Preparation method and application of Se defect type Fe3Se4 nano spindle structure catalyst
The Se-deficient Fe3Se4 nanospindle structure catalyst was prepared by electrodeposition on a nickel foam substrate, which solved the problems of slow reaction kinetics and high cost in electrocatalytic water splitting devices, and achieved efficient and stable oxygen evolution performance in electrolyzed water.
Patent Information
- Application Number
- CN202411252307.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-10-25
AI Technical Summary
The oxygen evolution reaction (OER) reaction kinetics of the anode of the existing electrocatalytic water splitting device is slow, and the precious metal catalyst has high cost and small reserves, which limits its large-scale application.
By preparing a Se-deficient Fe3Se4 nanospindle structure catalyst, it is synthesized on a nickel foam substrate using an electrodeposition method, and the molar ratio of selenium and iron is adjusted to control the Se defect content to form an efficient electrocatalyst.
It achieves efficient electrolysis of water for oxygen evolution under alkaline conditions, has good catalytic reaction kinetics and stability, low cost, high efficiency, and is superior to the performance of precious metal catalysts.
Smart Images

Figure CN118835262A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material synthesis and electrocatalysis, and specifically relates to a preparation method and application of a Se-deficient Fe3Se4 nano spindle structure catalyst. Background Art
[0002] As a clean energy carrier, hydrogen has the potential to solve the energy crisis. At present, the main method for industrial production of hydrogen is to obtain it through natural gas reforming. Natural gas is a non-renewable energy source, and the process of synthesizing hydrogen will produce greenhouse gas carbon dioxide. In contrast, electrocatalytic water decomposition to produce hydrogen is a sustainable and pollution-free method for hydrogen production, and is considered to be one of the most effective ways to produce high-purity hydrogen. However, the oxygen evolution reaction (OER) occurring at the anode of the electrocatalytic water splitting device involves a complex 4-electron transfer process, and thus exhibits slow reaction kinetics. Precious metal catalysts can accelerate the reaction kinetics and improve the catalytic efficiency, but precious metal catalysts are expensive and have small reserves, which limits their large-scale application. Therefore, it is urgent to develop low-cost, high-catalytic activity, and good stability OER electrocatalysts.
[0003] Transition metal chalcogenides are considered to be electrocatalysts with good performance due to their unique crystal structure and electrocatalytic activity, higher redox activity than their oxides, and advantages such as environmental friendliness and low cost. Among them, iron-based catalysts have attracted widespread attention due to their unique electronic structure and low price. Selenium has a larger ionic radius than sulfur. Among iron-based chalcogenides, iron selenide has better redox performance. The catalytic performance of iron selenide catalysts can be significantly improved by regulating the structure of the catalyst (e.g., doping, designing defective structures, etc.). Summary of the invention
[0004] The purpose of the present invention is to provide a preparation method and application of a Se-deficient Fe3Se4 nanospindle structure catalyst to solve the problems of high price and low efficiency of current water electrolysis catalysts.
[0005] The present invention is specifically implemented by the following technical scheme. According to the preparation method of a Se-deficient Fe3Se4 nanospindle structure catalyst proposed by the present invention, the method comprises the following steps:
[0006] (1) Take a certain amount of SeO2 and iron salt, dissolve them in ultrapure water respectively, and fully dissolve them by ultrasonic treatment to obtain a SeO2 solution of a certain concentration and an iron salt solution of a certain concentration.
[0007] (2) Use a pipette to transfer a certain amount of SeO2 solution and a certain amount of iron salt solution respectively and mix them thoroughly. Adjust the pH value of the mixed solution to control the pH value of the mixed solution within the range of 2.5±0.1.
[0008] (3) Using nickel foam as a working electrode, a saturated calomel electrode (SCE) as a reference electrode, a platinum sheet as a counter electrode, and the mixed solution obtained in step (2) as an electrodeposition solution to form a three-electrode system; using an electrochemical workstation, after connecting the circuit, at room temperature, at a voltage of -0.45 V relative to SCE, Fe3Se4 thin film is electro-deposited on the nickel foam; after the electrodeposition is completed, the nickel foam substrate with Fe3Se4 attached is rinsed with ultrapure water to remove surface impurities, and then placed in a vacuum drying oven and dried at 60°C for 6 hours to obtain a Se-deficient Fe3Se4 nanospindle structure catalyst uniformly covered on the nickel foam substrate.
