High-performance die steel for die casting and preparation method thereof
Through non-vacuum induction furnace, LF furnace and VD furnace smelting combined with the secondary remelting process of protective atmosphere electroslag furnace, the problem of insufficient red hardness and impact toughness of die-casting mold steel was solved, and a die-casting die steel with high thermal fatigue resistance and high toughness was produced. Mold steel meets the needs of high-end applications in new energy vehicles and other fields.
Patent Information
- Application Number
- CN202410890867.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-25
AI Technical Summary
Existing die-casting mold steels in high-end applications have insufficient red hardness and impact toughness, and the average grain size is low, resulting in thermal fatigue cracking resistance, hardenability and high-temperature softening resistance that cannot meet usage requirements.
Use non-vacuum induction furnace + LF furnace + VD furnace for smelting, combined with protective atmosphere electroslag furnace for secondary remelting, and prepare mold steel with high structural uniformity and high purity through high-temperature homogenization, forging and annealing processes. , the element composition includes C, Mn, Si, Cr, Ni, Mo, V, Cu, etc., and the material properties are improved through multiple forging and annealing treatments.
The obtained mold steel has high red hardness, excellent resistance to thermal fatigue cracking and high toughness. The hardness reaches 48-50HRC, the transverse unnotched impact toughness is above 400J, the V-notch impact is >20J, and the structure rating reaches AS4 level. The particle size reaches level 8, which is suitable for the high-end die-casting mold steel market.
Smart Images

Figure BDA0004927488000000051 
Figure BDA0004927488000000061 
Figure BDA0004927488000000121
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of mold steel preparation, and specifically relates to a high-performance die-casting mold steel and a preparation method thereof, and in particular to a die-casting mold steel for alloys such as aluminum and magnesium, which can be used in the fields of new energy vehicles, etc. Background Art
[0002] Die casting mold is a tool that completes the die casting process on a special die casting machine. It is used to cast metal parts and can be applied to industries such as automobiles, motors, and electrical appliances. Among automobile die casting molds, aluminum-magnesium alloy die casting molds are currently the most widely used molds.
[0003] In recent years, with the development of new energy vehicles, the demand for weight reduction of auto parts has become increasingly strong. Die-casting molds are widely used in the field of new energy vehicles, and the demand for large, precise and complex die-casting parts such as automobile cylinder blocks, instrument panels, and automatic transmission housings will become greater and greater. In order to achieve lightweight automobiles, molds must be used to form various materials. Therefore, the development and industrialization of lightweight automobile molds are very critical and very important for the development of a low-carbon economy. Die-casting molds based on lightweight automobiles mainly include aluminum alloy engine cylinder block and cylinder head die-casting molds, titanium aluminum alloy automobile valve die-casting molds, and aluminum alloy die-casting molds for automobile steering wheels and instrument panels.
[0004] With the current trend of integrated die-casting bodies for new energy vehicles, die-casting die steel product development will become an important direction for die steel in the future. However, in the actual manufacturing process, due to the large size of metal profiles used in automobile manufacturing, the hardness, strength, impact toughness and other properties of die-casting dies are significantly reduced under the continuous alternation of hot and cold and impact loads. Especially under the condition of thermal wear, it is very easy to crack and cause the die-casting dies to break.
[0005] Some studies have tried to improve the surface hardness of die steel by nitriding and carburizing castings, but in actual operation, the hardness of the die-casting die steel surface is not ideal due to the thin carburizing layer. In addition, various production processes have been proposed to improve the performance of die-casting die steel, but although the red hardness of die-casting die steel obtained by the current process has been improved, it is still not high enough, and the impact toughness is generally low, the average grain size is also low, and the mold steel's resistance to thermal fatigue cracking, hardenability and high temperature softening resistance are still insufficient.
[0006] Therefore, the preparation of die-casting mold materials with higher red hardness, better resistance to thermal fatigue cracking, high toughness, excellent hardenability and resistance to high-temperature softening has become a technical problem that needs to be solved urgently. Summary of the invention
[0007] The present invention is to solve the above technical problems, thereby providing a high-performance die-casting die steel and a preparation method thereof. The technical purpose of the present invention is to solve the problems existing in the preparation process of die-casting die steel that the die steel red hardness and impact toughness are insufficient, and the average grain size grade is low, so that the die steel's resistance to thermal fatigue cracking, hardenability and resistance to high temperature softening cannot meet the use requirements.
