Long-acting super-hydrophobic polyurethane sponge, preparation method of sponge and method for removing oil stains on water surface
Through silane compound treatment and in-situ polymerization technology, the hydrophobicity and mesoscopic roughness of polyurethane sponges are improved, which solves the problem of reduced hydrophobicity of polyurethane sponges after long-term use, achieves efficient oil-water separation and long-term recycling, and significantly improves water quality. and ecological environment.
Patent Information
- Application Number
- CN202410874857.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-07-02
AI Technical Summary
After long-term use of existing polyurethane sponges, the surface micro-nano composite structure is easily damaged and the hydrophobicity is reduced, resulting in a decrease in oil absorption efficiency, inability to achieve efficient oil-water separation, and poor reuse effect.
The surface energy of nano-ZnO and micron SiO2 is reduced through silane compound treatment, and they are added to the polyurethane prepolymer for in-situ polymerization to form a super-hydrophobic polyurethane sponge, which enhances the hydrophobicity and mesoscopic roughness of the sponge and extends its service life.
It achieves long-term oil and water separation of polyurethane sponge, with an adsorption capacity of 50 to 60 times its own weight. The adsorption effect remains above 95% after 100 cycles, and the separation efficiency is above 99%. The sponge can be recycled for a long time, improving water quality and ecological environment. .
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oil-water separation, and in particular relates to a long-acting super-hydrophobic polyurethane sponge, a preparation method of the sponge, and a method for removing oil stains on a water surface. Background Art
[0002] With the rapid development of modern industry, industries such as offshore oil transportation are also developing rapidly, but the frequent occurrence of oil spills and organic matter leakage accidents has caused great damage to the environment and had a serious impact on the ecological and environmental systems.
[0003] At present, the commonly used methods for removing oil pollutants from water bodies include adsorption treatment, chemical dispersion and sedimentation treatment, microbial degradation, etc. These methods have their own limitations, such as long treatment time, high production cost, low separation efficiency, and easy to produce secondary pollution. Relatively speaking, the material adsorption method is widely used in oil pollution treatment due to the material's own fast and efficient adsorption performance, recyclability, and no secondary pollution. The principle of the material adsorption method is to adsorb and store the oil in the pores of the material through capillary action, and the oil adsorbed in the pores can be recovered through external forces such as centrifugation and extrusion. However, traditional adsorption materials have poor selectivity for oil and water, and will also absorb water during the oil absorption process; the oil absorption rate for high-viscosity oil is slow and the efficiency is low, and it cannot achieve effective oil-water separation, which restricts the application of adsorption materials in oil spill emergency response.
[0004] Polyurethane sponge not only has good stability, resilience, chemical resistance and mechanical properties, but also has the advantages of high porosity, large specific surface area and interconnected pore structure when used as an adsorption material. However, ordinary polyurethane sponges lack the function of selectively absorbing oil and water, and cannot achieve efficient oil-water separation. To achieve efficient oil-water separation of polyurethane sponges, the surface of polyurethane sponges must be modified. The commonly used surface modification methods for polyurethane sponges are: first, constructing a micro-nano composite structure on the surface of polyurethane sponges to improve the mesoscopic roughness of the material, thereby increasing the contact angle of the material and enhancing the hydrophobicity, so that the polyurethane sponge has efficient oil-water separation performance; second, coating the low surface energy material on the surface of the polyurethane sponge to make the surface of the polyurethane sponge have super hydrophobic and oleophilic properties. However, after long-term use, the surface micro-nano composite structure will be destroyed, and the low surface energy material on the surface of the polyurethane sponge will also fall off, affecting the stability and hydrophobicity of the sponge, which will greatly reduce the oil absorption efficiency and the effect of repeated use is poor.
[0005] In summary, the development of an economical, long-term recyclable adsorbent material that can quickly and efficiently remove oil from water has great practical significance, but also faces many challenges. Summary of the invention
[0006] In order to overcome the deficiencies of the prior art, the first aspect of the present invention provides a long-acting super-hydrophobic polyurethane sponge and a preparation method thereof. Nano ZnO and micron SiO2 are treated with silane compounds to reduce the surface energy of nano ZnO and micron SiO2 and improve hydrophobicity; hydrophobically modified nano ZnO and hydrophobically modified micron SiO2 are added to polyurethane prepolymers and uniformly mixed, and then in-situ polymerization is performed to obtain super-hydrophobic polyurethane; and super-hydrophobic polyurethane is freely foamed in a mold to obtain a long-acting super-hydrophobic polyurethane sponge. On the one hand, the technology adopts silane compound modification treatment to reduce the surface energy of the powder, and on the other hand, nano-scale ZnO and micron-scale SiO2 are uniformly distributed in the polyurethane sponge obtained by in-situ polymerization and foaming, and a micro-nano composite structure can be formed on the surface and inside of the sponge, improving the mesoscopic roughness of the polyurethane sponge, and solving the problem that the micro-nano composite structure is easily destroyed. It is low in price, excellent in oil absorption performance and stable in performance, and can solve the problems of low separation efficiency and poor repeatability of the current oil-water separation polyurethane sponge.
