrapure water to pH 4-5;

[0055] S5, drying and packaging, the slurry is placed in a low-temperature drying box at 80°C for drying, and then crushed and packaged to obtain sub-nanometer high-purity ceramic powder. Vacuum low-temperature drying technology is used to reduce the degradation of material properties that may be caused by high temperature.

[0056] Finally, the obtained sub-nanometer high-purity ceramic powder has a median particle size of D50 of 0.42um, D90 of 0.18um, D10 of 0.42um, D100 of 0.76um, and a specific surface area of ​​18m 2 / g, suitable for semiconductor material substrates, invisible material coatings and semiconductor material crystal trays.

[0057] Embodiment 3,

[0058] This embodiment provides a sub-nanometer high-purity ceramic powder production process, which specifically includes the following steps:

[0059] S1. Raw material selection and pretreatment: high-purity quartz, high-purity carbon and high-purity salt with a purity of 99.99% are selected as the main raw materials, and high-purity alumina or high-purity magnesium oxide is introduced as a secondary dopant. The raw materials are ultrasonically cleaned to remove dust and attachments on the surface of the raw materials, as well as some trace impurities, and microwave-assisted chemical vapor deposition treatment is performed to form a thin protective film on the surface of the raw materials;

[0060] S2, high temperature sintering and crystal synthesis, high purity quartz, high purity carbon and high purity salt are mixed in a ratio of 1:1:0.5, 1.2% of the total raw materials are added as a secondary dopant of high purity aluminum oxide or high purity magnesium oxide to mix evenly, the mixed raw materials are placed in a high temperature sintering furnace, 0.7% of the total raw materials are added as boric acid or lithium carbonate as a sintering aid, and sintered at 2500°C in an oxygen-free environment to form green silicon carbide crystals, and during the sintering process, a mixed atmosphere of argon and hydrogen is continuously introduced, wherein the volume ratio of hydrogen is 6%;

[0061] S3, ultrafine grinding and doping, using a planetary ball mill as grinding equipment, selecting zirconium oxide and high-purity silicon carbide as grinding media to grind green silicon carbide crystals for 400 hours, while introducing 0.4% of the total raw materials of boron and phosphorus as trace and multi-element dopants;

[0062] S4, chemical reaction and cleaning, the ground slurry is placed in a reactor, sulfuric acid below 20PPM is added for preliminary reaction, nitric acid is added for reaction, and finally hydrofluoric acid is added for reaction, wherein the temperature is 200°C, the reaction time is 24h, and the slurry is placed in a stirring tank and washed with a mixed cleaning agent of ethanol and water in a ratio of 0.5:1 to a pH of 7;

[0063] Put the washed slurry into the reactor, add 20PPM hydrochloric acid, react for 24 hours, put it into the stirring tank, and wash it with 6PPM ultrapure water to pH 4-5;

[0064] S5, drying and packaging, the slurry is placed in a low-temperature drying box at 85°C for drying, and then crushed and packaged to obtain sub-nanometer high-purity ceramic powder. Vacuum low-temperature drying technology is used to reduce the degradation of material properties that may be caused by high temperature.

[0065] Finally, the obtained sub-nanometer high-purity ceramic powder has a median particle size of D50 of 0.37um, D90 of 0.2um, D10 of 0.5um, D100 of 0.7um, and a specific surface area of ​​13m 2 / g, suitable for semiconductor material substrates, invisible material coatings and semiconductor material crystal trays.

[0066] Embodiment 4,

[0067] This embodiment provides a sub-nanometer high-purity ceramic powder production process, which specifically includes the following steps:

[0068] S1. Raw material selection and pretreatment: high-purity quartz, high-purity carbon and high-purity salt with a purity of 99.99% are selected as the main raw materials, and high-purity alumina or high-purity magnesium oxide is introduced as a secondary dopant. The raw materials are ultrasonically cleaned to remove dust and attachments on the surface of the raw materials, as well as some trace impurities, and microwave-assisted chemical vapor deposition treatment is performed to form a thin protective film on the surface of the raw materials;

