Super wear-resistant and corrosion-resistant composite pipeline and preparation method thereof

Through the composite structure of the inner layer, middle layer and outer layer, combined with ultra-high molecular weight polyethylene, carbon nanotubes, nano-silver, glass fiber and other materials, the problem of insufficient corrosion resistance and wear resistance of composite pipes is solved, and a better High service life and environmentally friendly preparation process.

CN118836337AInactive Publication Date: 2024-10-25FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI

Patent Information

Application Number
CN202410829290.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing composite pipes have deficiencies in corrosion resistance and wear resistance, resulting in reduced service life, and are less targeted during the preparation process.

Method used

It adopts a composite structure of inner layer, middle layer and outer layer. The inner layer is composed of ultra-high molecular weight polyethylene, carbon nanotubes, nano-silver and montmorillonite. The middle layer contains high-density polyethylene, low-density polyethylene and waste polyethylene. Plastic and steel mesh skeleton, the outer layer is composed of polytetrafluoroethylene matrix, fiberglass, polyimide and graphite, and is connected by hot melt adhesive and epoxy resin protective layer to improve corrosion resistance and wear resistance.

Benefits of technology

The corrosion resistance and wear resistance of the composite pipe are significantly improved, the service life is extended, and environmental pollution and resource waste are reduced during the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118836337A_ABST
    Figure CN118836337A_ABST
Patent Text Reader

Abstract

The invention provides a super wear-resistant and corrosion-resistant composite pipeline and a preparation method, and relates to the technical field of composite pipelines, the super wear-resistant and corrosion-resistant composite pipeline comprises an inner layer, a middle layer and an outer layer, the surface of the outer layer is coated with a protective layer, the inner layer comprises ultra-high molecular weight polyethylene, carbon nanotubes, titanium dioxide, nano-silver and montmorillonite, and the middle layer is coated with a protective layer; the middle layer comprises high-density polyethylene, low-density polyethylene, waste polyethylene plastic, butadiene styrene rubber and kaolin, the outer layer comprises a polytetrafluoroethylene matrix, glass fibers, polyimide, aluminum oxide, graphite and an ultraviolet light absorber, the protective layer is an epoxy resin protective layer, and a steel mesh framework is further arranged in the middle layer; starting from the use condition of the pipeline, the composite structure of the outer layer, the middle layer and the inner layer is adopted, the outer layer faces an external corrosion environment, the corrosion resistance of the outer layer is enhanced, the outer layer has certain wear resistance, the inner layer faces an environment where the inner layer is in contact with a medium, the wear resistance of the inner layer is enhanced, and the overall pertinence is good; therefore, the corrosion resistance and the wear resistance of the pipeline are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite pipelines, and in particular to a super wear-resistant and corrosion-resistant composite pipeline and a preparation method thereof. Background Art

[0002] With the continuous improvement of industrial level, PE and PVC plastic pipes are constantly replacing metal pipes and are widely used in building water supply, building drainage, urban water supply, drainage and other fields. The pipes are favored by people because of their light weight, no rust, low cost and easy installation, but the current PE pipes cannot meet the demand in terms of mechanical properties, pressure resistance, impact resistance, wear resistance and water permeability, so composite pipes came into being. Composite pipes are combined by combining various materials to enhance the performance of the pipes.

[0003] Due to the enhanced performance of the composite pipe, its applicable scope and environment are more severe. Therefore, during the use of the composite pipe, problems such as poor corrosion resistance and poor wear resistance still occur, which reduces the service life of the composite pipe. At the same time, in the preparation process of the composite pipe, it is usually to improve the comprehensive performance of the composite pipe, and the specificity is relatively low. Therefore, the present invention proposes a super wear-resistant and corrosion-resistant composite pipe and a preparation method to solve the problems existing in the prior art. Summary of the invention

[0004] In view of the above problems, the purpose of the present invention is to propose a super wear-resistant and corrosion-resistant composite pipe and a preparation method. The super wear-resistant and corrosion-resistant composite pipe and the preparation method have the advantages of good targeting, improve the corrosion resistance and wear resistance of the composite pipe, and can solve the problems existing in the prior art.

