Rare earth gear steel and surface treatment method

By adding rare earth elements to the gear steel and using a composite surface chemical heat treatment, the problems of high temperature, long cycle and high energy consumption in the traditional process are solved, the thickness and mechanical properties of the penetration layer are improved, and the requirements of the modern automobile market for gears are met. High demands on steel performance.

CN118835149APending Publication Date: 2024-10-25TIANJIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310450531.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Traditional surface chemical heat treatment processes such as gas carburizing have problems such as high temperature, long process cycle, high energy consumption, large gear deformation, and short service life, and are difficult to meet the high performance requirements of gear steel in the modern automotive market.

Method used

Add appropriate amounts of rare earth elements, such as cerium and lanthanum, to gear steel, and use a variety of composite surface chemical heat treatments, including gas carburizing, gas nitriding and gas carbonitriding, to optimize the composition and heat treatment process of gear steel. , improve the thickness and mechanical properties of the permeable layer.

Benefits of technology

Under the same conditions, the thickness and mechanical properties of the infiltrated layer are improved, the surface chemical heat treatment temperature and time are reduced, energy consumption is reduced, the fatigue performance and corrosion resistance of gear steel are improved, and the service life is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BSA0000296880530000041
    Figure BSA0000296880530000041
  • Figure HSA0000296880540000011
    Figure HSA0000296880540000011
  • Figure HSA0000296880540000012
    Figure HSA0000296880540000012
Patent Text Reader

Abstract

The invention relates to the field of gear steel and surface treatment, discloses rare earth gear steel and a surface treatment method, and particularly relates to gear steel added with rare earth and a method for optimizing surface shot blasting, chemical heat treatment and pre-oxidation and surface chemical heat treatment. The problem that an existing gear steel surface chemical heat treatment process is too long in period is mainly solved. The rare earth gear steel comprises the following components in percentage by mass: 0.15-0.48% of C; 0.2 to 0.8 percent of Si; mn: 0.9 to 2.5%; 1.0 to 3.5 parts of Cr; 0.02 to 1.5 percent of Ti; 0.005% to 0.5% of Mo; 0.01 to 0.5 percent of Ni; 0.01 to 0.5 percent of Cu; 0 to 2 percent of La; 0-2% of Ce; p and S are less than or equal to 0.005%; and the balance of Fe. Main alloy elements and rare earth elements with different gradients are subjected to optimal alloy component design. On the basis, shot blasting treatment or pre-oxidation treatment is adopted, and then a surface chemical heat treatment process is carried out. Compared with gear steel without rare earth and a single surface chemical heat treatment process, the carburized layer depth of the pretreated rare earth gear steel is improved, and the performance of the gear steel is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of gear steel and metal surface treatment, and in particular to a composition design and surface treatment combination optimization method for rare earth gear steel. Background Art

[0002] Gears are important devices in automobile transmission and play an indispensable role. According to their working characteristics, the outer part of the gear needs to have a certain strength and hardness, and the core needs to have a certain toughness.

[0003] Surface chemical heat treatment is a heat treatment process that can meet the performance requirements of gears and is widely used in the heat treatment process of gears.

[0004] Gas carburizing is a widely used surface chemical heat treatment technology, but it also has many problems. The traditional carburizing process has problems such as high carburizing temperature, long process cycle, high energy consumption, large gear deformation, and short service life. The temperature of gas nitriding and carbonitriding is relatively low, but the carburizing layer is thinner. And with the rapid development of the automobile market and the huge improvement in performance, higher and higher requirements are also placed on the performance of gear steel. How to change the status quo of surface chemical heat treatment technology and meet the performance requirements of gear steel has become our research focus. Therefore, we urgently need a new process or new method to improve the status quo.

[0005] The present invention proposes a new gear steel composition design and surface chemical heat treatment optimization method. By adding an appropriate amount of rare earth elements to the gear steel and adopting a surface chemical heat treatment method with multiple composite processes, not only the thickness of the infiltration layer is increased within the same surface chemical heat treatment time, but also the mechanical properties of the infiltration layer are improved, thereby effectively solving the existing problems. Summary of the invention

[0006] The purpose of the present invention is to provide a rare earth gear steel and a surface treatment method, which can improve the current situation in the field of gear steel surface chemical heat treatment and has strong feasibility.

[0007] The technical solution of the present invention is:

[0008] A rare earth gear steel and surface treatment method, a new gear steel composition is designed, and different contents of rare earth elements are added to the gear steel, and the composition of the gear steel is optimized in combination with actual test results and experience. The gear steel is surface treated, and the surface chemical heat treatment process is optimized by using a variety of composite processes.