[0069] S2, high temperature sintering and crystal synthesis, high purity quartz, high purity carbon and high purity salt are mixed in a ratio of 1:1:0.5, 2% of the total raw materials are added as a secondary dopant of high purity aluminum oxide or high purity magnesium oxide to mix evenly, the mixed raw materials are placed in a high temperature sintering furnace, 1% of the total raw materials are added as a sintering aid of boric acid or lithium carbonate to sinter at 2500°C in an oxygen-free environment to form green silicon carbide crystals, and during the sintering process, a mixed atmosphere of argon and hydrogen is continuously introduced, wherein the volume ratio of hydrogen is 9%;

[0070] S3, ultrafine grinding and doping, using a planetary ball mill as grinding equipment, selecting zirconium oxide and high-purity silicon carbide as grinding media to grind green silicon carbide crystals for 400 hours, while introducing 0.5% of the total raw materials of boron and phosphorus as trace and multi-element dopants;

[0071] S4, chemical reaction and cleaning, the ground slurry is placed in a reactor, sulfuric acid below 20PPM is added for preliminary reaction, nitric acid is added for reaction, and finally hydrofluoric acid is added for reaction, wherein the temperature is 200°C, the reaction time is 24h, and the slurry is placed in a stirring tank and washed with a mixed cleaning agent of ethanol and water in a ratio of 0.5:1 to a pH of 7;

[0072] Put the washed slurry into the reactor, add 20PPM hydrochloric acid, react for 24 hours, put it into the stirring tank, and wash it with 6PPM ultrapure water to pH 4-5;

[0073] S5, drying and packaging, the slurry is placed in a low-temperature drying box at 100°C for drying, and then crushed and packaged to obtain sub-nanometer high-purity ceramic powder. Vacuum low-temperature drying technology is used to reduce the material performance degradation that may be caused by high temperature.

[0074] Finally, the obtained sub-nanometer high-purity ceramic powder has a median particle size of D50 of 0.42um, D90 of 0.22um, D10 of 0.7um, D100 of 1um, and a specific surface area of ​​18m 2 / g, suitable for semiconductor material substrates, invisible material coatings and semiconductor material crystal trays.

[0075] The sub-nanometer high-purity ceramic powders prepared in the above Examples 1-4 were subjected to performance tests, and two conventional ceramic powders were used as Comparative Examples 1 and 2 (conventional process A: using a lower sintering temperature and a simple chemical cleaning process, conventional process B: using a standard ball milling method and a shorter doping time), and the results are shown in the following table:

[0076] Among them, the particle size distribution test uses a laser particle size analyzer to measure the particle size distribution of the powder;

[0077] Specific surface area test, the Brunauer-Emmett-Teller (BET) method was used to measure the specific surface area of ​​the powder;

[0078] Purity test, chemical composition of powders was analyzed by inductively coupled plasma mass spectrometry (ICP-MS);

[0079] Thermal conductivity testing, using the laser flash method to measure the thermal diffusivity of the material and then calculate the thermal conductivity;

[0080] Electrical insulation strength test, measuring the electrical insulation strength of the powder through a high voltage breakdown test.

[0081]

[0082]

[0083] According to the data in the above table:

[0084] 1. Particle size and specific surface area: Compared with the conventional process, the process of the present invention significantly reduces the particle size of the ceramic powder and significantly increases the specific surface area, which indicates that the process of the present invention can produce finer and more active powders, which helps to improve their performance in high-performance applications;

[0085] 2. Purity: The process of the present invention achieves higher product purity through optimized raw material pretreatment and sintering process, which exceeds the level of traditional processes. This is an important improvement for applications requiring extremely high purity, such as electronics and biomedicine.

[0086] 3. Thermal conductivity: The ceramic powder produced by the process of the present invention exhibits higher thermal conductivity, especially Example 4, which may be due to the optimized sintering conditions and the use of dopants, which promote more efficient heat conduction;

[0087] 4. Electrical insulation strength: The process of the present invention also performs well in electrical insulation strength, especially Example 4, whose electrical insulation strength is much higher than that of the traditional process, which makes the material have better performance and safety in the field of electrical applications.

[0088] In summary, through these comparative data, the sub-nanoscale high-purity ceramic powder production process of the present invention shows significant advantages in multiple key performance indicators, proving that it has great advantages in improving product performance and production efficiency. These advantages provide a broader space for the application of high-end ceramic powders, especially in the fields of precision devices and high-performance materials.