[0005] To achieve the purpose of the present invention, the present invention is implemented by the following technical scheme: a super wear-resistant and corrosion-resistant composite pipe and a preparation method thereof, comprising an inner layer, an intermediate layer and an outer layer, wherein the inner layer, the intermediate layer and the outer layer are connected by a hot melt adhesive layer, and a protective layer is sprayed on the surface of the outer layer, wherein the inner layer comprises the following raw materials in parts by weight: 80-90 parts of ultra-high molecular weight polyethylene, 1-3 parts of carbon nanotubes, 2-4 parts of titanium dioxide, 3-5 parts of nano silver and 4-8 parts of montmorillonite, and the intermediate layer comprises the following raw materials in parts by weight: The outer layer comprises the following raw materials in parts by weight: 65-80 parts of polytetrafluoroethylene matrix, 5-10 parts of glass fiber, 5-10 parts of polyimide, 3-5 parts of alumina, 3-5 parts of graphite, 4-5 parts of ultraviolet absorber, the protective layer is an epoxy resin protective layer, and a steel mesh skeleton is also provided in the middle layer.

[0006] A further improvement is that the inner layer and the outer layer both comprise the following raw materials in parts by weight: 2 to 3 parts of antioxidant, 3 to 4 parts of plasticizer and 2 to 3 parts of cross-linking agent.

[0007] A further improvement is that the inner layer further comprises the following raw materials in parts by weight: 3 to 5 parts of coupling agent and 3 to 5 parts of dispersant.

[0008] A further improvement is that the cross-linking agent is one of benzoyl peroxide and dicumyl peroxide.

[0009] A further improvement is that the antioxidant is one of antioxidant 1010, antioxidant 1076, and antioxidant 168.

[0010] A further improvement is that the plasticizer is one of epoxy soybean oil, dibutyl phthalate and tributyl citrate.

[0011] A method for preparing a super wear-resistant and corrosion-resistant composite pipeline comprises the following steps:

[0012] Step 1: Material preparation

[0013] Accurately weigh all raw materials, including ultra-high molecular weight polyethylene, carbon nanotubes, titanium dioxide, nanosilver, montmorillonite, high-density polyethylene, low-density polyethylene, waste polyethylene plastics, styrene-butadiene rubber and kaolin, polytetrafluoroethylene matrix, glass fiber, polyimide, alumina, graphite, UV absorbers, antioxidants, plasticizers and crosslinkers, coupling agents and dispersants;

[0014] Step 2: Preparation of the middle layer

[0015] Add high-density polyethylene, low-density polyethylene, waste polyethylene plastic, styrene-butadiene rubber and kaolin into a high-speed mixer and mix them. The mixing time is 20 to 40 minutes and the mixer speed is 800 to 1200 rpm / min. Then, add the mixed raw materials into an extruder, extrude them through the extruder, and composite them with the steel mesh skeleton synchronously.

[0016] Step 3: Preparation of the inner layer

[0017] Ultra-high molecular weight polyethylene, carbon nanotubes, titanium dioxide, nano-silver and montmorillonite are added into a high-speed mixer and mixed for 10 minutes at a mixer speed of 600 rpm / min, and then antioxidants, plasticizers, cross-linking agents, coupling agents and dispersants are added and mixed for 20 minutes at a mixer speed of 1300 rpm / min, and then the mixed raw materials are added into an extruder and extruded by the extruder;

[0018] Step 4: Preparation of the outer layer

[0019] Add polytetrafluoroethylene matrix, glass fiber, polyimide, alumina, graphite, ultraviolet absorber, antioxidant, plasticizer and crosslinking agent into a high-speed mixer and mix them. The mixing time is 15 minutes and the mixer speed is 800 rpm / min. Then, add the mixed raw materials into an extruder and extrude them into a mold by the extruder.

