Negative ion antibacterial polyester fiber fabric and preparation method thereof
By using a composite dispersant of hyperdispersant and dispersant and N,N-dihydroxyethyl-3-aminopropionic acid methyl ester, the problems of spinnability and antibacterial performance of negative ion antibacterial polyester fiber fabrics were solved and achieved High negative ion release and good spinning performance, suitable for the clothing field.
Patent Information
- Application Number
- CN202411310921.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-09-20
AI Technical Summary
Existing negative ion antibacterial polyester fiber fabrics have poor spinnability when high-content negative ion powder is added, leading to breakage and clogging, and insufficient negative ion release, which affects the application in the clothing field.
Hyperdispersant Solsperse 32500 and dispersant DISPERS 655 are used as composite dispersants for negative ion powder, combined with N,N-dihydroxyethyl-3-aminopropionic acid methyl ester, and optimized through esterification polycondensation reaction and spinning process. Obtain high suspension rate and dispersion, improve spinning speed and antibacterial performance.
It achieves high negative ion release and good spinning performance. The fabric has excellent hand feel and significant antibacterial effect. It still maintains high negative ion release and antibacterial effect after 40 washes.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of textile fabric preparation, and in particular to a negative ion antibacterial polyester fiber fabric and a preparation method thereof. Background Art
[0002] Polyester fiber, commonly known as "terylene," is a synthetic fiber made by spinning polyester, a product of the polycondensation of organic dibasic acids and diols. Polyester fiber boasts a range of excellent properties, including wrinkle resistance, elasticity, dimensional stability, excellent heat setting, heat and light resistance, and acid resistance. It is widely used in clothing, home textiles, and other fields.
[0003] Negative ion fiber fabrics are a collection of negative ion fibers. These fibers contain materials that release negative ions. When these textiles rub against human skin, they continuously generate negative air ions, which eliminate odors, purify the air, and provide antibacterial and anti-electromagnetic radiation protection, thereby improving the air quality of the microenvironment surrounding the human body. Therefore, negative ion textile fabrics are popular and sought after by the public.
[0004] The preparation methods for negative ion antimicrobial fibers include the following: ① Surface coating modification. During fiber post-processing, a treatment solution containing inorganic particles such as tourmaline that can stimulate negative air ions is fixed to the fiber surface through resin finishing and surface treatment techniques. Negative ion fibers produced by this method have a hard feel and are not wash-resistant. ② Co-spinning. Negative ion fibers are produced by adding negative ion powder to the polymer melt or spinning solution before polymerization or spinning. ③ Copolymerization. Negative ion additives are added during the polymerization process to create chips that release negative ions, which are then spun. The fibers obtained by the latter two methods have a softer feel and are more wash-resistant. However, if high levels of negative ion powder are added, they will not disperse easily in the polymer matrix, resulting in poor spinnability and problems such as breakage and sticking to the roller. Low levels of negative ion addition to the fiber also result in poor negative ion release from the textile.
[0005] Therefore, how to obtain a polyester fabric with a higher amount of negative ion powder added and better spinnability and use it in the clothing field is a problem that still exists in the current research on negative ion antibacterial polyester fiber fabrics. Summary of the Invention
[0006] The purpose of the present invention is to provide a negative ion antibacterial polyester fiber fabric and a preparation method thereof in response to the above-mentioned problems. The polyester fiber fabric obtained by the method has a high amount of released negative ions and good spinning performance, which can increase the spinning speed.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A method for preparing a negative ion antibacterial polyester fiber fabric comprises the following steps: (1) Adding 1 to 2 parts of hyperdispersant Solsperse 32500, 2 to 4 parts of dispersant DISPERS 655, and 40 to 60 parts of negative ion powder to 200 to 300 parts of ethylene glycol by weight, stirring at high speed, and separating and removing undispersed particles by centrifuge to obtain a negative ion slurry; the negative ion powder is a mixture of opal powder and tourmaline powder; (2) 120 parts of terephthalic acid, 20-30 parts of ethylene glycol, and 0.2-0.3 parts of a catalyst were mixed uniformly by weight, added to an esterification polycondensation reactor, and esterified at 230-240° C. for 30-60 minutes; then, at the same temperature, 50-60 parts of anion slurry and 6-9 parts of N,N-dihydroxyethyl-3-aminopropionic acid methyl ester were uniformly added, and both were added within 60 minutes; thereafter, excess ethylene glycol was removed, the temperature of the reaction system was increased to 265-270° C., and the reaction was carried out under low vacuum conditions for 2-3 hours. The discharged material was granulated in a cooling water tank to obtain in-situ polymerized anion polyester chips; (3) After the negative ion polyester chips are dried, they are put into a spinning machine for spinning at a spinning temperature of 300-310° C. and a spinning speed of 3000-4500 m / min. The obtained fibers are woven to obtain negative ion textile fabrics.