[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A sub-nanometer high-purity ceramic powder production process, characterized by: The production process specifically comprises the following steps: S1. Raw material selection and pretreatment: high-purity quartz, high-purity carbon and high-purity salt with a purity of 99.99% are selected as the main raw materials, and high-purity alumina or high-purity magnesium oxide is introduced as a secondary dopant. The raw materials are ultrasonically cleaned to remove dust and attachments on the surface of the raw materials, as well as some trace impurities, and microwave-assisted chemical vapor deposition treatment is performed to form a thin protective film on the surface of the raw materials; S2, high temperature sintering and crystal synthesis, high purity quartz, high purity carbon and high purity salt are mixed in proportion, high purity alumina or high purity magnesium oxide secondary dopant is added to mix evenly, the mixed raw materials are placed in a high temperature sintering furnace, boric acid or lithium carbonate is added as a sintering aid, and sintered at 2000-2500°C in an oxygen-free environment to form green silicon carbide crystals; S3, ultrafine grinding and doping, using a planetary ball mill as the grinding equipment, using zirconium oxide and high-purity silicon carbide as grinding media to grind the green silicon carbide crystal for 300-400 hours, while introducing boron and phosphorus as trace and multi-element dopants; S4, chemical reaction and cleaning, put the ground slurry into the reactor, add sulfuric acid, nitric acid and hydrofluoric acid below 20PPM in turn, heat to 200℃, react for 24h, then put into the stirring tank and use cleaning agent to wash the acid to pH7; Put the washed slurry into the reactor, add 20PPM hydrochloric acid, react for 24 hours, put it into the stirring tank, and wash it with 6PPM ultrapure water to pH 4-5; S5, drying and packaging, the slurry is placed in a low-temperature drying oven at 80-100°C for drying, and then crushed and packaged.

2. The process for producing sub-nanometer high-purity ceramic powder according to claim 1, characterized in that: In S2, the mixing ratio of high-purity quartz, high-purity carbon and high-purity salt is 1:1:0.5, and high-purity alumina or high-purity magnesium oxide accounts for 0.5%-2% of the total raw materials.

3. The process for producing sub-nanometer high-purity ceramic powder according to claim 1, characterized in that: In S2, the sintering agent accounts for 0.5-1% of the total raw materials. During the sintering process, a mixed atmosphere of argon and hydrogen is continuously introduced, wherein the volume ratio of hydrogen is 5%-10%.

4. The process for producing sub-nanometer high-purity ceramic powder according to claim 1, characterized in that: In S3, the addition amount of boron and phosphorus is 0.1%-0.5% of the total raw materials.

5. The process for producing sub-nanometer high-purity ceramic powder according to claim 1, characterized in that: In S4, the chemical reaction is carried out in three stages; In the first stage, sulfuric acid is used to react to remove specific impurities in the raw materials or to pre-treat the raw materials; The second stage uses nitric acid to react, and nitric acid uses its strong oxidizing property to further purify the raw materials; In the third stage, hydrofluoric acid is used to react and optimize the purity and internal structure of the raw materials; The cleaning agent is a mixture of ethanol and water in a ratio of 0.5:

1.

6. The process for producing sub-nanometer high-purity ceramic powder according to claim 1, characterized in that: The sub-nanometer high-purity ceramic powder has a median particle size of D500.3-0.5um, D90≧0.15um, D10≦0.7um, D100≦1um, and a specific surface area of ​​13m 2 / g-20m 2 / g.

7. The process for producing sub-nanometer high-purity ceramic powder according to claim 1, characterized in that: The sub-nanometer high-purity ceramic powder is used for semiconductor material substrates, stealth material coatings and semiconductor material crystal holders.

Citation Information

Patent Citations

  • Low-temperature sintering method of high-performance silicon carbide ceramic material

    CN117088694A

  • Method for preparing SIC micro nano ceramic powder via refinery coke salt bath synthesis

    CN1511807A

  • High purity silicon carbide articles and methods

    TW200535115A

  • Method of producing carbide raw material

    US20180087186A1

  • Heat treating apparatuses for semiconductors and high purity silicon carbide parts for the apparatuses and a method of making thereof

    US5179049A