[0008] In order to achieve the above technical objectives, the technical solution adopted by the present invention is as follows:
[0009] The present invention first provides a method for preparing die steel for die casting to meet the use requirements in the field of high-end die steel products. The method for preparing high-performance die steel for die casting comprises the following steps:
[0010] (1) preparing alloys according to corresponding elemental compositions, melting molten steel in a non-vacuum induction furnace at a melting temperature of 1510-1520°C, adding slag for deoxidation and desulfurization during the melting process, removing slag ≥90% after the material is cleared, then adding slag again to make slag, adding Al powder for diffusion deoxidation, heating to 1560-1590°C for sampling and analysis, further heating to above 1640°C, tapping and entering an LF furnace;
[0011] (2) After the ladle is placed in the LF station, the temperature is raised and the slag is adjusted. The composition is adjusted according to the sampling results, and carbon powder, Al powder, and Si-Ca powder are added for diffusion deoxidation to maintain a reducing atmosphere. The slag is sampled, the temperature is raised to 1690-1700℃, and the slag removal is ≥60%. The steel is then discharged and sent to the VD station;
[0012] (3) Before the VD furnace is evacuated, 0.5 kg / T of rare earth is placed in the bag. The total evacuation time is ≥30 min, the ultimate vacuum is ≤133 Pa, and the holding time is ≥10 min. After breaking the vacuum, the temperature is measured, and the argon gas is blown for ≥10 min. The temperature is measured at 1535-1545 ° C, and the steel is poured;
[0013] (4) The electrode rod is demoulded after 4 hours of casting, slowly cooled to 300-400°C and then put into a furnace for annealing. After annealing, the ends of the electrode rod are flattened and the surface is polished;
[0014] (5) placing the electrode rod as an electrode in a protective atmosphere electroslag remelting furnace for secondary remelting and purification to form an electroslag ingot;
[0015] (6) The electroslag ingot is loaded into the furnace for forging within 24 hours after the cover is removed;
[0016] (7) Place the treated steel ingot in a heating furnace, heat it to 500°C at ≤100°C / h and keep it for 3h, then heat it to 850°C at ≤150°C / h and keep it for 4h, finally heat it to 1250°C at ≤200°C / h and keep it for 5h, after the steel ingot is pulled out of the billet, return to the furnace for high temperature diffusion at 1300°C for 40h, then open the furnace door for 30min or transfer it to a low temperature furnace and keep it at 1180°C for 2h before forging;
[0017] (8) The steel ingot is taken out of the furnace, and the intermediate billet is forged and drawn. The intermediate billet is returned to the furnace and kept at 1160°C for 1-2 hours;
[0018] (9) The intermediate billet is taken out of the furnace for upsetting and drawing, and after forging, it is water-cooled at 3 min / 100 mm. After taking out of the water, it is air-cooled to 350 ° C and then loaded into the furnace for spheroidizing annealing;
[0019] (10) After annealing, the module is flattened and surface ground;
[0020] (11) The module processed in step (10) is subjected to ultra-fine processing to prepare a mold steel with high purity and good structural uniformity.
[0021] The preparation method provided by the present invention adopts a non-vacuum induction furnace + LF furnace + VD furnace for primary smelting, and then adopts a protective atmosphere electroslag furnace for secondary remelting to obtain a uniform and highly pure electroslag ingot, and the steel ingot is subjected to high-temperature homogenization, cooling forging, water cooling after forging and other forging processes to obtain a module with uniform and highly pure structure. The steel has excellent resistance to thermal fatigue cracking, high red hardness and high toughness. The transverse unnotched impact toughness is above 400J at a hardness of 48-50HRC, and the V-notch impact is greater than 20J. The organization rating can be rated as AS4 according to the sampling and inspection of the NADCA-207 North American die casting standard. The banded organization rating can reach SA1 level by sampling and inspection according to the SEP1614 hot working die steel microscopic inspection and evaluation standard rating chart microscopic inspection method. The grain size grade can reach 8 levels according to the GB / T 6394-2002 metal average grain size determination method.