[0008] In the present invention, preferably, the weight ratio of the hyperdispersant Solsperse 32500 to the dispersant DISPERS 655 is 1:2.
[0009] In the present invention, preferably, the mass ratio of the opal to the tourmaline is 1 to 5:1.
[0010] In the present invention, preferably, the low vacuum condition refers to the pressure in the reactor being below 100 Pa.
[0011] In the present invention, preferably, the drying treatment of the anion polyester chips is carried out in a vacuum drum, firstly heating to 122-132°C at a rate of 1-2°C / min for pre-crystallization for 2-4 hours; then heating to 145-160°C at a rate of 8-10°C / min and keeping warm for 4-5 hours.
[0012] In the present invention, preferably, the catalyst is antimony trioxide or antimony glycolate.
[0013] In the present invention, preferably, the particle size of the opal powder and the tourmaline powder are both less than 1.000 μm.
[0014] The present invention also protects the negative ion antibacterial polyester fiber fabric prepared by the above preparation method.
[0015] Micron- and nano-scale negative ion powders are in an energy-unstable state due to their small particle size, large surface atomic ratio, large specific surface area, and high surface energy. Therefore, they are easily agglomerated and aggregated, forming secondary particles, which increases the particle size and loses the properties of nanoparticles. If they are not well dispersed during use, they will not be evenly dispersed in the polymer matrix, affecting product quality. Furthermore, they may break or clog filters during melt spinning. The present invention screens and obtains a dispersant suitable for such negative ion powders and the environment in which they are used. The hyperdispersant Solsperse 32500 and the dispersant DISPERS 655 are used as composite dispersants for the negative ion powders. When the two dispersants are combined in a certain mass ratio, their synergistic effect is very significant, resulting in improved suspension rate and dispersibility, and the ability to withstand high-temperature reactions, making them highly suitable for the polyester fiber production of the present invention.
[0016] There are many factors that affect the quality of polyester products during the polyester production process. From the perspective of spinning, the main factors include hue, terminal carboxyl groups, diethylene glycol content and viscosity, among which viscosity has the most significant effect on spinnability. This places higher demands on the quality of the melt, especially the stability of the intrinsic viscosity of the melt. Generally, it is necessary to stabilize at a characteristic viscosity center value of 0.65 and fluctuate within a range of 0.05, and the melt has good spinnability. After adding a dispersant and an anion slurry to the present invention, the polyester sheet is unstable during the molding process and the viscosity drops significantly. By adding a certain amount of N,N-dihydroxyethyl-3-aminopropionic acid methyl ester during the polymerization process, its chain structure is changed, so that the intrinsic viscosity drop during the molding process is reduced, thereby improving spinnability.
[0017] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. The present invention utilizes a hyperdispersant, Solsperse 32500, and a dispersant, DISPERS 655, as a composite dispersant for the negative ion powder, achieving excellent suspension efficiency and dispersibility, and withstanding high-temperature reactions. This composite dispersant is highly suitable for the production of polyester fibers. Compared to conventional polyester fibers, it increases the amount of negative ion powder incorporated while maintaining a high spinning speed, reducing the risk of breakage or filter clogging. The negative ion powder of the present invention effectively fuses with the polymer matrix, exhibiting excellent compatibility with the polymer, without affecting the softness of the polymer fiber, resulting in an excellent feel for the resulting fabric.