[0009] Preferably, the iron salt described in step (1) is one of ferrous nitrate, ferrous chloride and ferrous sulfate.
[0010] Preferably, in step (1), the concentration of the SeO2 solution is 0.01-0.02M, and the concentration of the iron salt solution is 0.02-0.1M.
[0011] Preferably, the power of the ultrasonic treatment in step (1) is 720 W and the time is 1 h.
[0012] Preferably, in step (2), the volume ratio of the SeO2 solution to the iron salt solution is 1:1.
[0013] Preferably, the ratio of the iron salt concentration to the SeO2 concentration in the mixed solution obtained in step (2) is 1:1 to 10:1. When ferrous sulfate is used as the iron salt, sulfuric acid solution is used to adjust the pH value of the mixed solution to within the range of 2.5±0.1. When ferrous chloride is used as the iron salt, hydrochloric acid solution is used to adjust the pH value of the mixed solution to within the range of 2.5±0.1. When ferrous nitrate is used as the iron salt, nitric acid solution is used to adjust the pH value of the mixed solution to within the range of 2.5±0.1.
[0014] Preferably, the electrodeposition time in step (3) is 30 to 90 minutes.
[0015] The present invention also provides a Se-deficient Fe3Se4 nanospindle structure catalyst obtained according to the above method and its application in electrocatalysis, especially in electrolysis of water and oxygen evolution under alkaline conditions. The prepared Se-deficient Fe3Se4 nanospindle structure catalyst has a polymer-like spindle morphology, is evenly distributed, has a uniform molding state, and has good stability. In the application of electrolysis of water and oxygen evolution, the catalyst has a high conductivity at 10 mA / cm 2 The overpotential of water electrolysis under current density is only 220mV, and it has a small Tafel slope value (52.1mV / dec), showing good catalytic reaction kinetics. 2It can be used stably for more than 100 hours at a current density of 1.5V, so it has good stability in use. It has good overall water splitting performance at a lower voltage (1.52V), which is better than the performance of the overall water splitting device assembled with a noble metal catalyst (RuO2) at the anode.
[0016] Compared with the prior art, the present invention has obvious advantages and beneficial effects. By means of the above technical solution, the present invention can achieve considerable technical progress and practicality, and has a wide range of utilization value, and has at least the following advantages:
[0017] (1) The present invention uses SeO2 as a selenium source and FeSO4·7H2O as an iron source to prepare a Se-deficient Fe3Se4 nanospindle structure catalyst by an electrodeposition method, and the content of Se defects can be precisely controlled by adjusting the molar ratio of selenium to iron. The preparation method of the present invention is simple, mild, low-cost, and high-efficiency. The prepared Se-deficient Fe3Se4 nanospindle structure catalyst exhibits efficient electrocatalytic water-to-oxygen separation performance, solving the problems of low efficiency and high price of the current electrolytic water-to-oxygen separation catalyst under alkaline conditions.
[0018] (2) The Se-deficient Fe3Se4 catalyst electroprecipitated on the nickel foam substrate of the present invention has a polymer-like spindle morphology, and is evenly distributed and uniformly formed. The lattice fringes of the HRTEM image were analyzed to obtain relatively clear lattice fringes corresponding to the diffraction crystal plane (404) of Fe3Se4, which is similar to the crystal structure of Tm3Se4. The XRD image proved that the synthesized sample is Fe3Se4. As the defect concentration of the electroprecipitated product increases, the Fe content in the Se-deficient Fe3Se4 catalyst increases. 3+ The molar proportion gradually increases with the formation of defect structures. The greater the ratio of FeSO4 concentration to SeO2 concentration, the greater the Se defect concentration in the Se-defective Fe3Se4 catalyst. The greater the Se defect concentration, the better the oxygen evolution performance of the catalyst. When the ratio of FeSO4 concentration to SeO2 concentration in the electroprecipitation mixed solution is 10:1, the Se-defective Fe3Se4 nanospindle structure catalyst synthesized by electroprecipitation has the smallest impedance value, and at 10mA / cm 2 The overpotential of water electrolysis is only 220mV, the Tafel slope is 52.1mV / dec, and the double layer capacitance C dl The value is 1.74mF / cm 2 , showing good catalytic reaction kinetics. The prepared Se-deficient Fe3Se4 nanospindle structure catalyst has a good catalytic reaction kinetics at 100mA / cm 2 The LSV polarization curve was tested without significant changes after being used for about 100 hours at a current density of . The above shows that the Se-deficient Fe3Se4 nanospindle structure catalyst prepared by the present invention has both good electrochemical oxygen evolution performance and good stability.