[0022] Furthermore, in step (1), the molten steel is melted in a 20T non-vacuum induction furnace, and pre-slag is made using a 3T furnace mixed blasting.
[0023] Furthermore, in step (2), the white slag is maintained for ≥30 min during the LF furnace refining period.
[0024] Furthermore, in step (4), the annealing temperature is 700-750°C, the holding time is ≥20h, and the furnace is cooled to 500°C at a rate of ≤30°C / h and then air-cooled out of the furnace.
[0025] Furthermore, in step (5), the protective atmosphere electroslag remelting uses 66# pre-melted slag with a melting rate of 7.0-6.5 kg / min. After the electroslag is finished, the furnace is cooled for ≥90 minutes and then hood-cooled, and the hood-cooling time is ≥72 hours.
[0026] Furthermore, in step (8) and step (9), the forging process includes two upsetting, two drawing and two fire forming, and the starting forging temperature is ≥1050°C, and the final forging temperature is 800-850°C.
[0027] Furthermore, in step (9), the annealing temperature is 850-880°C, the holding time is 4h / 100mm, and the temperature is lowered to 730°C at a rate of ≤30°C / h and kept at that temperature for 24 hours, and then the temperature is lowered to 500°C at a rate of ≤30°C / h and air-cooled before being taken out of the furnace.
[0028] Furthermore, in step (11), the ultra-fine treatment process is a quenching and a spheroidizing annealing treatment.
[0029] The second object of the present invention is to provide a high-performance die-casting die steel prepared by the above method. The element composition of the die steel includes, by weight percentage: C: 0.30-0.40%, Mn: 0.20-0.60%, Si: ≤0.30%, S: ≤0.002%, P: ≤0.015%, Cr: 4.70-5.50%, Ni: 0.50-0.80%, Ni: 0.50-0.80%, Mo: 2.00-2.40%, V: 0.50-0.70%, Cu: ≤0.20%, Al: ≤0.03%, and the balance is iron and unavoidable residual elements.
[0030] The beneficial effects of the present invention are as follows:
[0031] (1) The mold steel material prepared by the method provided by the present invention has excellent resistance to thermal fatigue cracking, high red hardness and high toughness. When the hardness is 48-50HRC, the transverse unnotched impact toughness is above 400J, and the V-notch impact is greater than 20J.
[0032] (2) The mold steel obtained by the method of the present invention has good uniformity of organization. The organization rating can be rated as AS4 according to the sampling and inspection of NADCA-207 North American die casting standard. The banded organization rating can reach SA1 according to the microscopic inspection method of SEP1614 hot working die steel microscopic inspection and evaluation standard rating chart. The grain size grade can reach 8 according to the GB / T 6394-2002 metal average grain size determination method.
[0033] (3) The mold steel material produced by the method of the present invention has good economic and social benefits in the high-end die-casting mold steel market and is suitable for promotion and use. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described in detail below in conjunction with the embodiments. It is necessary to point out that the following embodiments are only used to explain and illustrate the present invention and are not used to limit the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above invention content still belong to the protection scope of the present invention.