[0018] 2. The present invention adds a certain amount of N,N-dihydroxyethyl-3-aminopropionic acid methyl ester during the polymerization process to change the polyester chain structure, so that the intrinsic viscosity drop during the molding process is reduced and maintained within 0.05 dL / g, thereby improving the spinnability.
[0019] 3. The negative ion antibacterial polyester fiber fabric prepared by the present invention has a high negative ion release rate of 5900-8100 / cm 3 , has good antibacterial and health-care effects. After 40 washes, the negative ion release can still be maintained at 3500 / cm 3 above. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. In the embodiments of the present invention, opal powder was purchased from 14639-88-4 of Hubei Shixing Chemical Co., Ltd., and tourmaline powder was purchased from ZX-022D of Zhengxu Mineral Products Processing Plant. Example 1
[0021] A method for preparing a negative ion antibacterial polyester fiber fabric comprises the following steps: (1) By weight, 2 parts of hyperdispersant Solsperse 32500, 2 parts of dispersant DISPERS 655, and 40 parts of negative ion powder are added to 200 parts of ethylene glycol, stirred at high speed, and undispersed particles are removed by centrifuge to obtain a negative ion slurry; the negative ion powder is a mixture of opal powder and tourmaline powder in a mass ratio of 1:1; the particle size of the opal powder and the tourmaline powder is less than 1.000 μm.
[0022] (2) 120 parts of terephthalic acid, 20 parts of ethylene glycol, and 0.2 parts of antimony trioxide were mixed uniformly by weight, added to an esterification polycondensation reactor, and esterified at 230-235° C. for 30 minutes; then, at the same temperature, 60 parts of anion slurry and 6 parts of N,N-dihydroxyethyl-3-aminopropionic acid methyl ester were uniformly added, and both were added within 60 minutes; thereafter, excess ethylene glycol was removed, the temperature of the reaction system was increased to 265-270° C., the reactor was evacuated to a pressure below 100 Pa, and the reaction was carried out for 2 hours. The discharged material was granulated in a cooling water tank to obtain in-situ polymerized anion polyester chips; (3) After the negative ion polyester chips are dried, they are first heated to 122°C at a rate of 1°C / min in a vacuum drum for pre-crystallization for 2 hours; then heated to 145°C at a rate of 8°C / min and kept warm for 4 hours, and then put into a spinning machine for spinning at a spinning temperature of 300-305°C and a spinning speed of 3000 m / min. The obtained fibers are woven to obtain negative ion textile fabrics.
[0023] This example spun the polyester chips at a relatively high speed without any breakage, roller sticking, or filter clogging. The intrinsic viscosity drop of the polyester chip melt (the absolute value of the difference between the intrinsic viscosity of the polyester melt before conveying and the intrinsic viscosity of the polyester melt after extrusion) from before conveying to after extrusion was no more than 0.05 dL / g.
[0024] According to GB / T 30128-2013 "Detection and Evaluation of Negative Ion Generation", the negative ion generation of the prepared fabric is 8100 / cm 3 , after washing 40 times, it can still maintain 4500 pieces / cm 3 The antibacterial effect was tested in accordance with GBT 20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method". The inhibition rates against Escherichia coli, Staphylococcus aureus and Streptococcus albus were 100%, 99% and 99% respectively; after washing 40 times, they still maintained 89%, 88% and 87%. The air permeability was tested in accordance with GB / T5453-1997 "Determination of air permeability of textile fabrics". The sample area was 20cm 2 , the sample pressure difference is set to 100±2Pa, and the air permeability is 569mm / s. Example 2
[0025] A method for preparing a negative ion antibacterial polyester fiber fabric comprises the following steps: (1) By weight, 1.75 parts of hyperdispersant Solsperse 32500, 3.5 parts of dispersant DISPERS 655, and 60 parts of negative ion powder are added to 300 parts of ethylene glycol, stirred at high speed, and undispersed particles are removed by centrifuge to obtain a negative ion slurry; the negative ion powder is a mixture of opal powder and tourmaline powder in a mass ratio of 3:1; the particle size of the opal powder and the tourmaline powder is less than 1.000 μm.
