Aluminum alloy profile surface oxidation coloring treatment process
Through multi-step processes such as sandblasting, degreasing, alkali etching, acid etching and oxidation coloring treatment, the problems of poor surface gloss and insufficient corrosion resistance of aluminum alloy profiles are solved, and the surface gloss and corrosion resistance are significantly improved.
Patent Information
- Application Number
- CN202410851440.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-25
AI Technical Summary
The surface oxidation and coloring treatment process of aluminum alloy profiles is simple, resulting in poor gloss and insufficient corrosion resistance, which affects the quality of aluminum alloy profiles.
The multi-step process includes shelf cleaning, sandblasting passivation treatment, chemical degreasing, alkali etching treatment, acid etching lightening treatment, neutralization treatment, oxidation coloring treatment and sealing treatment. Through these steps, the surface roughness is improved, corrosion is delayed, and oil stains are removed. and attachments, forming a dense oxide film and enhancing corrosion resistance.
Significantly improves the gloss and corrosion resistance of the aluminum alloy profile surface, enhances the surface density and adhesion, and extends the service life.
Smart Images

Figure CN118835294A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy processing, in particular to a process for oxidation and coloring treatment of the surface of an aluminum alloy profile. Background Art
[0002] Aluminum alloy is the most widely used type of non-ferrous metal structural material in industry. It has been widely used in aviation, aerospace, automobile, machinery manufacturing, shipbuilding and chemical industries. With the rapid development of industrial economy, the demand for aluminum alloy welded structural parts is increasing, which has led to in-depth research on the weldability of aluminum alloy. At present, aluminum alloy is the most widely used alloy. Aluminum alloy has low density, but relatively high strength, close to or exceeding that of high-quality steel, good plasticity, and can be processed into various profiles. It has excellent electrical conductivity, thermal conductivity and corrosion resistance. It is widely used in industry, and its usage is second only to steel. Some aluminum alloys can be heat treated to obtain good mechanical properties, physical properties and corrosion resistance.
[0003] In order to extend the service life of aluminum alloy profiles and increase their color, they need to be oxidized and colored. The basic process of oxidation and coloring is aluminum surface treatment, oxidation, coloring and subsequent hydration and sealing. At present, the process of oxidation and coloring treatment on the surface of aluminum alloy profiles is relatively simple, and the gloss of the aluminum alloy profile surface is poor, and the corrosion resistance is insufficient, which affects the quality of the aluminum alloy profile. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a process for oxidation and coloring treatment of the surface of aluminum alloy profiles, which solves the problem that the current process for oxidation and coloring treatment of the surface of aluminum alloy profiles is relatively simple, the gloss of the surface of the aluminum alloy profiles is poor, the corrosion resistance is insufficient, and the quality of the aluminum alloy profiles is affected.
[0005] To achieve the above object, the present invention provides the following technical solution: a process for oxidation coloring treatment of the surface of aluminum alloy profiles, the treatment process comprising the following steps:
[0006] S1, rack cleaning, S2, sandblasting passivation treatment, S3, chemical degreasing, S4, alkaline etching treatment, S5, acid etching polishing treatment, S6, neutralization treatment, S7, oxidation coloring treatment, S8, sealing treatment, S9, acceptance.
[0007] As a preferred technical solution of the present invention, the rack cleaning in S1 is to place the aluminum alloy profile in clean water for cleaning to remove a large amount of aluminum chips on the surface. After cleaning, take it out and use an air pipe connected to an air compressor to blow air and remove water from the surface of the aluminum alloy profile.
[0008] As a preferred technical solution of the present invention, the sandblasting passivation treatment in S2 cleans the surface of the aluminum alloy profile again, and sandblasts the painted surface to improve the surface roughness, which contributes to the adhesion to a certain extent. Then, the metal surface of the aluminum alloy profile is converted into a non-oxidizing method to delay the corrosion rate of the metal.