[0035] The following examples provide four new die-casting die steels, respectively. The element composition of the die steels in each example is shown in Table 1 by weight percentage:
[0036] Table 1
[0037]
[0038]
[0039] Example 1
[0040] A method for preparing a novel die-casting die steel comprises the following steps:
[0041] (1) The alloy was prepared according to the element composition of Example 1 in Table 1 above, and the molten steel was melted in a 20T non-vacuum induction furnace at a melting temperature of 1510°C. The slag was pre-made by using a 3T furnace mixed blasting. During the smelting process, slag was added for deoxidation and desulfurization. After the material was cleared, 90% of the slag was removed. Then, slag was added again for slag making, and Al powder was added for diffusion deoxidation. The temperature was raised to 1560°C for sampling and analysis, and the temperature was further raised to above 1640°C, and the steel was tapped and sent to the LF furnace;
[0042] (2) After the ladle is placed in the LF station, the temperature is raised and the slag is adjusted. The composition is adjusted according to the sampling results, and carbon powder, Al powder, and Si-Ca powder (m:m=1:1) are added for diffusion deoxidation to maintain a reducing atmosphere. The slag is sampled, the temperature is raised to 1690℃ to remove 60% of the slag, and the steel is tapped into the VD station; the white slag is kept for 30 minutes during the LF furnace refining period;
[0043] (3) Before the VD furnace is evacuated, 0.5 kg / T of rare earth is placed in the bag. The total evacuation time is 30 min, the ultimate vacuum is 133 Pa, the holding time is 10 min, the temperature is measured after the vacuum is broken, argon is blown for 10 min, the temperature is measured at 1535 ° C, and the steel is poured;
[0044] (4) The electrode rod is demoulded 4 hours after casting, slowly cooled to 300°C and then put into furnace for annealing. After annealing, the ends of the electrode rod are flattened and the surface is polished. The annealing temperature is 700°C, the holding time is 20h, and the electrode rod is cooled to 500°C at 30°C / h and then air-cooled out of the furnace.
[0045] (5) Placing the electrode rod as an electrode in a protective atmosphere electroslag remelting furnace for secondary remelting and purification to form an electroslag ingot; the protective atmosphere electroslag remelting uses 66# pre-melted slag with a melting rate of 7.0 kg / min. After the electroslag is finished, the furnace is cooled for 90 minutes and then covered with cooling for 72 hours;
[0046] (6) The electroslag ingot is loaded into the furnace for forging within 24 hours after the cover is removed;
[0047] (7) Place the treated steel ingot in a heating furnace, heat it to 500°C at 100°C / h and keep it for 3 hours, then heat it to 850°C at 150°C / h and keep it for 4 hours, and finally heat it to 1250°C at 200°C / h and keep it for 5 hours. After the steel ingot is pulled out of the billet, it is returned to the furnace for high-temperature diffusion at 1300°C for 40 hours, and then the furnace door is opened for 30 minutes or transferred to a low-temperature furnace and kept at 1180°C for 2 hours before being taken out of the furnace for forging;
[0048] (8) The steel ingot is taken out of the furnace, and then the intermediate billet is forged and drawn. The intermediate billet is returned to the furnace and kept at 1160°C for 1 hour;
[0049] (9) The intermediate billet is taken out of the furnace for upsetting and drawing, and after forging, it is water-cooled at 3 min / 100 mm. After taking out of the water, it is air-cooled to 350 ° C and then charged into the furnace for spheroidizing annealing; the annealing temperature is 850 ° C, the holding time is 4 h / 100 mm, and the temperature is reduced to 730 ° C at 30 ° C / h and kept for 24 hours, and then the temperature is reduced to 500 ° C at 30 ° C / h and air-cooled out of the furnace; the forging process of steps (8) and (9) includes two upsetting, two drawing and two fire forming, and the starting forging temperature is 1050 ° C and the final forging temperature is 800 ° C;
[0050] (10) After annealing, the module is flattened and surface ground;
[0051] (11) The module processed in step (10) is subjected to ultra-fine processing. The ultra-fine processing process includes one quenching and one spheroidizing annealing treatment to prepare a mold steel with high purity and good structural uniformity.
[0052] Example 2
[0053] A method for preparing a novel die-casting die steel comprises the following steps:
[0054] (1) The alloy was prepared according to the element composition of Example 2 in Table 1 above, and the molten steel was melted in a 20T non-vacuum induction furnace at a melting temperature of 1515°C. The slag was pre-made by using a 3T furnace mixed blasting. During the smelting process, slag was added for deoxidation and desulfurization. After the material was cleared, 92% of the slag was removed. Then, slag was added again for slag making, and Al powder was added for diffusion deoxidation. The temperature was raised to 1570°C for sampling and analysis, and the temperature was further raised to above 1640°C, and the steel was tapped and sent to the LF furnace;
[0055] (2) After the ladle is placed in the LF station, the temperature is raised and the slag is adjusted. The composition is adjusted according to the sampling results, and carbon powder, Al powder, and Si-Ca powder (m:m=1:1) are added for diffusion deoxidation to maintain a reducing atmosphere. The slag is sampled, the temperature is raised to 1695℃ to remove 62% of the slag, and the steel is tapped into the VD station; the white slag is kept for 35 minutes during the LF furnace refining period;
[0056] (3) Before the VD furnace is evacuated, 0.5 kg / T of rare earth is placed in the bag. The total evacuation time is 32 min, the ultimate vacuum is 131 Pa, the holding time is 12 min, the temperature is measured after the vacuum is broken, argon is blown for 12 min, the temperature is measured at 1538 ° C, and the steel is poured;
[0057] (4) The electrode rod is demoulded 4 hours after casting, slowly cooled to 325°C and then put into furnace for annealing. After annealing, the ends of the electrode rod are flattened and the surface is polished. The annealing temperature is 720°C, the holding time is 22h, and the electrode rod is cooled to 500°C at 28°C / h and then air-cooled out of the furnace.