[0020] Step 5: Pipeline Composite and Post-processing

[0021] The inner layer and the middle layer, and the middle layer and the outer layer are connected in sequence using hot melt adhesive to obtain a composite pipe, and then a layer of epoxy resin protective layer is sprayed on the surface of the outer layer to complete the preparation and obtain an ultra-wear-resistant and corrosion-resistant composite pipe.

[0022] A further improvement is that in step three, before using the montmorillonite, the montmorillonite is organically modified by an ion exchange reaction method.

[0023] The beneficial effects of the present invention are as follows: based on the usage of the pipeline, the present invention adopts a composite structure of an outer layer, an intermediate layer and an inner layer. Facing the external corrosive environment, polytetrafluoroethylene with good corrosion resistance is selected as the matrix, and glass fiber, polyimide, alumina, graphite and ultraviolet absorption are used to improve the comprehensive performance of the outer layer. For the intermediate layer, its pressure resistance, corrosion resistance and wear resistance are guaranteed. Furthermore, the inner layer selects ultra-high molecular weight polyethylene, and is supplemented with carbon nanotubes, titanium dioxide, nano-silver and montmorillonite. While strengthening the wear resistance of the inner side of the composite isolated pipeline, it has certain corrosion resistance. Therefore, the composite pipeline provided by the present invention has good corrosion resistance and wear resistance, and improves the service life of the composite pipeline. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the preparation method steps of the present invention. DETAILED DESCRIPTION

[0025] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0026] The raw materials used in the following examples were obtained through conventional commercial channels. The ultraviolet absorber was phenyl salicylate, the molecular weight of the ultra-high molecular weight polyethylene was more than 1.5 million, and the density of the high-density polyethylene was 0.950 g / cm 3 , the density of low-density polyethylene is 0.910g / cm 3The source of waste polyethylene plastic is screened and crushed waste polyethylene plastic powder purchased from the market. The carbon nanotubes are single-walled carbon nanotubes with a particle size of 2nm. The average particle size of titanium dioxide is 25nm. The epoxy resin protective layer is sprayed on the surface by electrostatic spraying. The coupling agent is a silane coupling agent and the dispersant is a polyvinyl alcohol dispersant.

[0027] Embodiment 1

[0028] according to Figure 1 As shown, this embodiment proposes a super wear-resistant and corrosion-resistant composite pipe, including an inner layer, a middle layer and an outer layer, the inner layer, the middle layer and the outer layer are connected by a hot-melt adhesive layer, and the surface of the outer layer is sprayed with a protective layer, that is, the structure of the composite pipe has a total of six layers, namely protective layer-outer layer-hot-melt adhesive layer-middle layer-hot-melt adhesive layer-inner layer, the inner layer comprises the following raw materials in parts by weight: 90 parts of ultra-high molecular weight polyethylene, 1 part of carbon nanotubes, 2 parts of titanium dioxide, 3 parts of nano silver and 4 parts of montmorillonite, the middle layer comprises the following raw materials in parts by weight: 60 parts of high-density polyethylene, 10 parts of low-density polyethylene, and waste polyethylene The outer layer comprises the following raw materials in parts by weight: 65 parts of polytetrafluoroethylene matrix, 10 parts of glass fiber, 10 parts of polyimide, 5 parts of alumina, 5 parts of graphite, 5 parts of ultraviolet absorber, the protective layer is an epoxy resin protective layer, and a steel mesh skeleton is also provided in the middle layer. The inner and outer layers both comprise the following raw materials in parts by weight: 3 parts of antioxidant, 3 parts of plasticizer and 2 parts of cross-linking agent, the inner layer also comprises the following raw materials in parts by weight: 5 parts of coupling agent and 5 parts of dispersant, the cross-linking agent is benzoyl peroxide, the antioxidant is antioxidant 1010, and the plasticizer is epoxy soybean oil.