[0009] The rare earth gear steel and surface treatment method contain cerium and lanthanum as the added rare earth elements.

[0010] The role of rare earth elements in gear steel in the present invention is as follows:

[0011] Purification: Rare earths can react with oxygen, sulfur and other impurities in molten steel to form rare earth oxides, sulfides or oxysulfides. Therefore, rare earths can be used as strong deoxidizers and desulfurizers for molten steel to purify it. Modification: After deoxidation and desulfurization, rare earths can be transformed into oxides and sulfides. Due to the high melting point of these inclusions, they can be used as non-uniform nucleation centers during solidification of molten steel, and play a role in refining the solidification structure of steel. Since these inclusions are not easily deformed at the rolling temperature and still maintain a small spherical shape, the morphology of inclusions in steel can be controlled, thereby avoiding or overcoming the deformation of other types of inclusions during hot pressure processing of steel. Alloying: Rare earth elements dissolved in steel may produce certain alloying effects. This alloying effect is manifested in the rare earth affecting the phase change process of steel, changing the composition and structure of the phase change products, thereby improving the fatigue performance and corrosion resistance of steel, and increasing the microhardness of steel.

[0012] The rare earth gear steel and surface treatment method have the following components and contents: C: 0.15-0.48%; Si: 0.2-0.8%; Mn: 0.9-2.5%; Cr: 1.0-3.5; Ti: 0.02-1.5%; Mo: 0.005-0.5%; Ni: 0.01-0.5%; Cu: 0.01-0.5%; La: 0-2%; Ce: 0-2%; P, S≤0.005%; the rest is Fe.

[0013] The design steps of the present invention are:

[0014] Design different gradients of rare earth element content and adjust the proportions.

[0015] Different gradients of rare earth elements are added during the gear steel smelting process, and gear steels with different rare earth element contents are finally obtained.

[0016] The final rare earth gear steel bar is obtained by performing smelting + refining + vacuum treatment + continuous casting + forging + slow cooling according to the designed rare earth element content.

[0017] The forged gear steel is pre-normalized at 900-930°C and kept warm for 2 hours.

[0018] In order to facilitate observation and subsequent processing, as some optional embodiments of the present invention, the size of the sample is cut into 15x15x15mm by wire cutting.

[0019] The surface roughness of the gear steel that has been pre-heat treated is processed to Ra3.2.

[0020] The sample with surface roughness treatment is placed in a pit furnace for surface chemical heat treatment.

[0021] Surface chemical heat treatment processes include gas carburizing, gas nitriding and gas carbonitriding.

[0022] The carbon potential during gas carburizing is 0.9-1.2%, the temperature is 890-930℃, and the time is 15-25h. After gas carburizing, a heat treatment of heating and quenching is adopted, and finally a low-temperature tempering treatment is adopted. The temperature of the first heating and quenching is 860-890℃, and the time is 3-5h. The quenching medium is oil; the temperature of the low-temperature tempering treatment is 180-200℃, and the time is 1-2h.

[0023] The gas carbonitriding temperature is 820-860°C, the time is 3-6 hours, and the quenching medium is oil; the low-temperature tempering treatment temperature is 180-200°C, and the time is 1-2 hours.

[0024] Before gas nitriding, quenching and tempering treatment is required. The quenching temperature is 860-900℃, the time is 2-3h, and the quenching medium is oil; the tempering temperature is 560-600℃, and the time is 2-3h. The gas nitriding atmosphere is ammonia, the gas nitriding temperature is 460-500℃, the time is 40-50h, and the cooling method is furnace cooling.

[0025] The penetration depth of the samples after surface chemical heat treatment was measured by hardness method.

[0026] Based on the above test results, the sample with the best surface chemical heat treatment effect can be obtained, and the corresponding rare earth content can be obtained.

[0027] A group of samples with rare earth content corresponding to the best gas nitriding effect are selected, and this group of samples are tempered and then pre-oxidized at a temperature of 300-400°C for 0.5-2h. Gas nitriding is then performed at the same temperature as the samples that have not been pre-oxidized.

[0028] A group of samples with rare earth content corresponding to the best gas nitriding effect are selected, and these samples are tempered and then shot peened for 1 to 2 hours, and gas nitrided at the same temperature as the samples that have not been shot peened.

[0029] The penetration depths of the samples after the above two groups of composite processes were measured, and they were both increased compared with the penetration depths of the samples after single surface chemical heat treatment.