[0058] (5) Placing the electrode rod as an electrode in a protective atmosphere electroslag remelting furnace for secondary remelting and purification to form an electroslag ingot; the protective atmosphere electroslag remelting uses 66# pre-melted slag with a melting rate of 6.6 kg / min. After the electroslag is finished, the furnace is cooled for 92 minutes and then covered with cooling for 73 hours;
[0059] (6) The electroslag ingot is loaded into the furnace for forging within 24 hours after the cover is removed;
[0060] (7) Place the treated steel ingot in a heating furnace, heat it to 500°C at 98°C / h and keep it for 3 hours, then heat it to 850°C at 148°C / h and keep it for 4 hours, and finally heat it to 1250°C at 198°C / h and keep it for 5 hours. After the steel ingot is pulled out of the billet, return it to the furnace for high-temperature diffusion at 1300°C for 40 hours, then open the furnace door for 30 minutes or transfer it to a low-temperature furnace and keep it at 1180°C for 2 hours before forging;
[0061] (8) The steel ingot is taken out of the furnace, and then the intermediate billet is forged and drawn. The intermediate billet is returned to the furnace and kept at 1160°C for 1.2 hours;
[0062] (9) The intermediate billet is taken out of the furnace for upsetting and drawing, and after forging, it is water-cooled at 3 min / 100 mm. After taking out of the water, it is air-cooled to 350 ° C and then charged into the furnace for spheroidizing annealing; the annealing temperature is 860 ° C, the holding time is 4 h / 100 mm, and the temperature is reduced to 730 ° C at 28 ° C / h and kept for 24 hours, and then the temperature is reduced to 500 ° C at 28 ° C / h and air-cooled out of the furnace; the forging process of steps (8) and (9) is two upsetting, two drawing and two fire forming, and the starting forging temperature is 1050 ° C and the final forging temperature is 800 ° C;
[0063] (10) After annealing, the module is flattened and surface ground;
[0064] (11) The module processed in step (10) is subjected to ultra-fine processing. The ultra-fine processing process includes one quenching and one spheroidizing annealing treatment to prepare a mold steel with high purity and good structural uniformity.
[0065] Example 3
[0066] A method for preparing a novel die-casting die steel comprises the following steps:
[0067] (1) The alloy was prepared according to the element composition of Example 3 in Table 1 above, and the molten steel was melted in a 20T non-vacuum induction furnace at a melting temperature of 1518°C. The slag was pre-made by using a 3T furnace mixed blasting. During the smelting process, slag was added for deoxidation and desulfurization. After the material was cleared, 94% of the slag was removed. Then, slag was added again for slag making, and Al powder was added for diffusion deoxidation. The temperature was raised to 1580°C for sampling and analysis, and the temperature was further raised to above 1640°C, and the steel was tapped and sent to the LF furnace;
[0068] (2) After the ladle is placed in the LF station, the temperature is raised and the slag is adjusted. The composition is adjusted according to the sampling results, and carbon powder, Al powder, and Si-Ca powder (m:m=1:1) are added for diffusion deoxidation to maintain a reducing atmosphere. The slag is sampled, the temperature is raised to 1697℃ to remove 65% of the slag, and the steel is tapped into the VD station; the white slag is kept for 35 minutes during the LF furnace refining period;
[0069] (3) Before the VD furnace is evacuated, 0.5 kg / T of rare earth is placed in the bag. The total evacuation time is 35 min, the ultimate vacuum is 131 Pa, the holding time is 14 min, the temperature is measured after the vacuum is broken, argon is blown for 15 min, the temperature is measured at 1541 ° C, and the steel is poured;
[0070] (4) The electrode rod is demoulded 4 hours after casting, slowly cooled to 360°C and then put into furnace for annealing. After annealing, the ends of the electrode rod are flattened and the surface is polished. The annealing temperature is 740°C, the holding time is 23h, and the electrode rod is cooled to 500°C at 26°C / h and then air-cooled out of the furnace.