[0029] A method for preparing a super wear-resistant and corrosion-resistant composite pipeline comprises the following steps:

[0030] Step 1: Material preparation

[0031] Accurately weigh all raw materials, including ultra-high molecular weight polyethylene, carbon nanotubes, titanium dioxide, nanosilver, montmorillonite, high-density polyethylene, low-density polyethylene, waste polyethylene plastics, styrene-butadiene rubber and kaolin, polytetrafluoroethylene matrix, glass fiber, polyimide, alumina, graphite, UV absorbers, antioxidants, plasticizers and crosslinkers, coupling agents and dispersants;

[0032] Step 2: Preparation of the middle layer

[0033] High-density polyethylene, low-density polyethylene, waste polyethylene plastics, styrene-butadiene rubber and kaolin are added into a high-speed mixer for mixing, the mixing time is 40 minutes and the mixer speed is 800 rpm / min, and then the mixed raw materials are added into an extruder, extruded through the extruder, and composited with the steel mesh skeleton synchronously;

[0034] Step 3: Preparation of the inner layer

[0035] Ultra-high molecular weight polyethylene, carbon nanotubes, titanium dioxide, nano-silver and montmorillonite are added into a high-speed mixer and mixed for 10 minutes at a mixer speed of 600 rpm / min, and then antioxidants, plasticizers, crosslinking agents, coupling agents and dispersants are added and mixed for 20 minutes at a mixer speed of 1300 rpm / min, and then the mixed raw materials are added into an extruder and extruded by the extruder, and before the montmorillonite is used, the montmorillonite is organically modified by an ion exchange reaction method;

[0036] Step 4: Preparation of the outer layer

[0037] Add polytetrafluoroethylene matrix, glass fiber, polyimide, alumina, graphite, ultraviolet absorber, antioxidant, plasticizer and crosslinking agent into a high-speed mixer and mix them. The mixing time is 15 minutes and the mixer speed is 800 rpm / min. Then, add the mixed raw materials into an extruder and extrude them into a mold by the extruder.

[0038] Step 5: Pipeline Composite and Post-processing

[0039] The inner layer and the middle layer, and the middle layer and the outer layer are connected in sequence using hot melt adhesive to obtain a composite pipe, and then a layer of epoxy resin protective layer is sprayed on the surface of the outer layer to complete the preparation and obtain an ultra-wear-resistant and corrosion-resistant composite pipe.

[0040] In this embodiment, the extruder is a single-screw machine, the processing temperature of the single-screw machine is 250° C., and the screw speed is 100 r / min.

[0041] Embodiment 2

[0042] according to Figure 1As shown, this embodiment proposes a super wear-resistant and corrosion-resistant composite pipe, including an inner layer, an intermediate layer and an outer layer, the inner layer, the intermediate layer and the outer layer are connected by a hot melt adhesive layer, the surface of the outer layer is sprayed with a protective layer, the inner layer comprises the following raw materials in parts by weight: 80 parts of ultra-high molecular weight polyethylene, 3 parts of carbon nanotubes, 4 parts of titanium dioxide, 5 parts of nano silver and 8 parts of montmorillonite, the intermediate layer comprises the following raw materials in parts by weight: 40 parts of high-density polyethylene, 25 parts of low-density polyethylene, 15 parts of waste polyethylene plastic, 15 parts of styrene-butadiene rubber and 5 parts of kaolin, The outer layer comprises the following raw materials in parts by weight: 80 parts of polytetrafluoroethylene substrate, 5 parts of glass fiber, 5 parts of polyimide, 3 parts of aluminum oxide, 3 parts of graphite, and 4 parts of ultraviolet absorber. The protective layer is an epoxy resin protective layer. A steel mesh skeleton is also provided in the middle layer. The inner and outer layers both comprise the following raw materials in parts by weight: 2 parts of antioxidant, 4 parts of plasticizer, and 3 parts of cross-linking agent. The inner layer also comprises the following raw materials in parts by weight: 3 parts of coupling agent and 3 parts of dispersant. The cross-linking agent is diisopropyl peroxide, the antioxidant is antioxidant 1076, and the plasticizer is dibutyl phthalate.