[0019] (3) The preparation method of the present invention is simple, and can quickly and at low cost obtain Fe3Se4 nanospindle structure catalysts with controllable selenium defect content under mild conditions. The obtained Se-deficient Fe3Se4 nanospindle structure catalyst can effectively decompose water under electrocatalytic conditions, solving the problems of low efficiency and high cost of electrolytic water catalysts under alkaline conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a schematic diagram of the electroplating process.
[0021] Figure 2 The following are the scanning electron microscope image (a) of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Example 1, the TEM image before the stability test using the chronoamperometry (b), and the TEM image after the stability test using the chronoamperometry for 100 hours (c).
[0022] Figure 3 HRTEM images of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Example 1 before (a) and after (b) the stability test using the chronoamperometry for 100 h.
[0023] Figure 4 These are the XRD patterns of the Se-deficient Fe3Se4 nanospindle structure catalysts d-Fe3Se4-3, d-Fe3Se4-2, and d-Fe3Se4-1 prepared in Examples 1 to 3, wherein d-Fe3Se4-1 indicates that the ratio of the FeSO4 concentration to the SeO2 concentration in the electroprecipitation solution is 1:1 (Example 3), d-Fe3Se4-2 indicates that the ratio of the FeSO4 concentration to the SeO2 concentration in the electroprecipitation solution is 5:1 (Example 2), and d-Fe3Se4-3 indicates that the ratio of the FeSO4 concentration to the SeO2 concentration in the electroprecipitation solution is 10:1 (Example 1), and the same applies below.
[0024] Figure 5 These are the XPS graphs of the Se-deficient Fe3Se4 nanospindle structure catalysts d-Fe3Se4-3, d-Fe3Se4-2, and d-Fe3Se4-1 prepared in Examples 1 to 3.
[0025] Figure 6 These are the EPR graphs of the Se-deficient Fe3Se4 nanospindle structure catalysts d-Fe3Se4-3, d-Fe3Se4-2, and d-Fe3Se4-1 prepared in Examples 1 to 3.
[0026] Figure 7It is the LSV curve diagram of the Se-deficient Fe3Se4 nanospindle structure catalysts d-Fe3Se4-3, d-Fe3Se4-2, and d-Fe3Se4-1 prepared in Examples 1 to 3.
[0027] Figure 8 It is the EIS graph of Se-deficient Fe3Se4 nanospindle structure catalysts d-Fe3Se4-3, d-Fe3Se4-2, and d-Fe3Se4-1 prepared in Examples 1 to 3;
[0028] Fig. 9 It is the Tafel slope diagram of the Se-deficient Fe3Se4 nanospindle structure catalysts d-Fe3Se4-3, d-Fe3Se4-2, and d-Fe3Se4-1 prepared in Examples 1 to 3.
[0029] Fig.10 It is the double layer capacitance diagram of the Se-deficient Fe3Se4 nanospindle structure catalysts d-Fe3Se4-3, d-Fe3Se4-2, and d-Fe3Se4-1 prepared in Examples 1 to 3.
[0030] Fig.11 This is the OER stability test graph of the Se-deficient Fe3Se4 nanospindle structure catalyst d-Fe3Se4-3 prepared in Example 1.
[0031] Fig.12 This is a test diagram of the overall water splitting performance of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Example 1.