[0071] (5) Placing the electrode rod as an electrode in a protective atmosphere electroslag remelting furnace for secondary remelting and purification to form an electroslag ingot; the protective atmosphere electroslag remelting uses 66# pre-melted slag with a melting rate of 6.8 kg / min. After the electroslag is finished, the furnace is cooled for 94 minutes and then covered with cooling for 75 hours;
[0072] (6) The electroslag ingot is loaded into the furnace for forging within 24 hours after the cover is removed;
[0073] (7) Place the treated steel ingot in a heating furnace, heat it to 500°C at 96°C / h and keep it for 3 hours, then heat it to 850°C at 145°C / h and keep it for 4 hours, and finally heat it to 1250°C at 195°C / h and keep it for 5 hours. After the steel ingot is pulled out of the billet, it is returned to the furnace for high-temperature diffusion at 1300°C for 40 hours, and then the furnace door is opened for 30 minutes or transferred to a low-temperature furnace and kept at 1180°C for 2 hours before being taken out of the furnace for forging;
[0074] (8) The steel ingot is taken out of the furnace, and then the intermediate billet is forged and drawn. The intermediate billet is returned to the furnace and kept at 1160°C for 1.8 hours;
[0075] (9) The intermediate billet is taken out of the furnace for upsetting and drawing, and after forging, it is water-cooled at 3 min / 100 mm. After taking out of the water, it is air-cooled to 350 ° C and then charged into the furnace for spheroidizing annealing; the annealing temperature is 870 ° C, the holding time is 4 h / 100 mm, and the temperature is reduced to 730 ° C at 25 ° C / h and kept for 24 hours, and then the temperature is reduced to 500 ° C at 25 ° C / h and air-cooled out of the furnace; the forging process of steps (8) and (9) is two upsetting, two drawing and two fire forming, and the starting forging temperature is 1050 ° C and the final forging temperature is 800 ° C;
[0076] (10) After annealing, the module is flattened and surface ground;
[0077] (11) The module processed in step (10) is subjected to ultra-fine processing. The ultra-fine processing process includes one quenching and one spheroidizing annealing treatment to prepare a mold steel with high purity and good structural uniformity.
[0078] Example 4
[0079] A method for preparing a novel die-casting die steel comprises the following steps:
[0080] (1) The alloy was prepared according to the element composition of Example 4 in Table 1 above, and the molten steel was melted in a 20T non-vacuum induction furnace at a melting temperature of 1520°C. The slag was pre-made by using a 3T furnace mixed blasting. During the smelting process, slag was added for deoxidation and desulfurization. After the material was cleared, 96% of the slag was removed. Then, slag was added again for slag making, and Al powder was added for diffusion deoxidation. The temperature was raised to 1590°C for sampling and analysis, and the temperature was further raised to above 1640°C before the steel was tapped and sent to a LF furnace.
[0081] (2) After the ladle is placed in the LF station, the temperature is raised and the slag is adjusted. The composition is adjusted according to the sampling results, and carbon powder, Al powder, and Si-Ca powder (m:m=1:1) are added for diffusion deoxidation to maintain a reducing atmosphere. The slag is sampled, the temperature is raised to 1700℃, and the slag is removed by 68%. The steel is then tapped and sent to the VD station. The white slag is kept for 36 minutes during the LF furnace refining period.