[0043] A method for preparing a super wear-resistant and corrosion-resistant composite pipeline comprises the following steps:

[0044] Step 1: Material preparation

[0045] Accurately weigh all raw materials, including ultra-high molecular weight polyethylene, carbon nanotubes, titanium dioxide, nanosilver, montmorillonite, high-density polyethylene, low-density polyethylene, waste polyethylene plastics, styrene-butadiene rubber and kaolin, polytetrafluoroethylene matrix, glass fiber, polyimide, alumina, graphite, UV absorbers, antioxidants, plasticizers and crosslinkers, coupling agents and dispersants;

[0046] Step 2: Preparation of the middle layer

[0047] High-density polyethylene, low-density polyethylene, waste polyethylene plastic, styrene-butadiene rubber and kaolin are added into a high-speed mixer for mixing. The mixing time is 20 minutes and the mixer speed is 1200 rpm / min. The mixed raw materials are then added into an extruder, extruded through the extruder, and composited with a steel mesh skeleton synchronously.

[0048] Step 3: Preparation of the inner layer

[0049] Ultra-high molecular weight polyethylene, carbon nanotubes, titanium dioxide, nanosilver and montmorillonite are added into a high-speed mixer and mixed for 10 minutes at a mixer speed of 600 rpm / min, and then antioxidants, plasticizers, crosslinking agents, coupling agents and dispersants are added and mixed for 20 minutes at a mixer speed of 1300 rpm / min, and then the mixed raw materials are added into an extruder and extruded by the extruder. In step three, before using the montmorillonite, the montmorillonite is organically modified by an ion exchange reaction method;

[0050] Step 4: Preparation of the outer layer

[0051] Add polytetrafluoroethylene matrix, glass fiber, polyimide, alumina, graphite, ultraviolet absorber, antioxidant, plasticizer and crosslinking agent into a high-speed mixer and mix them. The mixing time is 15 minutes and the mixer speed is 800 rpm / min. Then, add the mixed raw materials into an extruder and extrude them into a mold by the extruder.

[0052] Step 5: Pipeline Composite and Post-processing

[0053] The inner layer and the middle layer, and the middle layer and the outer layer are connected in sequence using hot melt adhesive to obtain a composite pipe, and then a layer of epoxy resin protective layer is sprayed on the surface of the outer layer to complete the preparation and obtain an ultra-wear-resistant and corrosion-resistant composite pipe.

[0054] In this embodiment, the extruder is a single-screw machine, the processing temperature of the single-screw machine is 280° C., and the screw speed is 120 r / min.

[0055] Embodiment 3

[0056] according to Figure 1As shown, this embodiment proposes a super wear-resistant and corrosion-resistant composite pipe, including an inner layer, an intermediate layer and an outer layer, the inner layer, the intermediate layer and the outer layer are connected by a hot melt adhesive layer, the surface of the outer layer is sprayed with a protective layer, the inner layer comprises the following raw materials in parts by weight: 85 parts of ultra-high molecular weight polyethylene, 2 parts of carbon nanotubes, 3 parts of titanium dioxide, 4 parts of nano silver and 6 parts of montmorillonite, the intermediate layer comprises the following raw materials in parts by weight: 50 parts of high-density polyethylene, 18 parts of low-density polyethylene, 13 parts of waste polyethylene plastic, 13 parts of styrene-butadiene rubber and 5.5 parts of kaolin, the outer layer The invention comprises the following raw materials in parts by weight: 73 parts of polytetrafluoroethylene matrix, 7 parts of glass fiber, 6 parts of polyimide, 4 parts of aluminum oxide, 4 parts of graphite, 4.5 parts of ultraviolet absorber, the protective layer is an epoxy resin protective layer, a steel mesh skeleton is also provided in the middle layer, the inner layer and the outer layer both comprise the following raw materials in parts by weight: 2.5 parts of antioxidant, 3.5 parts of plasticizer and 2.5 parts of cross-linking agent, the inner layer also comprises the following raw materials in parts by weight: 4 parts of coupling agent and 4 parts of dispersant, the cross-linking agent is diisopropyl peroxide, the antioxidant is antioxidant 168, and the plasticizer is tributyl citrate.

