Negative active material as well as preparation method and application thereof

By using a core-shell structure negative active material in lithium-ion batteries and using a carbon layer doped with metal elements to wrap elemental phosphorus, the problems of volume expansion of phosphorus and dissolution of intermediate products are solved, and the cycle stability and battery life of lithium-ion batteries are improved. chemical properties.

CN118841545APending Publication Date: 2024-10-25ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410860385.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

The huge volume expansion of phosphorus in lithium-ion batteries and the dissolution behavior of the intermediate lithium polyphosphide lead to a reduction in Coulombic efficiency and seriously damage long-term cycle stability. It is difficult to effectively alleviate this problem with existing technology.

Method used

The anode active material uses a core-shell structure, in which the core is elemental phosphorus and the shell is a carbon layer of doped metal elements Zr, Zn, Co, Fe, Ce, and La. Through the calcination preparation method of MOF materials, high conductivity and The hard carbon layer with high lithium ion transmission efficiency synergistically improves the specific capacity and dynamic performance of the material.

Benefits of technology

It effectively alleviates the volume change of phosphorus, improves the specific capacity and kinetic properties of the negative electrode material, enhances the cycle stability and electrochemical performance of lithium-ion batteries, and reduces structural damage during charge and discharge.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841545A_ABST
    Figure CN118841545A_ABST
Patent Text Reader

Abstract

The invention discloses a negative electrode active material and a preparation method and application thereof, and belongs to the technical field of new energy. The negative electrode active material provided by the invention comprises a core and a shell wrapping the core, the core comprises elemental phosphorus; the core accounts for 20-80% of the mass of the negative electrode active material; the shell is a carbon layer doped with a metal element A, a metal element B and N; the metal element A comprises at least one of Zr, Zn, Co and Fe; the metal element B comprises at least one of Ce, La and Pr. The negative electrode active material provided by the invention can effectively relieve the problems of great volume change and poor cycle performance when the phosphorus elementary substance is used as a negative electrode. The invention also provides a preparation method and application of the negative electrode active material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy technology, and in particular to a negative electrode active material and a preparation method and application thereof. Background Art

[0002] Phosphorus has a high theoretical specific capacity (2596 mAh / g) and a suitable lithiation potential (0.7 V vs Li + / Li), is a fast-charging, high-capacity lithium-ion battery negative electrode material with great application potential. However, the huge volume expansion (~300%) of the phosphorus negative electrode after lithiation will lead to the instability of the solid electrolyte interface. What's worse, the dissolution behavior of the intermediate product lithium polyphosphide will lead to a decrease in Coulomb efficiency and continuous capacity decay, which seriously damages the long-cycle stability.

[0003] How to alleviate the volume change of phosphorus during the process of lithium insertion and extraction and improve its practicality as a negative electrode active material is a technical problem that urgently needs to be solved in this field. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a negative electrode active material that can effectively alleviate the volume change during the lithium insertion and extraction process.

[0005] The invention also provides a method for preparing the negative electrode active material.

[0006] The invention also provides application of the negative electrode active material.

[0007] According to an embodiment of the first aspect of the present invention, there is provided a negative electrode active material, the negative electrode active material comprising a core and a shell wrapping the core;

[0008] The core includes elemental phosphorus; the core accounts for 20 to 80% of the mass percentage of the negative electrode active material;

[0009] The shell is a carbon layer doped with metal element A, metal element B and N; the metal element A includes at least one of Zr, Zn, Co and Fe; the metal element B includes at least one of Ce, La and Pr.

[0010] The negative electrode active material according to the embodiment of the present invention has at least the following beneficial effects:

[0011] In the negative electrode active material provided by the present invention, the shell is actually a multi-doped hard carbon layer. Due to the special design of the shell material, it has high conductivity and high lithium ion transmission efficiency. While achieving high capacity and excellent kinetics, it can effectively alleviate the volume expansion of elemental phosphorus in the core. Specifically,

[0012] Doping with N elements will change the electronic structure of the shell hard carbon layer, enhance its conductivity, and improve its kinetic performance and rate performance; it will introduce more reversible defects and lithium ion reaction active sites, so that the shell layer also has a certain capacity, which can ultimately improve the specific capacity of the resulting negative electrode active material.

[0013] Compared with doping with a single metal element, doping the shell material with two metal elements can produce a synergistic effect between the two metal elements. Specifically, the conductivity of the shell material can be further improved; the introduction of lanthanide metals (metal element B) can increase the oxygen vacancy content of the shell material, thereby increasing the lithium ion active sites and reducing the Li + Diffusion barrier is conducive to lithium ion transmission; doping with rare earth elements (metal element B) can also improve the crystallinity of the shell, making the electron mobility and conductivity of the shell higher than that of a single metal element. The above performance can only be achieved when metal element A and metal element B work together, that is, metal element A has a significant promoting effect on the performance of metal element B.

