By simultaneously spraying fast-crack high-solid content emulsified asphalt and steel slag, and spraying a fog seal layer on them, the problems of low construction efficiency and poor bonding effect in the existing technology are solved, achieving rapid opening to traffic and improving road durability. and water sealing performance.
Patent Information
- Application Number
- CN202411225394.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-10-25
AI Technical Summary
When the existing technology uses steel slag to prepare asphalt simultaneous gravel sealing layer, the construction efficiency is low, resulting in the inability to quickly open traffic, and the bonding effect between steel slag and asphalt is poor, making it difficult to apply to high-grade roads.
Simultaneous spraying of fast-cracked high-solid content emulsified asphalt and steel slag is used to form a steel slag layer through rolling, and a fog seal layer is sprayed on it to simplify the process, improve the demulsification speed and bonding effect, and achieve rapid opening to traffic.
It significantly shortens the construction time, improves the wear resistance and water sealing ability of the road surface, enhances the bonding effect between steel slag and asphalt, ensures the safety and durability of the road, and expands the application scope of steel slag.
Smart Images

Figure CN118835503A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of highway maintenance, and in particular relates to a method for preparing a fast-opening traffic synchronous emulsified asphalt chip seal layer by using steel slag. Background Art
[0002] Steel slag is an industrial solid waste, which is produced in large quantities every year. If it is not treated, it will have an adverse impact on the environment. Although steel slag has a wide range of applications, its utilization rate in my country is still low. The rational use of steel slag to reuse resources can turn waste into treasure and create huge economic benefits. It is an effective way to achieve sustainable development and is of great significance to the country and society.
[0003] Chinese patent CN113250036A discloses a method for preparing asphalt synchronous crushed stone upper sealing layer using steel slag, which includes the following steps: the first step is pretreatment of the base layer; the second step is spraying the first layer of emulsified asphalt, rolling it flat, drying it, and spreading steel slag; the third step is spraying the second layer of emulsified asphalt, rolling it flat, and drying it. This patent adopts a variant asynchronous construction method, first spreading emulsified asphalt to break the emulsion, then spreading stones, and then spreading emulsified asphalt after the stones stick to it. The steps are relatively cumbersome, resulting in low construction efficiency, which leads to long construction time, and traffic cannot be opened quickly, which is easy to cause traffic congestion; at the same time, because the process is not perfect after the emulsified asphalt is spread, the bonding effect between stones and asphalt is poor, and the bonding between steel slag and asphalt is insufficient. After opening the traffic, there may be a risk of stone falling off and scattering, which affects traffic and causes harm to vehicles. Therefore, it can only be used to make low-grade roads and cannot be used on high-grade roads.
[0004] The difference between low-grade and high-grade pavements in the highway industry is that high-grade roads refer to expressways and first-class roads, which generally have faster speeds and larger traffic volumes. Currently, the technology of directly using steel slag as raw material to prepare high-grade pavements and the technology of quickly opening up traffic have yet to be improved. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing an emulsified asphalt chip seal with rapid traffic opening, shortening the time from the preparation of the chip seal to the completion of the traffic opening, using steel slag to prepare the chip seal, making full use of the hardness and wear resistance of the steel slag, greatly improving the wear resistance of the road surface, improving the water sealing coefficient, and increasing the life of the road; recycling steel slag resources, turning waste into treasure, and creating huge economic benefits.
[0006] To achieve the above purpose, the technical solution of the present invention is as follows:
[0007] A method for preparing a synchronous emulsified asphalt chip seal using steel slag comprises the following steps:
[0008] 1) Clean and blow away the debris on the base layer and repair the base layer;
[0009] 2) Spraying fast-cracking high-solid emulsified asphalt and steel slag simultaneously, rolling the emulsified asphalt after initial demulsification, and forming a steel slag layer after molding; the solid content of the high-solid emulsified asphalt is ≥65%;
[0010] 3) Adsorb pumice and spray a mist seal layer on the slag layer. After the mist seal layer is demulsified and formed, a crushed stone seal layer is obtained.
[0011] Preferably, the particle size of the steel slag is 3-10 mm, the crushing value is ≤26%, and the f-CaO content is ≤5%.
[0012] Preferably, the time taken for the initial demulsification of the emulsified asphalt is 5 to 15 minutes.
[0013] Preferably, the temperature of the emulsified asphalt is 40-60°C, preferably 55-60°C.
[0014] Preferably, the thickness of the slag layer is 3 to 10 mm, preferably 3 mm, 5 mm or 9 mm.
[0015] Preferably, the amount of emulsified asphalt sprayed is 1.3-2.3 kg / m according to the thickness of the slag layer. 2 Preferably, for steel slag thickness of 3mm, 5mm or 9mm, the amount of emulsified asphalt sprayed is 1.3-1.6kg / m 2 , 1.4~1.9kg / m 2 , 1.7~2.3kg / m 2 .
[0016] Preferably, the rolling time is 5 to 10 minutes.
[0017] Preferably, the spraying amount of the fog seal layer is 0.2-1.2 kg / m 2 , preferably 0.4kg / m 2 .