[0026] (2) 120 parts of terephthalic acid, 25 parts of ethylene glycol, and 0.25 parts of ethylene glycol antimony were mixed uniformly by weight, added to an esterification polycondensation reactor, and esterified at 232-236°C for 45 minutes; then, at the same temperature, 55 parts of anion slurry and 8 parts of N,N-dihydroxyethyl-3-aminopropionic acid methyl ester were uniformly added, and both were added within 60 minutes; thereafter, excess ethylene glycol was removed, the temperature of the reaction system was increased to 268-270°C, the reactor was evacuated to a pressure below 100 Pa, and the reaction was carried out for 2.5 hours. The discharged material was granulated in a cooling water tank to obtain in-situ polymerized anion polyester chips; (3) After the negative ion polyester chips are dried, they are first heated to 130°C at a rate of 2°C / min in a vacuum drum for pre-crystallization for 3 hours; then heated to 150°C at a rate of 9°C / min and kept warm for 4.5 hours, and then put into a spinning machine for spinning treatment at a spinning temperature of 305°C and a spinning speed of 3500 m / min. The obtained fibers are woven to obtain negative ion textile fabrics.
[0027] This example spun the polyester chips at a relatively high speed without any breakage, roller sticking, or filter clogging. The intrinsic viscosity drop of the polyester chip melt (the absolute value of the difference between the intrinsic viscosity of the polyester melt before conveying and the intrinsic viscosity of the polyester melt after extrusion) from before conveying to after extrusion was no more than 0.05 dL / g.
[0028] According to GB / T 30128-2013 "Detection and Evaluation of Negative Ion Generation", the negative ion generation of the prepared fabric is 7500 / cm 3 , after washing 40 times, it can still maintain 4000 pieces / cm 3 The antibacterial effect was tested in accordance with GBT 20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method". The inhibition rates against Escherichia coli, Staphylococcus aureus and Streptococcus albus were 100%, 97% and 97% respectively; after washing 40 times, they still maintained 85%, 84% and 83%. The air permeability was tested in accordance with GB / T5453-1997 "Determination of air permeability of textile fabrics". The sample area was 20cm 2 , the sample pressure difference is set to 100±2Pa, and the air permeability is 550mm / s. Example 3
[0029] A method for preparing a negative ion antibacterial polyester fiber fabric comprises the following steps: (1) By weight, 1 part of hyperdispersant Solsperse 32500, 4 parts of dispersant DISPERS 655, and 50 parts of negative ion powder are added to 240 parts of ethylene glycol, stirred at high speed, and undispersed particles are removed by centrifuge to obtain a negative ion slurry; the negative ion powder is a mixture of opal powder and tourmaline powder in a mass ratio of 5:1; the particle size of the opal powder and the tourmaline powder is less than 1.000 μm.
[0030] (2) 120 parts of terephthalic acid, 30 parts of ethylene glycol, and 0.3 parts of ethylene glycol antimony were mixed uniformly by weight, added to an esterification polycondensation reactor, and esterified at 235-240° C. for 60 minutes; then, at the same temperature, 40 parts of anion slurry and 9 parts of N,N-dihydroxyethyl-3-aminopropionic acid methyl ester were uniformly added, and both were added within 60 minutes; thereafter, excess ethylene glycol was removed, the temperature of the reaction system was increased to 270° C., the reactor was evacuated to a pressure below 100 Pa, and the reaction was carried out for 3 hours. The discharged material was granulated in a cooling water tank to obtain in-situ polymerized anion polyester chips; (3) After the negative ion polyester chips are dried, they are first heated to 132°C at a rate of 2°C / min in a vacuum drum for pre-crystallization for 4 hours; then heated to 160°C at a rate of 10°C / min and kept warm for 5 hours, and then put into a spinning machine for spinning at a spinning temperature of 310°C and a spinning speed of 4500m / min. The obtained fibers are woven to obtain negative ion textile fabrics.