[0007] The preparation method of the long-acting super-hydrophobic polyurethane sponge of the present invention comprises the following steps:
[0008] Step 1: 50-80 parts by weight of polyol, 2-3 parts by weight of water, 1-4 parts by weight of foaming agent, 0.5-1.5 parts by weight of catalyst, and 0.4-1 parts by weight of foam stabilizer are uniformly mixed at a temperature of 15-30° C. to obtain a polyurethane auxiliary material, namely component A;
[0009] Step 2: Add 50 to 75 parts by weight of polyisocyanate into a reaction container, stir at a temperature of 60 to 80° C. for 20 to 40 minutes, then add polyol at a mass ratio of polyisocyanate to polyol of 100:40 to 100:75, and react at a temperature of 60 to 80° C. to obtain a polyurethane prepolymer, i.e., component B;
[0010] Step 3: Disperse 5 to 20 parts by mass of nano ZnO in 60 to 80 parts by mass of a solvent, then dropwise mix in 1 to 3 parts by mass of a silane compound, and react at a temperature of 60 to 80° C. for 3 to 6 hours, then separate the solid, wash and dry it to obtain a hydrophobically modified ZnO powder, i.e., component C;
[0011] Step 4: 5 to 20 parts by mass of micronized SiO2 are dispersed in 60 to 80 parts by mass of a solvent, and then 1 to 3 parts by mass of a silane compound are added dropwise, and reacted at a temperature of 60 to 80°C for 3 to 6 hours, and then the solid is separated, washed and dried to obtain a hydrophobically modified SiO2 powder, i.e., component D;
[0012] Step 5: According to the mass ratio of component A: component B: component C: component D of 45-55:100: 5-20: 5-20, component A, component B, component C and component D are mixed, and an in-situ polymerization reaction is carried out to prepare a super hydrophobic polyurethane;
[0013] Step 6: Pour the super-hydrophobic polyurethane obtained in the above step 5 into a mold to carry out a free foaming reaction, and after drying, obtain a long-lasting super-hydrophobic polyurethane sponge.
[0014] Preferably, in step 3, 5 to 20 parts by mass of nano ZnO are added to 60 to 80 parts by mass of 80% ethanol aqueous solution, and then acetic acid is added dropwise until the pH value of the solution is 4. After mixing, 1 to 3 parts by mass of silane compound are added dropwise under stirring conditions, and the reaction is carried out at a temperature of 60 to 80° C. for 3 to 6 hours. The solid is then separated by centrifugation, washed with distilled water and filtered, and then the washing and filtering steps are repeated 1 to 4 times. The filtered solid is vacuum dried at 60° C. to constant weight, crushed and sieved to obtain hydrophobically modified ZnO powder, i.e., component C.
[0015] Preferably, in step 4, 5 to 20 parts by mass of nano-SiO2 are added to 60 to 80 parts by mass of 80% ethanol aqueous solution, and then acetic acid is added dropwise until the pH value of the solution is 4. After mixing, 1 to 3 parts by mass of silane compound are added dropwise under stirring conditions, and the reaction is carried out at a temperature of 60 to 80°C for 3 to 6 hours. The solid is then separated by centrifugation, washed with distilled water and filtered, and then the washing and filtration steps are repeated 1 to 4 times. The filtered solid is vacuum dried at 60°C to constant weight, crushed and sieved to obtain hydrophobically modified SiO2 powder, i.e., component D.
[0016] Preferably, in step 5, according to the mass ratio of component A: component B: component C: component D of 50:100:5-20:5-20, component A, component B, component C and component D are respectively weighed and placed in a reaction vessel, and in-situ polymerization is carried out for 10-30 minutes at a temperature of 20-40° C. and a rotation speed of 200-300 r / min to obtain a super hydrophobic polyurethane.
[0017] Preferably, in step 6, the super hydrophobic polyurethane obtained in step 5 is poured into a mold, stirred for 15 to 30 seconds at a temperature of 20 to 40°C and a rotation speed of 1000 to 1500 r / min, then poured into a mold, and subjected to free foaming reaction at 20 to 40°C for 3 to 5 minutes, and then the foamed polyurethane sponge is taken out and placed in a 60 to 80°C oven with a flow rate of 50 ml / min of flowing N2 and dried for 3 to 6 hours to obtain the long-lasting super hydrophobic polyurethane sponge.
[0018] Preferably, the polyol in step 1 and step 2 is one or more of polytetrahydrofuran diol, polycarbonate diol, polycaprolactone diol and polypropylene glycol.
[0019] Preferably, the foaming agent in step 1 is one or more of dichloromethane, 1,1,1,3,3-pentafluorobutane, 1,1,1,3,3-pentafluoropropane, 1,1,1,2-tetrafluoroethane, difluoroethane, and heptafluoropropane.
[0020] Preferably, the catalyst in step 1 is selected from an organic metal catalyst and a tertiary amine catalyst, preferably an organic metal catalyst, wherein the organic metal catalyst is one or more of dibutyltin dilaurate, distannous octoate, and dibutyltin acetate.