[0018] Preferably, the demulsification forming time of the mist seal layer is 0.5 to 1 hour.
[0019] The present invention uses steel slag to prepare a crushed stone seal layer, thereby increasing the life of the pavement, increasing the pavement's water damage resistance, improving the pavement's water sealing capacity, and increasing the application scope of the steel slag, thereby making the utilization rate of the steel slag more sufficient.
[0020] The present invention sprays fast-cracking high-solid emulsified asphalt and steel slag simultaneously, so that the emulsified asphalt and steel slag are mixed together to form a steel slag layer; the emulsified asphalt is prepared with a fast-cracking emulsifier; the solid content of the emulsified asphalt is ≥65%, thereby increasing the viscosity of the emulsified asphalt and greatly improving the emulsification speed of the emulsified asphalt. The use temperature of the emulsified asphalt is increased to 40-60°C, preferably 55-60°C, to improve the emulsification speed of the emulsified asphalt. During construction, a chip seal synchronous seal vehicle is used for construction, which can achieve synchronous and rapid spreading of the emulsified asphalt and steel slag.
[0021] There is no restriction on the source of the steel slag, which is preferably crushed converter drum steel slag with a particle size of 3 to 10 mm and an f-CaO content of ≤5%. By limiting the particle size of the steel slag, the strength of the steel slag particles meets the requirements of road construction. The f-CaO content refers to the free CaO content in the steel slag. The f-CaO content of the steel slag is limited to ≤5%, eliminating the instability of the steel slag, making its performance indicators meet the requirements of industry standards, and preventing the subsequent disintegration and pulverization of the steel slag from causing road surface bulges and cracks. In some embodiments of the present invention, the particle size of the steel slag is 3 to 10 mm, and the f-CaO content is ≤5%. In some embodiments of the present invention, the crushing value of the steel slag is further limited to ≤26%, thereby meeting the requirements of high-grade roads.
[0022] The thickness of the steel slag gravel seal is generally 3-10mm. According to the actual road conditions and steel slag conditions, the preferred thickness of the steel slag gravel seal is 3mm, 5mm, 9mm, etc. According to the thickness of the steel slag gravel seal, the amount of emulsified asphalt to be spread is 1.3-2.3kg / m 2 For the thickness of steel slag gravel seal layer of 3mm, 5mm and 9mm, the amount of emulsified asphalt sprayed is 1.3-1.6kg / m 2 , 1.4 -1.9kg / m 2 , 1.7-2.3kg / m 2 .
[0023] After the emulsified asphalt is initially demulsified, it is introduced into a rubber-wheel roller for rolling. On the one hand, rolling increases the demulsification speed of the raw materials and shortens the molding time; on the other hand, it helps the steel slag to arrange, enhances the bonding between the steel slag and asphalt, increases the bonding effect between the steel slag gravel seal layer and the original road surface, and increases the durability of the steel slag gravel seal layer.
[0024] After the slag layer is formed, spray the mist seal layer on the slag layer, and the mist seal layer is demulsified and formed. The introduction of the mist seal layer also increases the durability and water sealing performance of the slag layer. The spraying amount of the mist seal layer is 0.2-1.2kg / m 2 , preferably 0.4kg / m 2 Traffic can be opened directly after the fog seal layer is demulsified and formed, and the demulsification time is 0.5-1h.
[0025] The original process of emulsified asphalt, steel slag, and emulsified asphalt step-by-step spreading and waiting was simplified to a fast process of emulsified asphalt / steel slag and fog seal. At the same time, fast-cracking high-solid emulsified asphalt and fog seal were selected to increase the demulsification speed, increase construction efficiency, and achieve the purpose of rapid opening of traffic.
[0026] Compared with the existing process, the invention has the following beneficial effects:
[0027] The invention simultaneously sprays fast-cracking high-solid emulsified asphalt and steel slag when preparing the chip seal, which simplifies the process and shortens the time. At the same time, the fast-cracking high-solid emulsified asphalt and the mist seal are selected to increase the demulsification speed, increase the construction efficiency, and achieve the purpose of quickly opening traffic.
[0028] Using steel slag as aggregate for gravel seal can replace commonly used aggregates such as basalt, which is a recycling of resources. The surface of steel slag is microscopically porous. After being sprayed with emulsified asphalt, it is rolled with a rubber-wheeled roller to help the steel slag to align and enhance the adhesion between the steel slag and asphalt. It can effectively integrate the steel slag and emulsified asphalt, enhance the adhesion between the steel slag layer and the original road surface, avoid the risk of stone falling off and scattering, and ensure the durability and safety of the road surface; further, a fog seal layer is added to the steel slag layer to improve the durability and water sealing performance of the gravel seal layer. After the fog seal layer is demulsified and formed, it can be directly opened to traffic without worrying about the impact of the risk of stone falling off and scattering on traffic. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Schematic diagram of a flow chart of an embodiment of the present invention. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with the embodiments and drawings.