[0031] This example spun the polyester chips at a relatively high speed without any breakage, roller sticking, or filter clogging. The intrinsic viscosity drop of the polyester chip melt (the absolute value of the difference between the intrinsic viscosity of the polyester melt before conveying and the intrinsic viscosity of the polyester melt after extrusion) from before conveying to after extrusion was no more than 0.05 dL / g.
[0032] According to GB / T 30128-2013 "Detection and Evaluation of Negative Ion Generation", the negative ion generation of the prepared fabric is 5900 / cm 3 , after washing 40 times, it can still maintain 3500 pieces / cm 3 The antibacterial effect was tested in accordance with GBT 20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method". The inhibition rates against Escherichia coli, Staphylococcus aureus and Streptococcus albus were 96%, 94% and 92% respectively; after washing 40 times, they still maintained 80%, 78% and 76%. The air permeability was tested in accordance with GB / T5453-1997 "Determination of air permeability of textile fabrics". The sample area was 20cm 2 , the sample pressure difference was set to 100±2Pa, and the air permeability was measured to be 578mm / s.
[0033] Comparative Example 1 The hyperdispersant Solsperse 32500 used in step (1) was replaced by an equal amount of dispersant DISPERS 655, and the remaining steps were exactly the same as those in Example 2.
[0034] The spinning process in this comparative example experienced multiple instances of yarn breakage and filter clogging. The intrinsic viscosity drop of the polyester chip melt from before conveying to after extrusion (the absolute value of the difference between the intrinsic viscosity of the polyester melt before conveying and the intrinsic viscosity of the polyester melt after extrusion) was 0.09 dL / g.
[0035] Comparative Example 2 The dispersant DISPERS 655 used in step (1) was replaced by an equal amount of hyperdispersant Solsperse 32500, and the remaining steps were exactly the same as those in Example 2.
[0036] This comparative example exhibited multiple instances of yarn breakage and filter clogging during the spinning process. The intrinsic viscosity drop of the polyester chip melt from before conveying to the end of extrusion (the absolute difference between the intrinsic viscosity of the polyester melt before conveying and the intrinsic viscosity of the polyester melt after extrusion) was 0.12 dL / g.
[0037] Comparative Example 3 The hyperdispersant Solsperse 32500 used in step (1) was replaced by an equal amount of sodium pyrophosphate, and the remaining steps were exactly the same as those in Example 2.
[0038] This comparative example exhibited multiple instances of yarn breakage and filter clogging during the spinning process. The intrinsic viscosity drop of the polyester chip melt from before conveying to the end of extrusion (the absolute difference between the intrinsic viscosity of the polyester melt before conveying and the intrinsic viscosity of the polyester melt after extrusion) was 0.29 dL / g.
[0039] Comparative Example 4 In step (2), no N,N-dihydroxyethyl-3-aminopropionic acid methyl ester was added, and the remaining operation steps were exactly the same as those in Example 2.
[0040] In this comparative example, the spinning process exhibited roller sticking. The intrinsic viscosity drop of the polyester chip melt from before conveying to after extrusion (the absolute value of the difference between the intrinsic viscosity of the polyester melt before conveying and the intrinsic viscosity of the polyester melt after extrusion) was 0.68 dL / g.
[0041] Comparative Example 5 The negative ion slurry and N,N-dihydroxyethyl-3-aminopropionic acid methyl ester in step (2) were quickly added within 10 minutes, and the remaining operating steps were exactly the same as those in Example 2.
[0042] During the spinning process of this comparative example, a few instances of yarn breakage and roller sticking occurred. The intrinsic viscosity drop of the polyester chip melt from before conveying to the end of extrusion (the absolute value of the difference between the intrinsic viscosity of the polyester melt before conveying and the intrinsic viscosity of the polyester melt after extrusion) was 0.25 dL / g.