[0057] A method for preparing a super wear-resistant and corrosion-resistant composite pipeline comprises the following steps:

[0058] Step 1: Material preparation

[0059] Accurately weigh all raw materials, including ultra-high molecular weight polyethylene, carbon nanotubes, titanium dioxide, nanosilver, montmorillonite, high-density polyethylene, low-density polyethylene, waste polyethylene plastics, styrene-butadiene rubber and kaolin, polytetrafluoroethylene matrix, glass fiber, polyimide, alumina, graphite, UV absorbers, antioxidants, plasticizers and crosslinkers, coupling agents and dispersants;

[0060] Step 2: Preparation of the middle layer

[0061] Add high-density polyethylene, low-density polyethylene, waste polyethylene plastic, styrene-butadiene rubber and kaolin into a high-speed mixer and mix them. The mixing time is 30 minutes and the mixer speed is 1000 rpm / min. Then, add the mixed raw materials into an extruder, extrude them through the extruder, and composite them with the steel mesh skeleton synchronously.

[0062] Step 3: Preparation of the inner layer

[0063] Ultra-high molecular weight polyethylene, carbon nanotubes, titanium dioxide, nanosilver and montmorillonite are added into a high-speed mixer and mixed for 10 minutes at a mixer speed of 600 rpm / min, and then antioxidants, plasticizers, crosslinking agents, coupling agents and dispersants are added and mixed continuously for 20 minutes at a mixer speed of 1300 rpm / min, and then the mixed raw materials are added into an extruder and extruded by the extruder. Before the montmorillonite is used, the montmorillonite is organically modified by an ion exchange reaction method, that is, the sodium ions between the montmorillonite layers are replaced by organic cations, such as long-chain alkyl ammonium salts, by an ion exchange reaction to enhance its compatibility with the polymer;

[0064] Step 4: Preparation of the outer layer

[0065] Add polytetrafluoroethylene matrix, glass fiber, polyimide, alumina, graphite, ultraviolet absorber, antioxidant, plasticizer and crosslinking agent into a high-speed mixer and mix them. The mixing time is 15 minutes and the mixer speed is 800 rpm / min. Then, add the mixed raw materials into an extruder and extrude them into a mold by the extruder.

[0066] Step 5: Pipeline Composite and Post-processing

[0067] The inner layer and the middle layer, and the middle layer and the outer layer are connected in sequence using hot melt adhesive to obtain a composite pipe, and then a layer of epoxy resin protective layer is sprayed on the surface of the outer layer to complete the preparation and obtain an ultra-wear-resistant and corrosion-resistant composite pipe.

[0068] In this embodiment, the extruder is a single-screw machine, the processing temperature of the single-screw machine is 295° C., and the screw speed is 140 r / min.

[0069] In combination with Example 1, Example 2 and Example 3, the ultra-wear-resistant and corrosion-resistant composite pipe provided by the present invention adopts a combination of an inner layer, an intermediate layer and an outer layer. First, based on the intermediate layer, a steel skeleton plastic pipe is adopted, with polyethylene as the matrix, and a steel mesh skeleton is matched. The steel mesh skeleton is formed by continuous winding and welding. It has the effect of pressure resistance and corrosion resistance, so that the pipeline can withstand higher pressure and weight load. Specifically, for the matrix, a combination of high-density polyethylene and low-density polyethylene is adopted to improve the processing performance of the mixture, so that the product is easier to form, and further waste polyethylene plastics, kaolin and styrene-butadiene rubber are added. The introduction of waste polyethylene plastics can reduce environmental pollution and waste of resources. The addition of styrene-butadiene rubber can improve the elasticity and impact resistance of the intermediate layer, and at the same time can also improve the wear resistance of the material. Kaolin improves the stability of the mixture, thereby ensuring the performance of the intermediate layer itself.