[0014] According to some embodiments of the present invention, in the shell, the molar ratio of A to B is 1.8 to 2.1:1; for example, it may be about 2:1.

[0015] According to some embodiments of the present invention, the metal element A is Zn.

[0016] According to some embodiments of the present invention, the metal element B is Ce.

[0017] According to some embodiments of the present invention, the mass percentage of the core to the negative electrode active material is 40-60%, for example, specifically about 50%.

[0018] According to an embodiment of the second aspect of the present invention, a method for preparing the negative electrode active material is provided, the method comprising the following steps:

[0019] S1. preactivating the elemental phosphorus;

[0020] S2. The product of step S1, salt A containing the metal element A, salt B containing the metal element B and a N-containing ligand are mixed in a solvent to obtain a precursor;

[0021] S3. calcining the precursor in an atmosphere containing ammonia.

[0022] The mechanism of the preparation method is as follows:

[0023] In step S1, elemental phosphorus is activated to generate surface defects or specific groups.

[0024] In step S2, metal element A in salt A serves as the metal center of the MOF material, and is assembled with the N-containing ligand to form a cage-shaped MOF material, and metal element B is doped into the MOF material; by combining with defects or specific groups on the surface of elemental phosphorus, the product obtained in step S1 is finally encapsulated.

[0025] Step S3 is the process of carbonizing the MOF material and also the process of supplementing nitrogen doping.

[0026] The preparation method according to the embodiment of the present invention has at least the following beneficial effects:

[0027] Since the preparation method adopts all the technical solutions of the negative electrode active material of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.

[0028] Furthermore, the unique conductive network of MOF materials is utilized to generate metal-doped hard carbon after calcination, which can improve the overall conductivity of the material. The wrapping effect of MOF materials is also utilized to form a good core-shell structure.

[0029] The present invention adopts a preparation method of calcining MOFs to obtain a shell layer, so that the shell layer retains the large specific surface area, high porosity and abundant unsaturated sites of MOFs. Since MOFs have excellent hydrophilicity, the shell layer also inherits the above advantages to a certain extent, which is beneficial to improving the dispersibility and slurry stability of the obtained negative electrode active material in water, and is beneficial to prolonging the storage time (no sedimentation). Combined with the doping element B and the N element, the B element is a heavy rare earth element with greater hydrophilicity, and the N element can form hydrogen bonds with water. The three act synergistically, greatly improving the hydrophilicity of the material, which can also improve the subsequent coating of convex black spots; further, in MOFs The introduction of multi-metal nodes can improve the efficiency of electron transfer. For example, the introduction of Ce in MOF (Zn and Ce both have two valence states, and their electronegativity is greater than that of lithium, which can store electrons and avoid lithium precipitation). Therefore, the shell formed by calcining MOFs not only improves the overall conductivity, but also enhances the storage capacity of lithium through synergistic effects, which is beneficial to improving the charging and high and low temperature discharge performance of the battery cell and reducing swelling. The formation of Zn-P bonds (P is the core, and Zn is the metal element A doped in the shell) can serve as a charge and lithium ion transfer channel to prevent lithium ions from staying on the shell and not entering the core, which is beneficial to fading and rate charging and discharging.

[0030] Furthermore, although the nitrogen-containing ligand will introduce a certain amount of nitrogen doping into the shell, if calcined in an inert gas such as nitrogen, the N in the nitrogen-containing ligand will evaporate out of the system in the form of ammonia or the like; therefore, an ammonia atmosphere is required in step S3 to ensure sufficient N doping to fully exert the synergistic effect between A, B and N.

[0031] According to some embodiments of the present invention, in step S1, the elemental phosphorus includes at least one of red phosphorus, black phosphorus, blue phosphorus and purple phosphorus.

[0032] According to some embodiments of the present invention, in step S1, the pre-activation method includes at least one of acid oxidation treatment, plasma treatment and chemical grafting treatment. Thereby, defects can be generated on the surface of the elemental phosphorus, or at least one of amination, carboxylation and oxidation can be achieved on the surface of the elemental phosphorus. Furthermore, the above activation can cause a tight bond between the MOF generated in step S2 and the elemental phosphorus, thereby improving the core-shell bonding strength. Furthermore, the bonding mode between the core and shell includes at least one of electrostatic action, covalent bond, hydrogen bond and van der Waals force. Ultimately, the above-mentioned special core-shell structure and the connection mode between the core and shell can effectively alleviate the volume change of the negative electrode active material during the charge and discharge process and the structural damage caused by the volume change.