[0009] As a preferred technical solution of the present invention, the chemical degreasing in S3 uses a degreasing compound to degrease the aluminum alloy profile treated in S2 to remove oil stains on the surface of the aluminum alloy profile to avoid the influence of the oil stains on the subsequent processes. The workpiece is treated with an alkaline chemical degreasing liquid at 60-65 degrees Celsius for about two minutes to remove oil stains on the surface of the workpiece to ensure uniform alkaline etching and prevent the workpiece from producing spots.
[0010] As a preferred technical solution of the present invention, the alkaline etching treatment in S4 is to place the aluminum alloy profile treated in S3 into a sodium hydroxide solution for alkaline etching to remove the residual oxide film and modified alloy on the surface of the aluminum alloy profile, and alkaline etching for 1-2 minutes in a NaOH (p(NaOH)=40-50G / L) solution at 60 degrees Celsius to remove the residual natural oxide film and modified alloy layer on the surface of the workpiece, and adjust the surface of the substrate to make it uniform. In order to reduce the aluminum oxide flocs precipitated during the corrosion process, ammonium citrate (p=10G / L) can be used as an integrator.
[0011] As a preferred technical solution of the present invention, the acid etching and polishing treatment in S5 uses an acid etching solution with volume concentrations of H2SO4 and HNO3 of 15-20mL / L and 3-5mL / L respectively to neutralize the residual alkali and dissolve the dust attachments to expose the smooth active surface of the workpiece.
[0012] As a preferred technical solution of the present invention, the neutralization treatment in S6 is to put the aluminum alloy profile treated in S5 into a nitric acid solution for cleaning to prevent alkaline corrosion marks and streaks from forming on the profile surface, and to neutralize the sodium hydroxide solution.
[0013] As a preferred technical solution of the present invention, the oxidation coloring treatment in S7 is to place the aluminum alloy profile treated by S6 into a sulfuric acid solution for oxidation treatment, and add sulfosalicylic acid and additives during the treatment process to form a thick and dense oxide film layer on the surface of the aluminum alloy profile. Then, the aluminum alloy profile treated by S7 is placed in ammonia water for neutralization, and then the aluminum alloy profile is taken out and placed in a colorant for coloring treatment.
[0014] As a preferred technical solution of the present invention, the oxidation coloring treatment in S7 is specifically divided into two steps: a. Use the traditional chromate oxidation process to chemically oxidize the aluminum alloy profile in time to avoid re-contamination or generation of a new natural oxide film. The process parameters are: SnSO45-6G / L, NiSO416-18G / L, colorant 9-12G / L, free acid 17-20G / L, pH value = 0.8-1.2, tank temperature 19-21°C, the coloring voltage should be lower than the oxidation voltage, i.e. 14-16V. After this step of treatment, an oxide film with basically up-to-standard corrosion resistance can be obtained. b. The oxidized workpiece is colored black. The formula uses a transition metal compound A as a colorant, KMnO4 as an oxidant, NiSO4 as a catalyst, and HNO3 is added to adjust the pH value to about 5. The workpiece is treated at 80-90 degrees Celsius for about 8 minutes.
[0015] As a preferred technical solution of the present invention, the sealing treatment in S8 is to place the aluminum alloy profile treated in S7 into a sealing compound for sealing treatment. The sealing can be performed by a hydrolysis salt method to produce hydroxide precipitation in the formed membrane pores to block the micropores. The sealing can further improve the surface density and corrosion resistance of the aluminum alloy profile and increase the glossiness of the surface of the aluminum alloy profile.
[0016] Compared with the prior art, the present invention provides a process for oxidation coloring treatment of aluminum alloy profile surface, which has the following beneficial effects:
[0017] The process for oxidation and coloring treatment of the surface of aluminum alloy profiles can improve the surface roughness by sandblasting the painted surface of the aluminum alloy profiles, which has a certain contribution to the adhesion. The method of converting the metal surface of the aluminum alloy profiles into a non-oxidizing method can delay the corrosion rate of the metal. The oil stains on the surface of the aluminum alloy profiles can be removed by degreasing the aluminum alloy profiles. The dust attachments on the surface of the aluminum alloy profiles can be dissolved by acid etching and polishing the aluminum alloy profiles, so that the aluminum alloy profiles reveal a smooth active surface. The density and corrosion resistance of the aluminum alloy profile surface can be further improved by oxidation, coloring and sealing the aluminum alloy profiles, and the glossiness of the aluminum alloy profile surface can be increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The present invention is a process flow chart of the treatment process. DETAILED DESCRIPTION
[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example
[0021] See also Figure 1 In this embodiment: a process for oxidation coloring treatment of aluminum alloy profile surface, the treatment process comprises the following steps:
[0022] S1, shelf cleaning.