[0070] Secondly, for the inner layer, since the inner side of the composite pipe is used for the transmission of the medium, it is necessary to strengthen the wear resistance of the inner side of the composite pipe. Then the present invention uses ultra-high molecular weight polyethylene as the matrix, which has excellent wear resistance and impact resistance, and then supplemented with carbon nanotubes, titanium dioxide, nano-silver and montmorillonite. Carbon nanotubes, titanium dioxide, montmorillonite and nano-silver are mixed with ultra-high molecular weight polyethylene as reinforcing materials to improve the corrosion resistance of the inner layer. Thus, the wear resistance of the inner layer of the composite pipe is strengthened and its certain corrosion resistance is guaranteed.

[0071] Finally, the outer layer is usually exposed to the external environment and is susceptible to corrosion, so its corrosion resistance needs to be enhanced. Therefore, the present invention uses polytetrafluoroethylene as the main material, supplemented by glass fiber, polyimide, alumina, graphite and ultraviolet absorber. Polytetrafluoroethylene itself is a very excellent corrosion-resistant material, and its mechanical strength and heat resistance are improved by glass fiber while maintaining its corrosion resistance. Polyimide, alumina and graphite are used as functional additives to enhance the performance of the outer layer while maintaining its corrosion resistance, making it more suitable for various complex and harsh application environments. Correspondingly, a layer of epoxy resin protective layer is sprayed on the surface of the outer layer, which has certain corrosion resistance. Therefore, the present invention targets the application characteristics of the pipeline and conducts targeted enhancement to provide a super wear-resistant and corrosion-resistant composite pipeline to meet the growing demand.

[0072] Secondly, the composite pipes prepared in Example 1, Example 2 and Example 3 were tested for corrosion resistance and wear resistance. The test was conducted by cutting test samples from the prepared composite pipes and using the test samples for testing. The wear resistance was tested using a friction and wear testing machine. The parameters of the testing machine were: sliding speed of 1 m / s, load of 1 MPa, and sliding distance of 9000 m, as shown in the following table:

[0073]

[0074] In comparison, the wear coefficient of the wear-resistant polyethylene single pipe purchased on the market is 0.41. The wear resistance of the composite pipes prepared in Examples 1, 2 and 3 is significantly improved.

[0075] Its corrosion resistance is measured by placing it in a 1 mol / L hydrochloric acid solution and a 1 mol / L sodium hydroxide solution for 12 hours, and then calculating the weight loss, as shown in the following table:

[0076] Embodiment 1 Embodiment 2 Embodiment 3 Acid immersion weight loss rate (%) 1.24 1.18 0.95 Alkali leaching weight loss rate (%) 1.41 1.33 1.25

[0077] In comparison, the weight loss rate of the corrosion-resistant polyethylene single pipe purchased on the market is 3.4% for acid immersion and 4.5% for alkali immersion. The corrosion resistance of the composite pipes prepared in Examples 1, 2 and 3 is significantly improved.

[0078] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the framework and scope of application of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A super wear-resistant and corrosion-resistant composite pipe, comprising an inner layer, an intermediate layer and an outer layer, wherein the inner layer, the intermediate layer and the outer layer are connected by a hot melt adhesive layer, characterized in that: The surface of the outer layer is sprayed with a protective layer, the inner layer comprises the following raw materials in parts by weight: 80-90 parts of ultra-high molecular weight polyethylene, 1-3 parts of carbon nanotubes, 2-4 parts of titanium dioxide, 3-5 parts of nano silver and 4-8 parts of montmorillonite, the middle layer comprises the following raw materials in parts by weight: 40-60 parts of high-density polyethylene, 10-25 parts of low-density polyethylene, 12-15 parts of waste polyethylene plastics, 12-15 parts of styrene-butadiene rubber and 5-6 parts of kaolin, the outer layer comprises the following raw materials in parts by weight: 65-80 parts of polytetrafluoroethylene matrix, 5-10 parts of glass fiber, 5-10 parts of polyimide, 3-5 parts of aluminum oxide, 3-5 parts of graphite and 4-5 parts of ultraviolet absorber, the protective layer is an epoxy resin protective layer, and a steel mesh skeleton is also provided in the middle layer.

2. The super wear-resistant and corrosion-resistant composite pipeline according to claim 1 is characterized in that: The inner layer and the outer layer both comprise the following raw materials in parts by weight: 2 to 3 parts of antioxidant, 3 to 4 parts of plasticizer and 2 to 3 parts of cross-linking agent.