[0021] Preferably, the foam stabilizer in step 1 is one or more of dimethyl silicone oil, dodecyl dimethyl amine oxide, and alkyl alcohol amide.
[0022] Preferably, the polyisocyanate in step 2 is one or more of isophorone diisocyanate, hexamethylene diisocyanate, and toluene diisocyanate.
[0023] Preferably, the silane compound in step 3 is one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β (aminoethyl) -γ-aminopropyltrimethoxysilane, N-β (aminoethyl) -γ-aminopropylmethyldimethoxysilane, and N-β (aminoethyl) -γ-aminopropyltriethoxysilane.
[0024] Preferably, the particle size of the nano ZnO in step 3 is 50 to 300 nm, more preferably 100 to 200 nm.
[0025] Preferably, the micron SiO2 particle size in step 4 is 50 to 300 μm, more preferably 50 to 100 μm.
[0026] The above method can be used to prepare a long-lasting super-hydrophobic polyurethane sponge, whose water contact angle can reach 150° to 165°, and the adsorption capacity of petroleum ether, kerosene, etc. can reach 50 to 60 times its own weight. After 100 adsorption-desorption cycles, the adsorption effect of oil can still maintain more than 95% of the initial oil absorption rate, and the separation efficiency of oil / water mixture is more than 99%. It can be used to quickly adsorb oils and various organic solvents in water to achieve efficient water-oil separation. Due to the simple preparation method, strong operability, and recyclable characteristics of the oil-absorbing sponge, it is expected to be widely used in the removal of oil pollutants in water bodies, thereby greatly improving the ecological environment.
[0027] The second aspect of the present invention is to provide a method for removing oil stains on a water surface based on the above-mentioned long-acting super-hydrophobic polyurethane sponge. Specifically, a long-acting super-hydrophobic polyurethane sponge is placed in an oily wastewater area, and after the oil stains on the water surface are adsorbed by the long-acting super-hydrophobic polyurethane sponge, they are salvaged and collected, and the oil stains are separated by centrifugation or extrusion. The regenerated sponge after the oil stains are separated is put into the next round of use. This method for removing oil stains on the water surface utilizes the long-acting super-hydrophobic polyurethane sponge to efficiently adsorb oil pollutants, realize rapid separation of oil and water, and the sponge can be recycled at the same time, which helps to continuously improve water quality and ecological environment.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) In the present invention, hydrophobically modified nano ZnO and hydrophobically modified micron SiO2 are added to polyurethane prepolymer to prepare a super hydrophobic polyurethane sponge. Since the hydrophobic modification reduces the surface energy of nano ZnO and micron SiO2, the hydrophobicity is improved, so that the polyurethane sponge has super hydrophobic properties, improves the oil-water separation ability, and has excellent oil-water separation performance. The water contact angle of the prepared hydrophobic polyurethane foam ranges from 150° to 165°, and the adsorption amount of petroleum ether, kerosene, etc. can reach 50 to 60 times its own weight.
[0030] (2) In the present invention, after the hydrophobic modification of nano ZnO and hydrophobically modified micron SiO2, on the one hand, the silane compound introduced on the surface enhances the interaction with the polyurethane molecules, and on the other hand, after in-situ polymerization with the polyurethane prepolymer and free foaming, the micro-nano composite structure is evenly distributed on the surface and inside of the sponge, thereby improving the mesoscopic roughness of the polyurethane sponge. The combined result of the two prolongs the life of the hydrophobic function of the sponge. After 100 adsorption-desorption cycles, the adsorption effect on oil can still maintain more than 95% of the initial oil absorption rate, and the separation efficiency of the oil / water mixture is more than 99%.
[0031] (3) The present invention relates to a method for preparing a long-lasting super-hydrophobic polyurethane sponge for oil-water separation, which only requires the use of conventional production equipment, does not require investment in special equipment, has simple process control, low production cost, and can be easily mass-produced.
[0032] (4) The present invention also proposes a method for removing oil stains from the water surface, which utilizes the excellent oil absorption capacity, oil-water separation efficiency and durability of the long-lasting super-hydrophobic polyurethane sponge to achieve rapid separation of oil and water. At the same time, the sponge can be recycled for a long time, which helps to continuously improve water quality and the ecological environment. DETAILED DESCRIPTION
[0033] The present invention is further illustrated by specific examples below. These examples are exemplary and are intended to illustrate the problem and explain the present invention, but are not intended to be limiting.
[0034] Example 1
[0035] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0036] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0037] Step 3: Add 5g of nano ZnO and 60g of 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g of 3-aminopropyltriethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24h to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0038] Step 4: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g 3-aminopropyltriethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. Wash the modified SiO2 with distilled water, filter it 3 times, and vacuum dry it at 60°C for 24h to constant weight, crush it, and pass it through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e. component D;
[0039] Step 5: According to the mass ratio of component A: component B: component C: component D being 50:100:5:5 and the total mass being 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in sequence, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0040] Step 6: Pour the super-hydrophobic polyurethane obtained in step 5 into a mold, and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a super-hydrophobic polyurethane sponge.