[0032] Fig.13 This is a test chart of the stability of the overall water splitting performance of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Example 1. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments and drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The present invention is described in detail with specific examples below. If no specific conditions are specified in the following examples, they are all carried out according to conventional conditions or conditions recommended by the manufacturer. The raw materials and reagents used without specifying the manufacturer are all conventional products that can be purchased from the market.
[0035] Embodiment 1:
[0036] (1) Take 0.056 g of SeO2 and dissolve it in 50 mL of ultrapure water. Then take 1.39 g of FeSO4·7H2O and dissolve it in 50 mL of ultrapure water. Ultrasonic treatment is used to fully dissolve them respectively to obtain a SeO2 solution with a concentration of 0.01 M and a FeSO4 solution with a concentration of 0.1 M.
[0037] (2) Use a pipette to transfer 25 mL of SeO2 solution and 25 mL of FeSO4 solution respectively, mix the two thoroughly, and control the pH value of the mixed solution within the range of 2.5±0.1.
[0038] (3) A saturated calomel electrode (SCE) was used as a reference electrode, nickel foam was used as a working electrode, and a platinum sheet was used as a counter electrode to form a three-electrode system. The mixed solution obtained in step (2) was used as an electrochemical precipitation solution. After the circuit was connected, an electrochemical workstation was used to electroprecipitate the Fe3Se4 thin film on the nickel foam at a voltage of -0.45 V relative to SCE for 30 min. The electrochemical precipitation is shown in the figure below: Figure 1 After the electrodeposition is completed, the nickel foam substrate with Fe3Se4 attached is rinsed with ultrapure water to remove surface impurities, and then placed in a vacuum drying oven and dried at 60°C for 6 hours to obtain a Se-deficient Fe3Se4 nanospindle structure catalyst uniformly covering the surface of the nickel foam substrate.
[0039] Electrochemical test process of Se-deficient Fe3Se4 nanospindle structure catalyst: All electrochemical analysis tests were carried out in 1M KOH electrolyte solution using a CHI760E electrochemical analyzer. The analyzer has a traditional three-electrode assembly consisting of a graphite rod, a Hg-HgO electrode, and a nickel foam loaded with Se-deficient Fe3Se4 samples as the counter electrode, reference electrode, and working electrode, respectively. Before the test, oxygen was passed through the electrolyte for 0.5 h to saturate the electrolyte with oxygen, and then linear sweep voltammetry (LSV), cyclic voltammetry (CV), and electrochemical impedance spectroscopy (EIS) tests were performed. The geometric area of the working electrode immersed in the electrolyte was controlled to be 1 cm 2 .
[0040] Figure 2 The SEM images (a) of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Example 1, the TEM image (b) before the stability test using the chronoamperometry, and the TEM image (c) after the stability test using the chronoamperometry for 100 hours. It can be seen from the SEM images that the Se-deficient Fe3Se4 catalyst electroprecipitated on the nickel foam substrate has a polymer-like spindle morphology, with a particle size of about 500-600nm, and is evenly distributed and uniformly formed. Figure 2As can be seen in b and c, the Se-deficient Fe3Se4 nanospindle structure catalyst after ultrasonic treatment presents a multilayer sheet structure in anhydrous ethanol dispersant, but is still distributed in the form of aggregates. Figure 2 By comparing a and b, we can see that at 100 mA cm -2 Before and 100 h after the stability test of the Se-deficient Fe3Se4 catalyst using the chronoamperometry under current density, there was no obvious change in the morphology of the Se-deficient Fe3Se4 catalyst, indicating that the prepared Se-deficient Fe3Se4 nanospindle structure catalyst has good stability.
[0041] Figure 3 This is a high-resolution transmission electron microscopy (HRTEM) image of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Example 1 before (a) and 100 hours after (b) the stability test using the chronoamperometry. By analyzing the lattice fringes in the HRTEM image, clearer lattice fringes corresponding to the diffraction crystal plane (404) of Fe3Se4, which is similar to the Tm3Se4 crystal structure, were obtained.