3. The super wear-resistant and corrosion-resistant composite pipeline according to claim 1 is characterized in that: The inner layer further comprises the following raw materials in parts by weight: 3 to 5 parts of coupling agent and 3 to 5 parts of dispersant.

4. The super wear-resistant and corrosion-resistant composite pipeline according to claim 2 is characterized in that: The cross-linking agent is one of benzoyl peroxide and dicumyl peroxide.

5. The super wear-resistant and corrosion-resistant composite pipeline according to claim 2, characterized in that: The antioxidant is one of antioxidant 1010, antioxidant 1076, and antioxidant 168.

6. The super wear-resistant and corrosion-resistant composite pipeline according to claim 2, characterized in that: The plasticizer is one of epoxidized soybean oil, dibutyl phthalate and tributyl citrate.

7. A method for preparing a super wear-resistant and corrosion-resistant composite pipe according to claim 1, characterized in that: The following steps are involved: Step 1: Material preparation Accurately weigh all raw materials, including ultra-high molecular weight polyethylene, carbon nanotubes, titanium dioxide, nanosilver, montmorillonite, high-density polyethylene, low-density polyethylene, waste polyethylene plastics, styrene-butadiene rubber and kaolin, polytetrafluoroethylene matrix, glass fiber, polyimide, alumina, graphite, UV absorbers, antioxidants, plasticizers and crosslinkers, coupling agents and dispersants; Step 2: Preparation of the middle layer Add high-density polyethylene, low-density polyethylene, waste polyethylene plastic, styrene-butadiene rubber and kaolin into a high-speed mixer and mix them. The mixing time is 20 to 40 minutes and the mixer speed is 800 to 1200 rpm / min. Then, add the mixed raw materials into an extruder, extrude them through the extruder, and composite them with the steel mesh skeleton synchronously. Step 3: Preparation of the inner layer Ultra-high molecular weight polyethylene, carbon nanotubes, titanium dioxide, nano-silver and montmorillonite are added into a high-speed mixer and mixed for 10 minutes at a mixer speed of 600 rpm / min, and then antioxidants, plasticizers, cross-linking agents, coupling agents and dispersants are added and mixed for 20 minutes at a mixer speed of 1300 rpm / min, and then the mixed raw materials are added into an extruder and extruded by the extruder; Step 4: Preparation of the outer layer Add polytetrafluoroethylene matrix, glass fiber, polyimide, alumina, graphite, ultraviolet absorber, antioxidant, plasticizer and crosslinking agent into a high-speed mixer and mix them. The mixing time is 15 minutes and the mixer speed is 800 rpm / min. Then, add the mixed raw materials into an extruder and extrude them into a mold by the extruder. Step 5: Pipeline Composite and Post-processing The inner layer and the middle layer, and the middle layer and the outer layer are connected in sequence using hot melt adhesive to obtain a composite pipe, and then a layer of epoxy resin protective layer is sprayed on the surface of the outer layer to complete the preparation and obtain an ultra-wear-resistant and corrosion-resistant composite pipe.

8. The method for preparing a super wear-resistant and corrosion-resistant composite pipe according to claim 7, characterized in that: In the step three, before using the montmorillonite, the montmorillonite is organically modified by an ion exchange reaction method.

Citation Information

Patent Citations

  • High-pressure-bearing ultrahigh-molecular-weight polyethylene reinforced composite pipe structure

    CN102478130A

  • Method for improving wear resistance and strength of ultrahigh-molecular-weight polyethylene

    CN104817751A

  • Compound tubular product of banded carbon fiber polyethylene of long fiber

    CN205424133U

  • Three -layer is compound tubular product of cohering ethylene carbon fiber altogether

    CN205504233U

  • Enhancement mode polyethylene and compound drain pipe of polytetrafluoroethylene

    CN208090087U

Cited By

  • Preparation method of explosion-proof thickened wear-resistant rubber and plastic pipe