[0041] Example 2
[0042] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0043] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0044] Step 3: Add 5g of nano ZnO and 60g of 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30 minutes, then add 1g of N-β (aminoethyl) -γ-aminopropyl dimethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4 hours, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20 minutes to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24 hours to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0045] Step 4: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g N-β (aminoethyl) -γ-aminopropyl dimethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. The modified SiO2 was washed with distilled water, filtered 3 times, and vacuum dried at 60°C for 24h to constant weight, crushed, and sieved through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e., component D;
[0046] Step 5: According to the mass ratio of component A: component B: component C: component D being 50:100:5:5 and the total mass being 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in sequence, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0047] Step 6: Pour the super-hydrophobic polyurethane obtained in step 5 into a mold, and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a super-hydrophobic polyurethane sponge.
[0048] Example 3
[0049] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0050] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0051] Step 3: Add 5g of nano ZnO and 60g of 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30 minutes, then add 1g of N-β (aminoethyl) -γ-aminopropyl trimethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4 hours, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20 minutes to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24 hours to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0052] Step 4: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g N-β (aminoethyl) -γ-aminopropyl trimethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. The modified SiO2 was washed with distilled water, filtered 3 times, and vacuum dried at 60°C for 24h to constant weight, crushed, and sieved through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e. component D;
[0053] Step 5: According to the mass ratio of component A: component B: component C: component D being 50:100:5:5 and the total mass being 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in sequence, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0054] Step 6: Pour the super-hydrophobic polyurethane obtained in step 5 into a mold, and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a super-hydrophobic polyurethane sponge.
[0055] Example 4
[0056] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0057] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0058] Step 3: Add 5g of nano ZnO and 60g of 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30 minutes, then add 1g of N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4 hours, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20 minutes to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24 hours to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0059] Step 4: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. The modified SiO2 was washed with distilled water, filtered 3 times, and vacuum dried at 60°C for 24h to constant weight, crushed, and sieved through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e. component D;
[0060] Step 5: According to the mass ratio of component A: component B: component C: component D being 50:100:5:5 and the total mass being 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in sequence, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0061] Step 6: Pour the super-hydrophobic polyurethane obtained in step 5 into a mold, and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a super-hydrophobic polyurethane sponge.
[0062] Example 5
[0063] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0064] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0065] Step 3: Add 5g of nano ZnO and 60g of ethanol aqueous solution in 80% ethanol aqueous solution in a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30 minutes, then add 1g of N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4 hours, pour it into a centrifuge tube and centrifuge it at a speed of 10000r / min for 20 minutes to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24 hours to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0066] Step 4: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. The modified SiO2 was washed with distilled water, filtered 3 times, and vacuum dried at 60°C for 24h to constant weight, crushed, and sieved through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e. component D;
[0067] Step 5: According to the mass ratio of component A: component B: component C: component D being 50:100:10:10 and the total mass being 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in sequence, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0068] Step 6: Pour the super-hydrophobic polyurethane obtained in step 5 into a mold, and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a super-hydrophobic polyurethane sponge.
[0069] Example 6
[0070] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0071] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0072] Step 3: Add 5g of nano ZnO and 60g of 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30 minutes, then add 1g of N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4 hours, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20 minutes to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24 hours to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0073] Step 4: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. The modified SiO2 was washed with distilled water, filtered 3 times, and vacuum dried at 60°C for 24h to constant weight, crushed, and sieved through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e. component D;
[0074] Step 5: According to the mass ratio of component A: component B: component C: component D of 50:100:15:15 and the total mass of 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in turn, and in situ polymerization was carried out at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0075] Step 6: Pour the super-hydrophobic polyurethane obtained in step 5 into a mold, and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a super-hydrophobic polyurethane sponge.
[0076] Example 7
[0077] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0078] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0079] Step 3: Add 5g of nano ZnO and 60g of 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30 minutes, then add 1g of N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4 hours, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20 minutes to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24 hours to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0080] Step 4: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. The modified SiO2 was washed with distilled water, filtered 3 times, and vacuum dried at 60°C for 24h to constant weight, crushed, and sieved through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e. component D;
[0081] Step 5: According to the mass ratio of component A: component B: component C: component D being 50:100:20:20 and the total mass being 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in sequence, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0082] Step 6: Pour the super-hydrophobic polyurethane obtained in step 5 into a mold, and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a super-hydrophobic polyurethane sponge.
[0083] Example 8
[0084] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0085] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0086] Step 3: Add 5g of nano ZnO and 60g of 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g of N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 70°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24h to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0087] Step 4: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 70°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. The modified SiO2 was washed with distilled water, filtered 3 times, and vacuum dried at 60°C for 24h to constant weight, crushed, and sieved through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e. component D;
[0088] Step 5: According to the mass ratio of component A: component B: component C: component D being 50:100:5:5 and the total mass being 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in sequence, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0089] Step 6: Pour the super-hydrophobic polyurethane obtained in step 5 into a mold, and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a super-hydrophobic polyurethane sponge.