[0082] (3) Before the VD furnace is evacuated, 0.5 kg / T of rare earth is placed in the bag. The total evacuation time is 38 minutes, the ultimate vacuum is 130 Pa, the holding time is 15 minutes, the temperature is measured after the vacuum is broken, argon is blown for 15 minutes, the temperature is measured at 1545°C, and the steel is poured;
[0083] (4) The electrode rod is demoulded 4 hours after casting, slowly cooled to 400°C and then put into furnace for annealing. After annealing, the ends of the electrode rod are flattened and the surface is polished. The annealing temperature is 750°C, the holding time is 28h, and the electrode rod is cooled to 500°C at 22°C / h and then air-cooled out of the furnace.
[0084] (5) Placing the electrode rod as an electrode in a protective atmosphere electroslag remelting furnace for secondary remelting and purification to form an electroslag ingot; the protective atmosphere electroslag remelting uses 66# pre-melted slag with a melting rate of 7.0 kg / min. After the electroslag is finished, the furnace is cooled for 98 minutes and then covered with cooling for 76 hours;
[0085] (6) The electroslag ingot is loaded into the furnace for forging within 24 hours after the cover is removed;
[0086] (7) Place the treated steel ingot in a heating furnace, heat it to 500°C at 92°C / h and keep it for 3 hours, then heat it to 850°C at 144°C / h and keep it for 4 hours, and finally heat it to 1250°C at 190°C / h and keep it for 5 hours. After the steel ingot is pulled out of the billet, it is returned to the furnace for high-temperature diffusion at 1300°C for 40 hours, and then the furnace door is opened for 30 minutes or transferred to a low-temperature furnace and kept at 1180°C for 2 hours before being taken out of the furnace for forging;
[0087] (8) The steel ingot is taken out of the furnace, and the intermediate billet is forged and drawn. The intermediate billet is returned to the furnace and kept at 1160°C for 2 hours;
[0088] (9) The intermediate billet is taken out of the furnace for upsetting and drawing, and after forging, it is water-cooled at 3 min / 100 mm. After taking out of the water, it is air-cooled to 350 ° C and then charged into the furnace for spheroidizing annealing; the annealing temperature is 880 ° C, the holding time is 4 h / 100 mm, and the temperature is reduced to 730 ° C at 24 ° C / h and kept for 24 hours, and then the temperature is reduced to 500 ° C at 24 ° C / h and air-cooled out of the furnace; the forging process of steps (8) and (9) is two upsetting, two drawing and two fire forming, and the starting forging temperature is 1050 ° C and the final forging temperature is 800 ° C;
[0089] (10) After annealing, the module is flattened and surface ground;
[0090] (11) The module processed in step (10) is subjected to ultra-fine processing. The ultra-fine processing process includes one quenching and one spheroidizing annealing treatment to prepare a mold steel with high purity and good structural uniformity.
[0091] Test Example 1
[0092] The properties of the die steel for die casting prepared in the above embodiments 1-4 were tested. The organization rating was rated as AS4 according to the sampling and inspection of NADCA-207 North American die casting standard. The banded organization rating was rated as SA1 according to the microscopic inspection method of SEP1614 hot working die steel microscopic inspection and evaluation standard rating chart. The grain size grade was rated as 8 according to the GB / T 6394-2002 metal average grain size determination method. The die steel material prepared by the above embodiment method has excellent resistance to thermal fatigue cracking, high red hardness and high toughness. The transverse unnotched impact toughness is above 400J when the hardness is 48-50HRC, and the V-notch impact is greater than 20J (see Table 2).