[0043] From the above preparation test and performance test results, it can be seen that the negative ion antibacterial polyester fiber fabrics prepared in Examples 1-3 have a high negative ion generation rate, which can reach up to 8100 / cm 3 , excellent antibacterial effect, good air permeability of the fabric. After 40 washes, it can still maintain a high amount of negative ion generation and antibacterial effect. The composition of the dispersant in Comparative Examples 1-3 changed, and clogging and broken ends occurred during the spinning process, indicating that the compounding of the dispersant has a greater impact on the dispersion effect, thereby affecting the preventability of the polyester. In Comparative Example 4, N,N-dihydroxyethyl-3-aminopropionic acid methyl ester was not added, and the roller sticking phenomenon occurred, and the intrinsic viscosity dropped significantly, causing instability in production, indicating that N,N-dihydroxyethyl-3-aminopropionic acid methyl ester can significantly improve the thermal stability of polyester. In Comparative Example 5, the addition of the negative ion slurry and N,N-dihydroxyethyl-3-aminopropionic acid methyl ester was done in a relatively short period of time, not gradually dropped, which had a certain impact on the dispersion of the negative ion powder and the copolymerization of the polyester, and ultimately affected the spinnability of the polyester chips.
[0044] The above description is a detailed description of the preferred embodiments of the present invention, but the embodiments are not intended to limit the scope of the patent application of the present invention. Any equivalent changes or modifications completed under the technical spirit suggested by the present invention should fall within the patent scope covered by the present invention.
Claims
1. A method for preparing a negative ion antibacterial polyester fiber fabric, characterized in that: The following steps are involved: (1) By weight, 1-2 parts of superdispersant Solsperse 32500, 2-4 parts of dispersant DISPERS 655, and 40-60 parts of negative ion powder are added to 200-300 parts of ethylene glycol, stirred at high speed, and undispersed particles are separated and removed by a centrifuge to obtain a negative ion slurry; the negative ion powder is a mixture of opal powder and tourmaline powder; (2) 120 parts of terephthalic acid, 20-30 parts of ethylene glycol, and 0.2-0.3 parts of a catalyst are mixed uniformly by weight, added to an esterification polycondensation reactor, and esterified at 230-240° C. for 30-60 minutes; then, 50-60 parts of anion slurry and 6-9 parts of N,N-dihydroxyethyl-3-aminopropionic acid methyl ester are uniformly added at the same temperature, and both are added within 60 minutes; thereafter, excess ethylene glycol is removed, the temperature of the reaction system is increased to 265-270° C., and the reaction is carried out under low vacuum conditions for 2-3 hours, and the discharged material is granulated in a cooling water tank to obtain in-situ polymerized anion polyester chips; (3) After the anion polyester chips are dried, they are put into a spinning machine for spinning at a spinning temperature of 300 to 310° C. and a spinning speed of 3000 to 4500 m / min. The obtained fibers are woven to obtain anion textile fabrics.
2. The preparation method according to claim 1, characterized in that: The weight ratio of the hyperdispersant Solsperse 32500 to the dispersant DISPERS 655 is 1:
2.
3. The preparation method according to claim 1, characterized in that: The mass ratio of the opal to the tourmaline is 1 to 5:
1.
4. The preparation method according to claim 1, characterized in that: The low vacuum condition refers to the pressure in the reactor being below 100 Pa.
5. The preparation method according to claim 1, characterized in that: The drying treatment of the anion polyester chips is carried out in a vacuum drum, firstly heating to 122-132° C. at a speed of 1-2° C. / min for pre-crystallization for 2-4 hours; then heating to 145-160° C. at a speed of 8-10° C. / min for preservation for 4-5 hours.
6. The preparation method according to claim 1, characterized in that: The catalyst is antimony trioxide or antimony glycolate.
7. The preparation method according to claim 1, characterized in that: The particle sizes of the opal powder and tourmaline powder are both less than 1.000 μm.
8. The negative ion antibacterial polyester fiber fabric prepared by the preparation method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Element-negative-ion-releasing sterilizing mite-preventing electromagnetic-wave-preventing fire-retarding nano-grade fabric used in vehicles
CN102400238A
Pearl and anion containing antibacterial underclothes
CN108720092A
Waterborne wood lacquer with super weather resistance and function of releasing negative ions and preparation method thereof
CN109280437A
Preparation method of fabric with functions of releasing negative ions, killing bacteria, removing stink and repelling mosquitoes
CN109706540A
Digital glaze with negative ion function, preparation method thereof, and functional ceramic