[0023] S2, sandblasting passivation treatment.
[0024] S3, chemical degreasing.
[0025] S4, alkaline etching treatment.
[0026] S5, acid etching and polishing treatment.
[0027] S6, neutralization treatment.
[0028] S7, oxidation coloring treatment.
[0029] S8, closed treatment.
[0030] S9, acceptance.
[0031] In a preferred embodiment, the rack cleaning in S1 is to place the aluminum alloy profile in clean water for cleaning to remove a large amount of aluminum chips on the surface. After cleaning, the aluminum alloy profile is taken out and the surface is blown and dehydrated with air using an air pipe connected to an air compressor.
[0032] In a preferred embodiment, the sandblasting passivation treatment in S2 cleans the surface of the aluminum alloy profile again, and sandblasting on the painted surface can improve the surface roughness and contribute to the adhesion to a certain extent. Then, the metal surface of the aluminum alloy profile is converted into a non-oxidizing method to delay the corrosion rate of the metal.
[0033] In a preferred embodiment, the chemical degreasing in S3 uses a degreasing compound to degrease the aluminum alloy profile treated in S2 to remove oil stains on the surface of the aluminum alloy profile to avoid the influence of the oil stains on the subsequent processes. The workpiece is treated with an alkaline chemical degreasing liquid at 60-65 degrees Celsius for about two minutes to remove oil stains on the surface of the workpiece to ensure uniform alkaline etching and prevent the workpiece from producing spots.
[0034] In a preferred embodiment, in the alkaline etching treatment in S4, the aluminum alloy profile treated in S3 is placed in a sodium hydroxide solution for alkaline etching to remove the residual oxide film and modified alloy on the surface of the aluminum alloy profile, and alkaline etching is performed in a 60 degree Celsius NaOH (p(NaOH)=40-50G / L) solution for 1-2 minutes to remove the residual natural oxide film and modified alloy layer on the surface of the workpiece, and adjust the surface of the substrate to make it uniform. In order to reduce the aluminum oxide flocs precipitated during the corrosion process, ammonium citrate (p=10G / L) can be used as an integrator.
[0035] In a preferred embodiment, the acid etching and polishing treatment in S5 uses an acid etching solution with volume concentrations of H2SO4 and HNO3 of 15-20mL / L and 3-5mL / L respectively to neutralize the residual alkali and dissolve the dust attachments to expose the smooth active surface of the workpiece.
[0036] In a preferred embodiment, in the neutralization treatment in S6, the aluminum alloy profile treated in S5 is placed in a nitric acid solution for cleaning to prevent alkaline corrosion marks and streaks from forming on the profile surface, and the sodium hydroxide solution is neutralized.
[0037] In a preferred embodiment, in the oxidation coloring treatment in S7, the aluminum alloy profile treated by S6 is placed in a sulfuric acid solution for oxidation treatment, sulfosalicylic acid and additives are added during the treatment process to form a thick and dense oxide film layer on the surface of the aluminum alloy profile, and then the aluminum alloy profile treated by S7 is placed in ammonia water for neutralization, and then the aluminum alloy profile is taken out and placed in a colorant for coloring treatment.