[0090] Example 9
[0091] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0092] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0093] Step 3: Add 5g of nano ZnO and 60g of 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g of N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 80°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24h to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0094] Step 4: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 80°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. The modified SiO2 was washed with distilled water, filtered 3 times, and vacuum dried at 60°C for 24h to constant weight, crushed, and sieved through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e., component D;
[0095] Step 5: According to the mass ratio of component A: component B: component C: component D being 50:100:5:5 and the total mass being 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in sequence, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0096] Step 6: Pour the super-hydrophobic polyurethane obtained in step 5 into a mold, and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a super-hydrophobic polyurethane sponge.
[0097] Example 10
[0098] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0099] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0100] Step 3: Add 5g of nano ZnO and 60g of 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30 minutes, then add 1g of N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4 hours, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20 minutes to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24 hours to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0101] Step 4: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. The modified SiO2 was washed with distilled water, filtered 3 times, and vacuum dried at 60°C for 24h to constant weight, crushed, and sieved through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e. component D;
[0102] Step 5: According to the mass ratio of component A: component B: component C: component D being 50:100:5:5 and the total mass being 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in sequence, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0103] Step 6: Pour the super-hydrophobic polyurethane obtained in step 5 into a mold, and perform free foaming reaction at 30°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a super-hydrophobic polyurethane sponge.
[0104] Embodiment 11
[0105] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0106] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0107] Step 3: Add 5g of nano ZnO and 60g of 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30 minutes, then add 1g of N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4 hours, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20 minutes to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24 hours to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0108] Step 4: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. The modified SiO2 was washed with distilled water, filtered 3 times, and vacuum dried at 60°C for 24h to constant weight, crushed, and sieved through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e. component D;
[0109] Step 5: According to the mass ratio of component A: component B: component C: component D being 50:100:5:5 and the total mass being 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in sequence, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0110] Step 6: Pour the super-hydrophobic polyurethane obtained in step 5 into a mold, and perform free foaming reaction at 40°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a super-hydrophobic polyurethane sponge.
[0111] Comparative Example 1
[0112] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0113] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0114] Step 3: According to the mass ratio of component A: component B: nano ZnO: micron SiO2 being 50:100:5:5 and the total mass being 50 g, component A, component B, component C and component D were weighed respectively, and put into a flask in sequence, and in situ polymerization was performed at a temperature of 20° C. and a rotation speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a rotation speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0115] Step 4: Pour the superhydrophobic polyurethane obtained in step 3 into a mold and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a polyurethane sponge.
[0116] Comparative Example 2
[0117] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir for 15 min at a temperature of 25° C. and a stirring speed of 200 r / min to obtain an auxiliary material, namely component A;
[0118] Step 2: Add 50 g of isophorone diisocyanate into a three-necked flask, stir for 30 min at a temperature of 60° C. and a stirring speed of 200 r / min, then add 25 g of polytetrahydrofuran diol, and react for 3 h at a temperature of 70° C. and a stirring speed of 200 r / min to obtain a prepolymer, i.e., component B;
[0119] Step 3: Add 5g of nano ZnO and 60g of 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid until the pH value of the solution is 4. Ultrasonic treatment for 30 minutes, then add 1g of N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4 hours, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20 minutes to obtain hydrophobically modified ZnO. The modified ZnO was washed with distilled water, filtered 3 times, and vacuum dried at 70°C for 24 hours to constant weight, crushed, and sieved through a 12500 mesh sieve to obtain hydrophobically modified ZnO powder, i.e. component C;
[0120] Step 4: According to the mass ratio of component A: component B: component C being 50:100:5 and the total mass being 50 g, component A, component B and component C were weighed respectively, and put into a flask in turn, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0121] Step 5: Pour the superhydrophobic polyurethane obtained in step 4 into a mold and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a polyurethane sponge.
[0122] Comparative Example 3
[0123] Step 1: Add 25 g of polytetrahydrofuran diol, 1 g of water, 1 g of dichloromethane, 0.4 g of dibutyltin dilaurate, and 0.5 g of dimethyl silicone oil into a three-necked flask, and stir and mix them thoroughly at a temperature of 25° C., a stirring speed of 200 r / min, and a stirring time of 15 min to obtain an auxiliary material, namely component A;
[0124] Step 2: Add 50 g of isophorone diisocyanate to a three-necked flask, stir for 30 min at 60° C. and 200 r / min, then add 25 g of polytetrahydrofuran diol, heat to 70° C., and react for 3 h at 200 r / min and 30 min to obtain a prepolymer, i.e., component B;
[0125] Step 3: Add 5g micron SiO2 and 60g 80% ethanol aqueous solution into a three-necked flask, and then add acetic acid dropwise until the pH value of the solution is 4. Ultrasonic treatment for 30min, then add 1g N-β (aminoethyl) -γ-aminopropyl triethoxysilane dropwise at a stirring speed of 250r / min, and condense and reflux at a temperature of 60°C and a stirring speed of 250r / min. After reacting for 4h, pour into a centrifuge tube and centrifuge at a speed of 10000r / min for 20min to obtain hydrophobically modified SiO2. The modified SiO2 was washed with distilled water, filtered 3 times, and vacuum dried at 60°C for 24h to constant weight, crushed, and sieved through a 250-mesh sieve to obtain hydrophobically modified SiO2 powder, i.e. component C;
[0126] Step 4: According to the mass ratio of component A: component B: component C being 50:100:5 and the total mass being 50 g, component A, component B and component C were weighed respectively, and put into a flask in turn, and in situ polymerization was performed at a temperature of 20° C. and a speed of 300 r / min for 30 min, and then stirred at a temperature of 25° C. and a speed of 1200 r / min for 30 s to obtain a super hydrophobic polyurethane;
[0127] Step 5: Pour the superhydrophobic polyurethane obtained in step 4 into a mold and perform free foaming reaction at 20°C for 5 minutes. Then take out the foamed polyurethane sponge and place it in a 60°C oven with flowing N2 at a flow rate of 50 ml / min for 4 hours to obtain a polyurethane sponge.