[0042] Figures 4 to 10 In the figure, d-Fe3Se4-1 indicates that the ratio of FeSO4 concentration to SeO2 concentration in the electroprecipitation solution is 1:1 (Example 3), d-Fe3Se4-2 indicates that the ratio of FeSO4 concentration to SeO2 concentration in the electroprecipitation solution is 5:1 (Example 2), and d-Fe3Se4-3 indicates that the ratio of FeSO4 concentration to SeO2 concentration in the electroprecipitation solution is 10:1 (Example 1). Figure 4 The XRD patterns of the Se-deficient Fe3Se4 nanospindle structure catalysts d-Fe3Se4-3, d-Fe3Se4-2 and d-Fe3Se4-1 prepared in Examples 1 to 3 show that the diffraction peaks of the synthesized Fe3Se4 show several peaks. Through the substitution method of transition metal elements with similar ionic radius, the cubic Tm3Se4 (JCPDS No.51-1483) with good comparison is successfully found in the Jade software atlas library. In the comparison, strong diffraction peaks corresponding to the (hkl) diffraction planes (130), (400) and (404) can be observed. Combined with the crystal distortion of the Se-deficient Fe3Se4, the problem of single peak mismatch occurs. The original single crystal Fe3Se4 was distorted during the electrochemical synthesis process, and a polycrystalline cubic Fe3Se4 was formed on the nickel foam substrate. According to the Goldschmidt method, the distance between ions is divided into ionic radius. As the ionic radius decreases, the unit cell parameters shrink and the peak shifts to the right. 3+ Ions and Fe 2+The ionic radii of the high-spin state are very similar, while the Tm3Se4 (JCPDS No.51-1403) PDF standard card is slightly shifted to the right as a whole, confirming that the synthesized sample is Fe3Se4.
[0043] Figure 5 The XPS graphs of the Se-deficient Fe3Se4 nanospindle structure catalysts d-Fe3Se4-3, d-Fe3Se4-2, and d-Fe3Se4-1 prepared in Examples 1 to 3 show that when the concentrations of FeSO4 and SeO2 are equal in the electroprecipitation mixed solution (Example 3), the corresponding XPS peak spectrum of the electroprecipitation product Fe3Se4 / NF (d-Fe3Se4-1) shows that the Fe 2p region can be deconvoluted to 706.4 eV (2p 3 / 2 , Fe 2+ )、710.2eV(2p 3 / 2 , Fe 3+ ), 712.9eV (sat), and 719.2eV (2p 1 / 2 , Fe 2 + )、722.9eV(2p 1 / 2 , Fe 3+ ), 726.6eV (sat). Among them, Fe 2+ , Fe 3+ By comparison, it can be seen that when the ratio of FeSO4 concentration to SeO2 concentration in the electroprecipitation mixed solution is 5:1 (Example 2), in the XPS peak spectrum of the corresponding electroprecipitation product Fe3Se4 / NF (d-Fe3Se4-2), Fe 2p 3 / 2 and Fe 2p 1 / 2 The XPS spectra of the electrochemical precipitation product (d-Fe3Se4-1) of Example 3 (the ratio of FeSO4 concentration to SeO2 concentration is 1:1) have positive shifts of 0.7eV and 0.8eV. This indicates that with the increase of the ratio of FeSO4 concentration to SeO2 concentration, the formation of Fe3Se4 defects causes changes in the electron energy. In the XPS spectrum of the electrochemical precipitation product (d-Fe3Se4-3) with the best electrochemical performance of 10:1 FeSO4 concentration to SeO2 concentration (Example 1), it can be observed that the 2p 3 / 2 , Fe 2+ and 2p 1 / 2 , Fe 2+ There is a negative shift of 0.8 eV in the XPS spectrum of the electroprecipitation product (d-Fe3Se4-2) of Example 2, and in 2p 3 / 2 , Fe 3+ and 2p 1 / 2 , Fe3+ There was a positive shift of 0.1 eV in the XPS spectrum of the electroprecipitation product (d-Fe3Se4-2) in Example 2. This indicates that as the ratio of the FeSO4 concentration to the SeO2 concentration in the electroprecipitation mixed solution increases, the electroprecipitation product undergoes a Fe 2+ , Fe 3+ The transfer of electronic energy between two ions of different valence states. Figure 5 Figure b shows the high-resolution XPS spectra of the Fe2p region of the electroprecipitated product Fe3Se4 / NF