[0030] The advantages and beneficial effects of the present invention are:

[0031] The operation of the present invention is relatively simple and can reduce production costs. Under the same gas carburizing conditions, samples containing an appropriate amount of rare earth elements can obtain a deeper carburizing layer thickness; when meeting the same performance requirements, samples containing an appropriate amount of rare earth elements can reduce the surface chemical heat treatment temperature, shorten the surface chemical heat treatment time, and reduce energy consumption. The surface chemical heat treatment of the composite process is superior to the single surface chemical heat treatment process. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the gas carburizing metallographic structure when the rare earth content is optimal.

[0033] Figure 2 This is the gas carbonitriding metallographic phase when the rare earth content is optimal.

[0034] Figure 3 This is the gas nitriding metallographic structure when the rare earth content is optimal. DETAILED DESCRIPTION

[0035] The present invention will be further explained below with reference to the embodiments, but the present invention is not limited to the following embodiments.

[0036] Examples 1-5

[0037] The present invention provides a rare earth gear steel and a surface treatment method, the main operation of which includes the following steps:

[0038] (1) Component design and implementation

[0039] A new gear steel composition was designed with different types of rare earth elements added.

[0040] The rare earth elements added to gear steel are cerium and lanthanum.

[0041] According to the determined rare earth element types, the corresponding rare earth element content is designed to prepare the raw materials.

[0042] The final rare earth gear steel bar is obtained by performing smelting + refining + vacuum treatment + continuous casting + forging + slow cooling according to the designed rare earth element content.

[0043] The composition of the rare earth gear steel is shown in Table 1

[0044] Table 1 Content of each component of five groups of rare earth gear steels (P, S ≤ 0.005, the balance is Fe, wt%)

[0045] C Si Mn Cr Ti Mo Ni Cu La Ce Example 1 0.20 0.23 1.0 1.50 0.64 0.007 0.08 0.03 0 0 Example 2 0.21 0.24 1.1 1.50 0.65 0.007 0.08 0.03 0.5 0.5 Example 3 0.21 0.23 1.0 1.49 0.64 0.006 0.08 0.03 1.0 1.0 Example 4 0.19 0.23 0.9 1.50 0.64 0.006 0.08 0.03 1.5 1.5 Example 5 0.20 0.23 0.9 1.51 0.65 0.006 0.08 0.03 2.0 2.0

[0046] (2) Pretreatment before infiltration

[0047] The obtained rod-shaped samples were subjected to a pre-normalizing heat treatment at 900-930°C and kept warm for 2h.

[0048] After normalizing, the specimens were wire cut into cubes of 15x15x15mm.

[0049] The surface roughness of the cubic specimen was machined to Ra3.2.

[0050] (3) Gas carburizing treatment

[0051] The samples with surface roughness treatment were placed in a pit furnace for gas carburizing treatment.

[0052] The carbon potential during the gas carburizing process is 0.9-1.2%, the temperature is 890-930°C, and the time is 15-25 hours. After the gas carburizing, a heat treatment of heating and quenching is adopted, and finally a low-temperature tempering treatment is adopted.

[0053] The temperature of the first heating quenching is 860-890℃, and the time is 3-5h. The quenching medium is oil; the temperature of the low-temperature tempering treatment is 180-200℃, and the time is 1-2h.

[0054] (4) Organization observation and performance testing

[0055] The five types of gear steels obtained after gas carburizing were cut by wire cutting to obtain the carburized layer cross section.

[0056] The cross section of the infiltrated layer is ground and polished, and then corroded using a 4% nitric acid alcohol solution. The metallographic structure of the cross section of the infiltrated layer can be observed under an optical microscope.

[0057] The cross section of the infiltration layer was ground and polished, and the hardness was tested using a Vickers microhardness tester, and the depth of the infiltration layer was determined by the hardness method.

[0058] The standard selected for measuring Vickers hardness is: load 9.8N, loading time 10s.

[0059] Embodiment 6-10

[0060] The sequence of Example 6-10 is the same as that of Example 1-5, except that Example 6-10 is gas carbonitriding, the gas carbonitriding temperature is 820-860°C, the time is 3-6h, the quenching medium is oil; the low-temperature tempering treatment temperature is 180-200°C, and the time is 1-2h.

[0061] Examples 11-15

[0062] The sequence of Examples 11-15 is the same as that of Examples 1-5, except that Examples 11-15 are gas nitriding. Before gas nitriding, a tempering treatment is required, the quenching temperature is 860-900°C, the time is 2-3h, the quenching medium is oil; the tempering temperature is 560-600°C, the time is 2-3h. The gas nitriding atmosphere is ammonia, the gas nitriding temperature is 460-500°C, the time is 40-50h, and the cooling method is furnace cooling. The load required to measure the Vickers hardness of the nitrided layer is 2.94N, and the time is 10s.