[0093] Table 2
[0094]
Claims
1. A method for preparing high-performance die-casting mold steel, characterized in that: The following steps are involved: (1) preparing alloys according to corresponding elemental compositions, melting molten steel in a non-vacuum induction furnace at a melting temperature of 1510-1520°C, adding slag for deoxidation and desulfurization during the melting process, removing slag ≥90% after the material is cleared, then adding slag again to make slag, adding Al powder for diffusion deoxidation, heating to 1560-1590°C for sampling and analysis, further heating to above 1640°C, tapping and entering an LF furnace; (2) After the ladle is placed in the LF station, the temperature is raised and the slag is adjusted. The composition is adjusted according to the sampling results, and carbon powder, Al powder, and Si-Ca powder are added for diffusion deoxidation to maintain a reducing atmosphere. The slag is sampled, the temperature is raised to 1690-1700℃, and the slag removal is ≥60%. The steel is then discharged and sent to the VD station; (3) Before the VD furnace is evacuated, 0.5 kg / T of rare earth is placed in the bag. The total evacuation time is ≥30 min, the ultimate vacuum is ≤133 Pa, and the holding time is ≥10 min. After breaking the vacuum, the temperature is measured, and the argon gas is blown for ≥10 min. The temperature is measured at 1535-1545 ° C, and the steel is poured; (4) The electrode rod is demoulded after 4 hours of casting, slowly cooled to 300-400°C and then put into a furnace for annealing. After annealing, the ends of the electrode rod are flattened and the surface is polished; (5) placing the electrode rod as an electrode in a protective atmosphere electroslag remelting furnace for secondary remelting and purification to form an electroslag ingot; (6) The electroslag ingot is loaded into the furnace for forging within 24 hours after the cover is removed; (7) Place the treated steel ingot in a heating furnace, heat it to 500°C at ≤100°C / h and keep it for 3h, then heat it to 850°C at ≤150°C / h and keep it for 4h, finally heat it to 1250°C at ≤200°C / h and keep it for 5h, after the steel ingot is pulled out of the billet, return to the furnace for high temperature diffusion at 1300°C for 40h, then open the furnace door for 30min or transfer it to a low temperature furnace and keep it at 1180°C for 2h before forging; (8) The steel ingot is taken out of the furnace, and the intermediate billet is forged and drawn. The intermediate billet is returned to the furnace and kept at 1160°C for 1-2 hours; (9) The intermediate billet is taken out of the furnace, upset and drawn to form, and after forging, it is water-cooled at 3min / 100mm. After taking out of the water, it is air-cooled to 350℃ and then loaded into the furnace for spheroidizing annealing; (10) After annealing, the module is flattened and surface ground; (11) The module processed in step (10) is subjected to ultra-fine processing to prepare a mold steel with high purity and good structural uniformity.
2. The preparation method according to claim 1, characterized in that: In step (1), molten steel is melted in a 20T non-vacuum induction furnace, and pre-slag is made using a 3T furnace mixed blasting.
3. The preparation method according to claim 1, characterized in that: In step (2), the white slag is maintained for ≥30 min during the LF furnace refining period.
4. The preparation method according to claim 1, characterized in that: In step (4), the annealing temperature is 700-750°C, the holding time is ≥20h, and the furnace is cooled to 500°C at a rate of ≤30°C / h and then air-cooled.
5. The preparation method according to claim 1, characterized in that: In step (5), protective atmosphere electroslag remelting uses 66# pre-melted slag with a melting rate of 7.0-6.5 kg / min. After the electroslag is finished, the furnace is cooled for ≥90 min and then hood-cooled, and the hood-cooling time is ≥72 h.
6. The preparation method according to claim 1, characterized in that: In step (8) and step (9), the starting forging temperature is ≥1050°C, and the final forging temperature is 800-850°C.
7. The preparation method according to claim 1, characterized in that: In step (9), the annealing temperature is 850-880°C, the holding time is 4h / 100mm, and the temperature is lowered to 730°C at a rate of ≤30°C / h and kept at that temperature for 24 hours, and then the temperature is lowered to 500°C at a rate of ≤30°C / h and air-cooled before being taken out of the furnace.
8. The preparation method according to claim 1, characterized in that: In step (11), the ultra-fine treatment process is a quenching and a spheroidizing annealing treatment.
9. High performance die casting die steel prepared by the method according to any one of claims 1 to 8.
10. The high performance die casting die steel according to claim 9, characterized in that: The element composition of the mold steel includes, by weight percentage: C: 0.30-0.40%, Mn: 0.20-0.60%, Si: ≤0.30%, S: ≤0.002%, P: ≤0.015%, Cr: 4.70-5.50%, Ni: 0.50-0.80%, Ni: 0.50-0.80%, Mo: 2.00-2.40%, V: 0.50-0.70%, Cu: ≤0.20%, Al: ≤0.03%, and the remainder is iron and unavoidable residual elements.