when the ratio of FeSO4 concentration to SeO2 concentration in the electroprecipitated mixed solution is 1:1, 5:1, and 10:1. It can be observed that in the XPS peak spectrum of the electroprecipitated product Fe3Se4 / NF when the ratio of FeSO4 concentration to SeO2 concentration in the electroprecipitated mixed solution is 5:1, the Se 3d region can be deconvoluted to 55.3 eV (Se 3d 5 / 2 )、56.1eV(Se 3d 3 / 2 ) peak. As the ratio of FeSO4 concentration to SeO2 concentration in the mixed solution increases, Se 3d 5 / 2 、Se 3d 3 / 2 All of them have negative shifts, proving that with the change of the concentration ratio of the electroprecipitation solution, the electron energy transfer between the Fe3Se4 phases is accompanied by strong electron interaction. According to the XPS fitting results of Fe3Se4, when the ratio of FeSO4 concentration to SeO2 concentration is 1:1, 5:1, and 10:1, respectively, the Fe in Fe3Se4 2+ with Fe 3+ The ratio of the content of Fe in the synthesized electroprecipitation product is 1.57, 1.29, and 1.03, indicating that with the increase of the defect concentration of the electroprecipitation product, the Fe 3+ The molar proportion of ions also gradually increases with the formation of defect structures.
[0044] Figure 6 The EPR characterization results of the Se-deficient Fe3Se4 nanospindle structure catalysts prepared in Examples 1 to 3. All samples showed symmetrical EPR signals, and g = 2.003 was due to the unpaired electrons at the selenium defect sites. Obviously, the Se-deficient Fe3Se4 catalyst obtained by electroplating when the ratio of FeSO4 concentration to SeO2 concentration was 10:1 (d-Fe3Se4-3, Example 1) had a higher Se defect concentration than other samples.
[0045] Figure 7The polarization curve (LSV) diagram of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Examples 1 to 3. When the ratio of FeSO4 concentration to SeO2 concentration in the electroprecipitation mixed solution is 10:1 (d-Fe3Se4-3, Example 1), the performance of the Se-deficient Fe3Se4 nanospindle structure catalyst synthesized by electroprecipitation is the best. Finally, the electroprecipitation method of 30 minutes was used to electroprecipitate and synthesize the catalyst at 10 mA / cm 2 Se-deficient Fe3Se4 nanospindle structure catalyst was used for water electrolysis with an overpotential of only 220mV.
[0046] Figure 8 This is the EIS graph of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Examples 1 to 3. It can be seen from the graph that when the ratio of FeSO4 concentration to SeO2 concentration in the electroprecipitation mixed solution is 10:1 (d-Fe3Se4-3, Example 1), the electroprecipitation synthesized product has the smallest impedance value.
[0047] Fig. 9 It is the Tafel slope diagram of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Examples 1 to 3; it can be seen from the figure that when the ratio of FeSO4 concentration to SeO2 concentration in the electroprecipitation mixed solution is 10:1 (d-Fe3Se4-3, Example 1), the product synthesized by electroprecipitation has a smaller Tafel slope value (52.1 mV / dec), showing good catalytic reaction kinetics.
[0048] Fig.10 The double layer capacitance diagram of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Examples 1 to 3. The C of the catalysts corresponding to the ratio of FeSO4 concentration to SeO2 concentration of 1:1, 5:1, and 10:1, respectively dl 1.8mFcm -2 、1.65mFcm -2 and 1.74mFcm -2 , indicating that the prepared Se-deficient Fe3Se4 nanospindle structure catalyst has a large electrochemical active area.
[0049] Fig.11 This is the OER stability test diagram of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Example 1 (d-Fe3Se4-3). The catalyst is at 100mA / cm 2 It can be used stably for more than 100 h at a current density of , indicating that the Se-deficient Fe3Se4 nanospindle structure catalyst has good stability.