[0038] In a preferred embodiment, the oxidation coloring treatment in S7 is specifically divided into two steps: a. Use the traditional chromate oxidation process to chemically oxidize the aluminum alloy profile in time to avoid re-contamination or generation of a new natural oxide film. The process parameters are: SnSO45-6G / L, NiSO416-18G / L, colorant 9-12G / L, free acid 17-20G / L, pH value = 0.8-1.2, tank temperature 19-21°C, the coloring voltage should be lower than the oxidation voltage, i.e. 14-16V. After this step of treatment, an oxide film with basically up-to-standard corrosion resistance can be obtained. b. The oxidized workpiece is colored black. The formula uses a transition metal compound A as a colorant, KMnO4 as an oxidant, NiSO4 as a catalyst, and HNO3 is added to adjust the pH value to about 5. The workpiece is treated at 80-90 degrees Celsius for about 8 minutes.
[0039] In a preferred embodiment, the sealing treatment in S8 is to place the aluminum alloy profile treated in S7 into a sealing compound for sealing treatment. The sealing can be performed by a hydrolysis salt method to produce hydroxide precipitation in the formed membrane pores to block the micropores. The sealing can further improve the surface density and corrosion resistance of the aluminum alloy profile and increase the glossiness of the surface of the aluminum alloy profile.
[0040] The working principle and use process of the present invention are as follows: firstly, the aluminum alloy profile is placed in clean water for cleaning to remove a large amount of aluminum chips on the surface, and then the aluminum alloy profile is taken out after cleaning, and then the surface of the aluminum alloy profile is cleaned again, and then the metal surface of the aluminum alloy profile is converted into a non-oxidizing method to delay the corrosion rate of the metal, and then the aluminum alloy profile is degreased with a degreasing compound to remove the oil stains on the surface of the aluminum alloy profile to avoid the influence of the oil stains on the next process, and then the aluminum alloy profile is placed in a sodium hydroxide solution for alkaline etching to remove the residual oxide film and metamorphic alloy on the surface of the aluminum alloy profile, and alkaline etching is carried out in a 60 degree Celsius NaOH (p (NaOH) = 40-50G / L) solution for 1-2min to remove the residual natural oxide film and metamorphic alloy layer on the surface of the workpiece, and the substrate surface is adjusted to make it uniform, in order to reduce the aluminum oxide flocs precipitated during the corrosion process;
[0041] Then, use H2SO4 and HNO3 with volume concentrations of 15-20mL / L and 3-5mL / L respectively to neutralize the residual alkali and dissolve the dust attachments to expose the smooth active surface of the workpiece. Then put the aluminum alloy profile into nitric acid solution for cleaning to prevent alkaline etching marks and streaks on the profile surface, and neutralize the sodium hydroxide solution. Then put the aluminum alloy profile into sulfuric acid solution for oxidation treatment. Sulfosalicylic acid and additives are added during the treatment process to form a thick and dense oxide film layer on the surface of the aluminum alloy profile. Then put the aluminum alloy profile into a closed compound for sealing treatment, and finally the aluminum alloy profile is inspected and accepted.
[0042] In the description of the present invention, the terms "comprises", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "comprising a reference structure" do not exclude the presence of other identical elements in the process, method, article or device comprising the elements. It should be noted that, in this article, relational terms such as "first", "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations.
[0043] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for oxidation and coloring of aluminum alloy profile surface, Features: The treatment process comprises the following steps: S1, shelf cleaning. S2, sandblasting passivation treatment. S3, chemical degreasing. S4, alkaline etching treatment. S5, acid etching and polishing treatment. S6, neutralization treatment. S7, oxidation coloring treatment. S8, closed treatment. S9, acceptance.
2. A process for oxidation coloring treatment of aluminum alloy profile surface according to claim 1, Features: In the above-mentioned rack cleaning in S1, the aluminum alloy profile is placed in clean water for cleaning to remove a large amount of aluminum chips on the surface. After the cleaning is completed, the aluminum alloy profile is taken out and the surface of the aluminum alloy profile is blown and dehydrated with air through an air pipe connected to an air compressor.
3. The process for oxidation coloring treatment of aluminum alloy profile surface according to claim 1, Features: The sandblasting passivation treatment in S2 cleans the surface of the aluminum alloy profile again, and sandblasts the painted surface to improve the surface roughness, which contributes to the adhesion to a certain extent. Then, the metal surface of the aluminum alloy profile is converted into a non-oxidizing method to delay the corrosion rate of the metal.