[0128] Effect verification
[0129] In order to fully understand the performance of the modified polyurethane sponge obtained in each embodiment and comparative example, the water contact angle, adsorption capacity, and adsorption capacity after 10 cycles and 100 cycles were tested, wherein the water contact angle test was conducted in accordance with GB / T 30693-2014; the adsorption capacity test used a weighing method to study the adsorption capacity of super-hydrophobic polyurethane sponge to kerosene. Super-hydrophobic polyurethane sponges of different proportions were cut into a plurality of small cubes of 1.0cmx1.0cmx1.0cm, and the mass of the sponge itself was weighed and recorded as m0. Different sponges were immersed in a beaker containing 30mL kerosene, soaked for 24h to reach adsorption saturation, the sponge was taken out, the excess oil droplets on the surface of the sponge were drained, and its mass was detected by a weighing balance and recorded as m1, and the adsorption capacity Q of the sponge to kerosene was calculated according to the formula Q=m1 / m0. The adsorption capacity test after 10 cycles and 100 cycles is the same as the above adsorption capacity test method, and the adsorption capacity Q of the sponge is calculated after recording the oil absorption-release experiment for 10 and 100 cycles. The above test results are shown in Table 1.
[0130] Table 1 Performance test results
[0131]
[0132] By analyzing the data of Table 1, it can be known that the polyurethane sponge (embodiment 4) prepared by modified nano ZnO and micron SiO and unmodified nano ZnO and micron SiO and the polyurethane sponge (reference example 1) prepared by comparison show that the hydrophobicity of the polyurethane sponge prepared by modified nano ZnO and micron SiO and the adsorption capacity of kerosene have been greatly improved, and the polyurethane sponge (embodiment 4) prepared by composite preparation and the single particle (reference examples 2,3) comparison show that nano ZnO and micron SiO and the hydrophobicity of the polyurethane sponge prepared by composite preparation are better. In the above-mentioned embodiment, the water contact angle of embodiment 7 and the adsorption capacity of diesel oil are the best.
[0133] As the chain length of the silane compound increases (Examples 1 to 4), the water contact angle, the adsorption capacity for kerosene, the adsorption capacity after 10 cycles, and the adsorption capacity after 100 cycles of the polyurethane sponge all increase, among which the best performance is N-β (aminoethyl) -γ-aminopropyltriethoxysilane (Example 4). The reason is that as the chain length of the silane compound increases, the surface energy of the silane compound decreases, which in turn leads to an increase in the water contact angle and the adsorption capacity for diesel of the polyurethane sponge.
[0134] Along with modified nano ZnO and micron SiO Content rises (embodiment 4 to 7), the water contact angle of polyurethane sponge, the adsorption capacity to diesel, the adsorption capacity after circulation 10 times, the adsorption capacity after circulation 100 times all rise to some extent.When nano ZnO and micron SiO The performance of super hydrophobic polyurethane sponge is best when mass parts reaches 20 parts (embodiment 7).Reason is along with modified nano ZnO and micron SiO The increase of content, nano ZnO and micron SiO on polyurethane sponge surface and inside Content increases, and the micro-nano composite structure formed on sponge surface and inside increases, improves the roughness on polyurethane sponge surface, increases the water contact angle of polyurethane sponge, and the adsorption capacity of kerosene is improved.
[0135] As the temperature of the modified nano ZnO and micron SiO2 increases (Example 4, Example 8, Example 9), the water contact angle of the polyurethane sponge, the adsorption capacity for diesel, the adsorption capacity after 10 cycles, and the adsorption capacity after 100 cycles decrease. When the temperature of the modified nano ZnO and micron SiO2 is 60°C (Example 4), the hydrophobicity and adsorption performance of the polyurethane sponge for kerosene are the best.
[0136] As the foaming temperature increases (Example 4, Example 10, Example 11), the water contact angle of the polyurethane sponge, the adsorption capacity for diesel, the adsorption capacity after 10 cycles, and the adsorption capacity after 100 cycles decrease. When the foaming temperature is 20°C (Example 4), the contact angle and the adsorption capacity for kerosene of the polyurethane sponge are the best.