[0063] Example 16

[0064] Example 16 is the same as Examples 11-15, except that Example 16 selects a group of samples with the best nitriding effect for shot peening after tempering before nitriding for 1 to 2 hours, and then performs nitriding treatment again, and compares them with nitrided samples that have not been shot peened.

[0065] Embodiment 17

[0066] Example 17 is the same as Example 16, except that the treatment after tempering before nitriding in Example 17 is pre-oxidation treatment, the pre-oxidation temperature is 300-400°C, the time is 0.5-2h, and it is compared with the nitrided samples without pre-oxidation treatment.

[0067] Table 2 Sample penetration depth (Examples 1-15)

[0068]

[0069] Table 3 Depth of nitriding layer treated by composite process

[0070] Nitriding layer depth (mm) Example 16 0.71 Embodiment 17 0.68

[0071] It can be seen from Table 2 that after the addition of rare earth elements, the penetration depth of the sample is improved.

[0072] By the same token, while achieving the same penetration layer requirements, the sample containing an appropriate amount of rare earth elements requires a shorter surface heat treatment time, thereby reducing energy consumption.

[0073] In Example 16, compared with the sample without shot peening treatment, the infiltration layer of the sample after shot peening treatment increased by 31%.

[0074] Compared with the sample without pre-oxidation, the diffusion layer of the sample in Example 17 increased by 26% after pre-oxidation.

[0075] Thickening effect of diffusion layer: surface chemical heat treatment of multiple composite processes with rare earth addition > surface chemical heat treatment with rare earth addition > surface chemical heat treatment.

Claims

1. A method for preparing rare earth gear steel, characterized in that: The method for preparing rare earth gear steel comprises the following steps: Determine the alloy composition of the gear steel; the basic components of the gear steel are C: 0.15-0.48%; Si: 0.2-0.8%; Mn: 0.9-2.5%; Cr: 1.0-3.5; Ti: 0.02-1.5%; Mo: 0.005-0.5%; Ni: 0.01-0.5%; Cu: 0.01-0.5%; P, S≤0.005%; the rest is Fe; rare earth alloying is performed on the basic components, the rare earth elements are La and Ce; among which, the rare earth elements The process of determining the content is: smelting + refining + vacuum treatment + continuous casting + forging + slow cooling steps to obtain rare earth gear steel bars; normalizing heat treatment of the rare earth gear steel bars; tempering treatment after normalizing; a group of rare earth gear steels are selected for pre-oxidation treatment, and gas nitriding is carried out at the same temperature as the samples in the same group that have not been pre-oxidized; the depth of the penetration layer of the samples after surface treatment is measured by hardness method, and the rare earth element content when the performance of the rare earth gear steel is optimal is determined according to the measurement results. According to the designed composition, smelting + refining + vacuum treatment + continuous casting + forging + slow cooling steps are performed to obtain rare earth gear steel bars; normalizing heat treatment is performed on the rare earth gear steel bars; tempering treatment is performed after normalizing treatment, pre-oxidation treatment is performed after tempering treatment, and gas nitriding treatment is performed after pre-oxidation treatment; the final rare earth gear steel is obtained.

2. A method for preparing rare earth gear steel, characterized in that: The method for preparing rare earth gear steel comprises the following steps: Determine the alloy composition of the gear steel; the basic components of the gear steel are C: 0.15-0.48%; Si: 0.2-0.8%; Mn: 0.9-2.5%; Cr: 1.0-3.5; Ti: 0.02-1.5%; Mo: 0.005-0.5%; Ni: 0.01-0.5%; Cu: 0.01-0.5%; P, S ≤ 0.005%; the rest is Fe; rare earth alloying is performed on the basic components, the rare earth elements are La and Ce; among which, the rare earth element The process of determining the element content is: smelting + refining + vacuum treatment + continuous casting + forging + slow cooling steps to obtain rare earth gear steel bars; normalizing heat treatment of the rare earth gear steel bars; tempering treatment after normalizing; a group of rare earth gear steels are selected for shot peening, and gas nitriding is performed at the same temperature as the samples in the same group that have not been shot peened; the depth of the penetration layer of the samples after surface treatment is measured by hardness method, and the rare earth element content when the performance of the rare earth gear steel is optimal is determined based on the measurement results. According to the designed composition, smelting + refining + vacuum treatment + continuous casting + forging + slow cooling steps are performed to obtain rare earth gear steel bars; normalizing heat treatment is performed on the rare earth gear steel bars; tempering treatment is performed after normalizing treatment, shot peening treatment is performed after tempering treatment, and gas nitriding treatment is performed after shot peening treatment; the final rare earth gear steel is obtained.