4. The process for oxidation coloring treatment of aluminum alloy profile surface according to claim 1, Features: The chemical degreasing in S3 uses a degreasing compound to degrease the aluminum alloy profile treated in S2 to remove oil stains on the surface of the aluminum alloy profile to avoid the influence of the oil stains on the subsequent processes. The workpiece is treated with an alkaline chemical degreasing liquid at 60-65 degrees Celsius for about two minutes to remove oil stains on the surface of the workpiece to ensure uniform alkaline etching and prevent the workpiece from producing spots.
5. The process for oxidation coloring treatment of aluminum alloy profile surface according to claim 1, Features: In the alkaline etching treatment in S4, the aluminum alloy profile treated in S3 is placed in a sodium hydroxide solution for alkaline etching to remove the residual oxide film and modified alloy on the surface of the aluminum alloy profile, and alkaline etching is performed in a 60 degree Celsius NaOH (p(NaOH)=40-50G / L) solution for 1-2min to remove the residual natural oxide film and modified alloy layer on the surface of the workpiece, and the substrate surface is adjusted to make it uniform. In order to reduce the aluminum oxide flocs precipitated during the corrosion process, ammonium citrate (p=10G / L) can be used as an integrator.
6. The process for oxidation coloring treatment of aluminum alloy profile surface according to claim 1, Features: The acid etching and polishing treatment in S5 uses an acid etching solution with volume concentrations of H2SO4 and HNO3 of 15-20mL / L and 3-5mL / L respectively to neutralize the residual alkali and dissolve the dust attachments to expose the smooth active surface of the workpiece.
7. The process for oxidation coloring treatment of aluminum alloy profile surface according to claim 1, Features: In the neutralization treatment in S6, the aluminum alloy profile treated in S5 is placed in a nitric acid solution for cleaning to prevent alkaline corrosion marks and streaks from forming on the profile surface, and the sodium hydroxide solution is neutralized.
8. The process for oxidation coloring treatment of aluminum alloy profile surface according to claim 1, Features: The oxidation coloring treatment in S7 is to place the aluminum alloy profile treated by S6 into a sulfuric acid solution for oxidation treatment, add sulfosalicylic acid and additives during the treatment process, so that a thick and dense oxide film layer is formed on the surface of the aluminum alloy profile, and then the aluminum alloy profile treated by S7 is placed in ammonia water for neutralization, and then the aluminum alloy profile is taken out and placed in a colorant for coloring treatment.
9. The process for oxidation coloring treatment of aluminum alloy profile surface according to claim 1, Features: The oxidation coloring treatment in S7 is specifically divided into two steps: a. Use the traditional chromate oxidation process to chemically oxidize the aluminum alloy profile in time to avoid re-contamination or generation of a new natural oxide film. The process parameters are: SnSO45-6G / L, NiSO416-18G / L, colorant 9-12G / L, free acid 17-20G / L, pH value = 0.8-1.2, tank temperature 19-21°C, and the coloring voltage should be lower than the oxidation voltage, i.e. 14-16V. After this step of treatment, an oxide film with basically up-to-standard corrosion resistance can be obtained. b. The oxidized workpiece is colored black. The formula uses a transition metal compound A as a colorant, KMnO4 as an oxidant, NiSO4 as a catalyst, and HNO3 is added to adjust the pH value to about 5. The workpiece is treated at 80-90 degrees Celsius for about 8 minutes.
10. The process for oxidation coloring treatment of aluminum alloy profile surface according to claim 1, Features: The sealing treatment in S8 is to place the aluminum alloy profile treated in S7 into a sealing compound for sealing treatment. The sealing can be performed by a hydrolysis salt method to produce hydroxide precipitation in the formed membrane pores to block the micropores. The sealing can further improve the surface density and corrosion resistance of the aluminum alloy profile and increase the glossiness of the surface of the aluminum alloy profile.