[0137] In summary, the present invention provides a long-acting super-hydrophobic polyurethane sponge and a preparation method thereof, wherein nano ZnO and micron SiO2 are treated with silane compounds to reduce the surface energy of nano ZnO and micron SiO2 and improve hydrophobicity; hydrophobically modified nano ZnO and hydrophobically modified micron SiO2 are added to a polyurethane prepolymer prepared by polyol and polyisocyanate, etc. and uniformly mixed, and in-situ polymerization is performed to obtain a super-hydrophobic polyurethane; and the super-hydrophobic polyurethane is freely foamed in a mold to obtain a long-acting super-hydrophobic polyurethane sponge. On the one hand, the silane compound treats the surface of nano ZnO and micron SiO2 powders, and introduces silane long-chain molecules on the surface of nano ZnO and micron SiO2 powders, which not only improves the interaction between nano ZnO and micron SiO2 powders and polyurethane molecules through covalent bond action, ensures that the powder is not easy to fall off from the polyurethane, but also reduces the surface energy of the powder, improves the hydrophobicity of the polyurethane sponge, and then improves the oil absorption efficiency of the polyurethane sponge. On the other hand, the polyurethane sponge obtained by in-situ polymerization and foaming has nano-ZnO and micro-SiO2 uniformly distributed, which can form a micro-nano composite structure on the surface and inside the sponge, thereby improving the mesoscopic roughness of the polyurethane sponge. Moreover, when the surface micro-nano composite structure loses its function due to long-term use and wear, the micro-nano composite structure inside the sponge will be exposed to the sponge surface, always ensuring that there is a micro-nano composite structure with a high roughness on the surface, solving the problem that the micro-nano composite structure is easily destroyed, thereby extending the life of the super-hydrophobic function of the polyurethane sponge. Under the combined effect of the above-mentioned low surface energy and micro-nano rough structure, the polyurethane sponge forms and continuously maintains super-hydrophobic properties, thereby having the function of long-term and efficient oil-water separation.
[0138] This polyurethane sponge with long-term and efficient oil-water separation ability can be used to efficiently remove oil pollution floating on the sea surface, lake surface and other water surfaces. Specifically, a long-lasting super-hydrophobic polyurethane sponge is placed in the oily sewage area. After the oil pollution on the water surface is adsorbed by the long-lasting super-hydrophobic polyurethane sponge, it is salvaged and collected, and the oil pollution is separated by centrifugation or extrusion. The regenerated sponge after the oil pollution is separated is put into the next round of use. This method of removing oil pollution on the water surface uses a long-lasting super-hydrophobic polyurethane sponge to efficiently absorb oil pollutants and achieve rapid separation of oil and water. At the same time, the sponge can be recycled, which helps to continuously improve water quality and the ecological environment.
[0139] Of course, the present invention may also have a variety of embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the disclosure of the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a long-lasting super-hydrophobic polyurethane sponge, characterized in that: The following steps are involved: Step 1: 50-80 parts by weight of polyol, 2-3 parts by weight of water, 1-4 parts by weight of foaming agent, 0.5-1.5 parts by weight of catalyst, and 0.4-1 parts by weight of foam stabilizer are uniformly mixed at a temperature of 15-30° C. to prepare a polyurethane auxiliary material, namely component A; Step 2: Add 50-75 parts by weight of polyisocyanate into a reaction container, stir at a temperature of 60-80° C. for 20-40 minutes, then add polyol at a mass ratio of polyisocyanate to polyol of 100:40-100:75, and react at a temperature of 60-80° C. to obtain a polyurethane prepolymer, i.e., component B; Step 3: 5-20 parts by mass of nano ZnO are dispersed in 60-80 parts by mass of a solvent, and then 1-3 parts by mass of a silane compound are added dropwise, and reacted at a temperature of 60-80° C. for 3-6 hours, and then the solid is separated, washed, and dried to obtain a hydrophobically modified ZnO powder, i.e., component C; Step 4: 5-20 parts by mass of micronized SiO2 is dispersed in 60-80 parts by mass of a solvent, and then 1-3 parts by mass of a silane compound is added dropwise, and reacted at a temperature of 60-80°C for 3-6 hours, and then the solid is separated, washed and dried to obtain a hydrophobically modified SiO2 powder, i.e., component D; Step 5: Component A, component B, component C and component D are mixed according to a mass ratio of component A: component B: component C: component D of 45-55:100:5-20:5-20, and an in-situ polymerization reaction is performed to obtain a super hydrophobic polyurethane; Step 6: Pour the super-hydrophobic polyurethane obtained in the above step 5 into a mold to carry out a free foaming reaction, and after drying, obtain a long-lasting super-hydrophobic polyurethane sponge.