[0050] Fig.12This is a test diagram of the overall water splitting performance of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Example 1. The Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Example 1 is used as the anode, and the loading amount is 0.25 mg / cm 2 The Pt / C electrode was used as the cathode to assemble a double electrode for water electrolysis testing. It had better overall water splitting performance at a lower voltage (1.52V), which was better than the performance of the overall water splitting device assembled with a noble metal catalyst (RuO2) as the anode.
[0051] Fig.13 This is a test chart of the stability of the overall water splitting performance of the Se-deficient Fe3Se4 nanospindle structure catalyst prepared in Example 1. 2 The stability test of the catalyst was carried out at a current density of , and the catalyst activity did not decay during the test time of 2.5 h, indicating that the Se-deficient Fe3Se4 nanospindle structure catalyst prepared according to the method of the present invention has good stability in use.
[0052] Embodiment 2:
[0053] (1) Take 0.111 g of SeO2 and dissolve it in 50 mL of ultrapure water. Then take 1.39 g of FeSO4·7H2O and dissolve it in 50 mL of ultrapure water. Ultrasonic treatment is used to fully dissolve them to obtain a 0.02 M SeO2 solution and a 0.1 M FeSO4 solution.
[0054] (2) Use a pipette to transfer 25 mL of SeO2 solution and 25 mL of FeSO4 solution respectively, mix the two thoroughly, and control the pH value of the mixed solution within the range of 2.5±0.1.
[0055] (3) Using a saturated calomel electrode (SCE) as a reference electrode, nickel foam as a working electrode, and a platinum sheet as a counter electrode to form a three-electrode system, the mixed solution obtained in step (2) is used as an electrochemical workstation, and after the circuit is connected, the Fe3Se4 thin film is synthesized by electrochemical precipitation on the nickel foam for 30 minutes at a voltage of -0.45V relative to SCE. After the electrochemical precipitation is completed, the nickel foam substrate with Fe3Se4 attached is rinsed with ultrapure water to remove impurities on the surface, and then placed in a vacuum drying oven and dried at 60°C for 6 hours to obtain a Se-deficient Fe3Se4 nanospindle structure catalyst uniformly covered on the surface of the nickel foam substrate.
[0056] The electrochemical performance test process of Se-deficient Fe3Se4 catalyst is the same as that in Example 1.
[0057] Embodiment 3:
[0058] (1) Take 0.111 g of SeO2 and dissolve it in 50 mL of ultrapure water. Then take a certain amount of 0.278 g of FeSO4·7H2O and dissolve it in 50 mL of ultrapure water. Ultrasonic treatment is used to fully dissolve them to obtain a 0.02 M SeO2 solution and a 0.02 M FeSO4 solution.
[0059] (2) Use a pipette to transfer 25 mL of SeO2 solution and 25 mL of FeSO4 solution respectively, mix the two thoroughly, and control the pH value of the mixed solution within the range of 2.5±0.1.
[0060] (3) Using a saturated calomel electrode (SCE) as a reference electrode, nickel foam as a working electrode, and a platinum sheet as a counter electrode to form a three-electrode system, the mixed solution obtained in step (2) is used as an electrochemical precipitation solution, and after connecting the circuit, an electrochemical workstation is used to electroprecipitate the iron selenide film on the nickel foam for 30 minutes at a voltage of -0.45V relative to SCE. After the electroprecipitation is completed, the nickel foam substrate with iron selenide attached is rinsed with ultrapure water to remove impurities on the surface, and then placed in a vacuum drying oven and dried at 60°C for 6 hours to obtain a Se-deficient Fe3Se4 nanospindle structure catalyst uniformly covered on the surface of the nickel foam substrate.
[0061] The electrochemical performance test process of Se-deficient Fe3Se4 catalyst is the same as that in Example 1.
[0062] Embodiment 4:
[0063] (1) Take 0.056 g of SeO2 and dissolve it in 50 mL of ultrapure water. Then take a certain amount of 1.39 g of FeSO4·7H2O and dissolve it in 50 mL of ultrapure water. Ultrasonic treatment is used to fully dissolve them respectively to obtain a SeO2 solution with a concentration of 0.01 M and a FeSO4 solution with a concentration of 0.1 M.