[0031] See also Figure 1 , Example 1
[0032] A method for preparing a cape seal using steel slag comprises the following steps:
[0033] 1) Clean and blow away the debris and soil on the road base, and cover the surface layers that need to be protected, such as curbstones and manhole covers, with plastic film;
[0034] 2) Spray fast-cracking high-solid emulsified asphalt and steel slag simultaneously. After the emulsified asphalt is initially demulsified, it is rolled for 10 minutes using a rubber-wheel roller to form a steel slag gravel seal layer. The emulsified asphalt is prepared using Shanghai Invitrogen's fast-cracking emulsifier Indulin AA-63D, with a solid content of 66% and a spreading temperature of 60°C. The steel slag used is from Shanghai Baosteel's converter drum slag, with a particle size range of 8-10mm and an f-CaO content of no more than 5%.
[0035] 3) Adsorb pumice and spray a mist seal layer on the steel slag gravel seal layer, and wait for the mist seal layer to break and form before opening to traffic.
[0036] Example 2
[0037] The difference from Example 1 is that the emulsified asphalt is prepared using the fast-cracking emulsifier IndulinAA-63D produced by Shanghai Invitrogen, with a solid content of 55% and a spreading temperature of 60°C; the steel slag used is the converter drum slag from Shanghai Baosteel, with a particle size range of 8-10mm and an f-CaO content of no more than 5%.
[0038] Example 3
[0039] The difference from Example 1 is that the steel slag used is from the converter drum slag of Anshan Iron and Steel, the particle size range is: 8-10mm, and the f-CaO content does not exceed 5%.
[0040] Comparative Example 1
[0041] The chip seal was prepared using the method disclosed in Chinese patent CN13250036A.
[0042] Comparative Example 2
[0043] The difference from Example 1 is that a medium-crack emulsifier is used for the emulsified asphalt.
[0044] Comparative Example 3
[0045] The difference from Example 2 is that the stone emulsified asphalt is not rolled after spreading.
[0046] Comparative Example 4
[0047] The difference from Example 2 is that no mist seal layer is sprayed.
[0048] Table 1
[0049]
[0050] The construction time includes the time of each step, among which the time of covering and removing the plastic film is calculated as the same time. For the method of sweeping loss rate and gravel shedding rate, please refer to T / CECS G: M54-01-2023 Technical Specification for Highway Maintenance Gravel Seal.
[0051] It can be seen from the data in Table 1 that the most direct improvement of the embodiment of the present invention over the comparative example is in the construction time, the sweeping loss rate indicates the forming speed of the chip seal, the chip shedding rate indicates the bonding effect of the chip seal, and the water permeability coefficient indicates the water sealing effect.
[0052] In comparative example 1, before the process was optimized, the construction time was long, and the molding speed and bonding effect were poor, resulting in poor water sealing effect.
[0053] In comparative example 2, the medium-crack emulsifier was used, and the sweeping loss rate was still relatively large, and a certain amount of gravel fell off, and the construction time was prolonged.
[0054] In comparison example 3, the lack of rolling results in slower stone demulsification and longer forming time. Although the stone shedding rate is low, the later water permeability coefficient will still shorten the pavement life.
[0055] In comparative example 4, the mist seal layer is not sprayed, the sweeping and brushing shedding rate is high, and the water permeability coefficient is high.
Claims
1. A method for preparing an emulsified asphalt chip seal for rapid traffic opening using steel slag, characterized in that: The steps include: 1) Clean and blow away the debris on the base layer and repair the base layer; 2) Spraying fast-cracking high-solid emulsified asphalt and steel slag simultaneously, rolling the emulsified asphalt after initial demulsification, and forming a steel slag layer after molding; the solid content of the high-solid emulsified asphalt is ≥65%; 3) Adsorb pumice and spray a mist seal layer on the slag layer. After the mist seal layer is demulsified and formed, a crushed stone seal layer is obtained.
2. The method according to claim 1, characterized in that: The particle size of the steel slag is 3-10 mm, the crushing value is ≤26%, and the f-CaO content is ≤5%.
3. The method according to claim 1, characterized in that: The temperature of the emulsified asphalt is 40-60°C, preferably 55-60°C.
4. The method according to claim 1, characterized in that: The time required for the initial demulsification of emulsified asphalt is 5 to 15 minutes.
5. The method according to claim 1, characterized in that: The thickness of the slag layer is 3 to 10 mm, preferably 3 mm, 5 mm or 9 mm.
6. The method according to claim 1 or 5, characterized in that: According to the thickness of the slag layer, the amount of emulsified asphalt to be spread is 1.3-2.3 kg / m 2 Preferably, for steel slag thickness of 3mm, 5mm or 9mm, the amount of emulsified asphalt sprayed is 1.3-1.6kg / m 2 , 1.4~1.9kg / m 2 , 1.7~2.3kg / m 2 .
7. The method according to claim 1, characterized in that: The rolling time is 5 to 10 minutes.
8. The method according to claim 1, characterized in that: The spraying amount of the fog seal layer is 0.2~1.2kg / m 2 , preferably 0.4kg / m 2 .
9. The method according to claim 1, characterized in that: The demulsification and forming time of the fog seal layer is 0.5 to 1.0h.