2. The method for preparing a long-acting super-hydrophobic polyurethane sponge according to claim 1, wherein: In step 3, 5 to 20 parts by mass of nano ZnO are added to 60 to 80 parts by mass of 80% ethanol aqueous solution, and then acetic acid is added dropwise until the pH value of the solution is 4. After mixing, 1 to 3 parts by mass of silane compound are added dropwise under stirring conditions, and the reaction is carried out at a temperature of 60 to 80° C. for 3 to 6 hours. The solid is then separated by centrifugation, washed with distilled water and filtered, and then the washing and filtering steps are repeated 1 to 4 times. The filtered solid is vacuum dried at 60° C. to constant weight, crushed and sieved to obtain a hydrophobically modified ZnO powder, i.e., component C.
3. The method for preparing a long-acting super-hydrophobic polyurethane sponge according to claim 1, wherein: In step 4, 5 to 20 parts by mass of nano-SiO2 are added to 60 to 80 parts by mass of 80% ethanol aqueous solution, and then acetic acid is added dropwise until the pH value of the solution is 4. After mixing, 1 to 3 parts by mass of silane compound are added dropwise under stirring conditions, and the reaction is carried out at a temperature of 60 to 80°C for 3 to 6 hours. The solid is then separated by centrifugation, washed with distilled water and filtered, and then the washing and filtering steps are repeated 1 to 4 times. The filtered solid is vacuum dried at 60°C to constant weight, crushed and sieved to obtain a hydrophobically modified SiO2 powder, i.e., component D.
4. The method for preparing a long-acting super-hydrophobic polyurethane sponge according to claim 1, wherein: In step 5, the mass ratio of component A: component B: component C: component D is 50:100:5~20:5~20, component A, component B, component C and component D are weighed respectively and placed in a reaction vessel, at a temperature of 20~40 ° C and a rotating speed of 200~300 r / min, after in-situ polymerization for 10~30 min, the super-hydrophobic polyurethane is prepared by stirring for 15~30 s at a temperature of 20~40 ° C and a rotating speed of 1000~1500 r / min.
5. The method for preparing a long-acting super-hydrophobic polyurethane sponge according to claim 1, wherein: In step 6, the super-hydrophobic polyurethane obtained in step 5 is poured into a mold, and a free foaming reaction is carried out at 20-40° C. for 3-5 minutes. Then, the foamed polyurethane sponge is taken out and placed in a 60-80° C. oven with a flow rate of 50 ml / min of flowing N2 to dry for 3-6 hours to obtain the long-lasting super-hydrophobic polyurethane sponge.
6. The method for preparing a long-acting super-hydrophobic polyurethane sponge according to claim 1, wherein: The polyol in step 1 and step 2 is one or more of polytetrahydrofuran diol, polycarbonate diol, polycaprolactone diol and polypropylene glycol.
7. The method for preparing a long-acting super-hydrophobic polyurethane sponge according to claim 1, wherein: The blowing agent in step 1 is one or more of dichloromethane, 1,1,1,3,3-pentafluorobutane, 1,1,1,3,3-pentafluoropropane, 1,1,1,2-tetrafluoroethane, difluoroethane, and heptafluoropropane; and / or The catalyst in step 1 is selected from an organic metal catalyst and a tertiary amine catalyst, wherein the organic metal catalyst is one or more of dibutyltin dilaurate, distannous octoate, and dibutyltin acetate; and / or The foam stabilizer in step 1 is one or more of dimethyl silicone oil, dodecyl dimethyl amine oxide, and alkyl alcohol amide; and / or The polyisocyanate in step 2 is one or more of isophorone diisocyanate, hexamethylene diisocyanate, toluene diisocyanate; and / or The silane compound in step 3 is one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β (aminoethyl) -γ-aminopropyltrimethoxysilane, N-β (aminoethyl) -γ-aminopropylmethyldimethoxysilane, and N-β (aminoethyl) -γ-aminopropyltriethoxysilane.
8. The method for preparing a long-acting super-hydrophobic polyurethane sponge according to claim 1, wherein: The nano ZnO particle size in step 3 is 50-300 nm, preferably 100-200 nm; and / or The micron SiO2 particle size in step 4 is 50-300 μm, preferably 50-100 μm.
9. A long-lasting super-hydrophobic polyurethane sponge, characterized in that: The method is prepared according to any one of claims 1 to 8.
10. A method for removing oil pollution from a water surface, characterized in that: A long-lasting super-hydrophobic polyurethane sponge is placed in an oily wastewater area. After the oil on the water surface is adsorbed by the long-lasting super-hydrophobic polyurethane sponge, it is salvaged and collected, and the oil is separated by centrifugation or extrusion. The regenerated sponge after the oil is separated is put into the next round of use.
Citation Information
Patent Citations
Super-hydrophobic coating, super-hydrophobic coating layer, and preparation method thereof
CN106366907A
Preparation method of polysiloxane modified super-hydrophobic sponge for oil-water separation
CN114561039A
Super-hydrophobic-super-oleophylic sponge and preparation method thereof
CN114874407A
ZnO / PUF composite material with high phosphorus adsorption and preparation method of ZnO / PUF composite material
CN117160427A
Preparation method and application of selective adsorption hydrophobic polyurethane sponge
CN118059832A