[0064] (2) Use a pipette to transfer 25 mL of SeO2 solution and 25 mL of FeSO4 solution respectively, mix the two thoroughly, and control the pH value of the mixed solution within the range of 2.5±0.1.
[0065] (3) Using a saturated calomel electrode (SCE) as a reference electrode, nickel foam as a working electrode, and a platinum sheet as a counter electrode, a three-electrode system is formed, and the mixed solution obtained in step (2) is used as an electrochemical precipitation solution. After connecting the circuit, an electrochemical workstation is used to electroprecipitate the Fe3Se4 film on the nickel foam for 60 minutes at a voltage of -0.45V relative to SCE. After the electroprecipitation is completed, the nickel foam substrate with Fe3Se4 attached is rinsed with ultrapure water to remove impurities on the surface, and then placed in a vacuum drying oven and dried at 60°C for 6 hours to obtain a Se-deficient Fe3Se4 nanospindle structure catalyst uniformly covered on the surface of the nickel foam substrate.
[0066] The electrochemical performance test process of Se-deficient Fe3Se4 catalyst is the same as that in Example 1.
[0067] Embodiment 5:
[0068] The electrochemical precipitation time was 90 min, and the rest was the same as in Example 4. The electrochemical performance test process of Se-deficient Fe3Se4 catalyst was the same as in Example 1.
[0069] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a Se-deficient Fe3Se4 nanospindle structure catalyst, characterized in that The following steps are involved: (1) taking a certain amount of SeO2 and iron salt, dissolving them in ultrapure water respectively, and subjecting them to ultrasonic treatment to fully dissolve them respectively, to obtain a SeO2 solution of a certain concentration and an iron salt solution of a certain concentration; (2) Use a pipette to transfer a certain amount of SeO2 solution and a certain amount of iron salt solution respectively, mix them thoroughly, and adjust the pH value of the mixed solution to 2.5±0.1; (3) Using nickel foam as a working electrode, a saturated calomel electrode as a reference electrode, and a platinum sheet as a counter electrode, the mixed solution obtained in step (2) is an electrodeposition solution to form a three-electrode system; using an electrochemical workstation, Fe3Se4 thin film is electrodeposited on the nickel foam at a voltage of -0.45 V relative to the saturated calomel electrode; after the electrodeposition is completed, the nickel foam substrate with Fe3Se4 attached is rinsed with ultrapure water to remove surface impurities, and then placed in a vacuum drying oven and dried at 60°C for 6 hours to obtain a Se-deficient Fe3Se4 nanospindle structure catalyst uniformly covered on the nickel foam substrate.
2. The method for preparing the Se-deficient Fe3Se4 nanospindle structure catalyst according to claim 1, characterized in that The iron salt described in step (1) is selected from one of ferrous nitrate, ferrous chloride and ferrous sulfate.
3. The method for preparing the Se-deficient Fe3Se4 nanospindle structure catalyst according to claim 1, characterized in that In step (1), the concentration of SeO2 solution is 0.01-0.02M, and the concentration of iron salt solution is 0.02-0.1M.
4. The method for preparing the Se-deficient Fe3Se4 nanospindle structure catalyst according to claim 1, characterized in that The power of the ultrasonic treatment in step (1) is 720 W and the time is 1 h.
5. The method for preparing the Se-deficient Fe3Se4 nanospindle structure catalyst according to claim 1, characterized in that In step (2), the volume ratio of the SeO2 solution to the iron salt solution is 1:
1.
6. The method for preparing the Se-deficient Fe3Se4 nanospindle structure catalyst according to claim 1, characterized in that The ratio of the iron salt concentration to the SeO2 concentration in the mixed solution obtained in step (2) is 1:1 to 10:
1.
7. The method for preparing the Se-deficient Fe3Se4 nanospindle structure catalyst according to claim 1, characterized in that The time of electrodeposition in step (3) is 30 to 90 minutes.
8. The Se-deficient Fe3Se4 nanospindle structure catalyst obtained by the preparation method according to claim 1.
9. Use of the Se-deficient Fe3Se4 nanospindle structure catalyst as claimed in claim 8 in electrolysis of water for oxygen evolution under alkaline conditions.