[0033] According to some embodiments of the present invention, in step S1, the pre-activation method is selected from plasma treatment, wherein the plasma treatment includes oxygen plasma.

[0034] The parameters of the oxygen plasma must satisfy at least one of the following parameters:

[0035] (1) Oxygen pressure ≤ 0.01 MPa;

[0036] (2) The discharge voltage is 12 to 17 kV, for example, specifically about 15 kV;

[0037] (3) The discharge power is 600-700 W, for example, about 650 W;

[0038] (4) The treatment time is 1.5 to 2.5 hours, for example, specifically about 2 hours.

[0039] According to some embodiments of the present invention, in step S2, the salt A includes at least one of chloride, nitrate and acetate.

[0040] More specifically, in step S2, the salt A includes at least one of zinc nitrate, zirconium nitrate, cobalt nitrate and iron nitrate. Unless otherwise specified, the salt A or salt B provided by the present invention can be an anhydrous structure or a structure containing crystal water commonly used in industry.

[0041] According to some embodiments of the present invention, in step S2, the salt B includes at least one of chloride, nitrate and acetate.

[0042] More specifically, in step S2, the salt B includes at least one of cerium nitrate, praseodymium nitrate and lanthanum nitrate.

[0043] According to some embodiments of the present invention, in step S2, the molar ratio of salt A to salt B is 1.8-2.2:1; for example, it can be specifically about 2:1.

[0044] According to some embodiments of the present invention, in step S2, the N-containing ligand includes at least one of dimethylimidazole, diaminoterephthalic acid and urea.

[0045] According to some embodiments of the present invention, in step S2, the molar ratio of the salt A to N in the nitrogen-containing ligand is 4 to 10:1, for example, about 5:1, 6:1, 7:1, 8:1 or about 9:1.

[0046] According to some embodiments of the present invention, in step S2, the solvent includes at least one of N,N-dimethylformamide, water and methanol.

[0047] According to some embodiments of the present invention, step S2 includes:

[0048] S2a. The product obtained in step S1, salt A, salt B and part of the solvent are mixed to obtain a dispersion A;

[0049] Mixing the N-containing ligand and the remaining solvent to obtain a dispersion B;

[0050] S2b. The dispersion A and the dispersion B are mixed and reacted.

[0051] According to some embodiments of the present invention, in step S2a, in the dispersion A, the mass ratio of the salt A to the volume ratio of part of the solvent is 1 g: 10-25 mL. For example, it can be about 1 g: 11 mL, 1 g: 13 mL, 1 g: 15 mL, 1 g: 20 mL or about 1 g: 23 mL.

[0052] According to some embodiments of the present invention, in step S2a, the volume ratio of part of the solvent to the remaining solvent is 1.5 to 2.5:1, for example, specifically about 2:1.

[0053] According to some embodiments of the present invention, in step S2 (i.e., step S2b), the temperature of the mixing reaction is room temperature. Unless otherwise specified, room temperature in the present invention refers to 15-40°C, for example, specifically about 25°C.

[0054] According to some embodiments of the present invention, in step S2, the duration of the mixing reaction is 20 to 30 hours, for example, 24 to 25 hours.

[0055] According to some embodiments of the present invention, step S2 further includes washing and drying performed in sequence after the mixing reaction. The detergent used for washing includes methanol. The drying temperature is 60 to 100° C., for example, specifically about 80° C. The drying time is 10 to 15 hours, for example, specifically 12 to 13 hours.

[0056] According to some embodiments of the present invention, in step S2, the obtained precursor has a core-shell structure, wherein the core includes elemental phosphorus and the shell is a MOF material.

[0057] According to some embodiments of the present invention, in step S3, the maximum calcination temperature is ≥ 1300°C.

[0058] According to some embodiments of the present invention, in step S3, the insulation time at ≥1300°C is about 5 to 10 hours; for example, it can be about 7 hours, 8 hours or about 9 hours.

[0059] According to some embodiments of the present invention, in step S3, the flow rate of the atmosphere is 0.05 to 0.13 m / s. For example, it can be about 0.06 m / s, 0.08 m / s, 0.1 m / s or about 0.12 m / s. By adjusting the flow rate of ammonia during the calcination process, the content of N in the obtained negative electrode active material can be adjusted, and ultimately the conductivity, hydrophilicity and other related properties of the obtained shell can be affected.

[0060] According to some embodiments of the present invention, in step S3, the heating rate of the calcination is:

[0061] (1) When the temperature is less than 500°C, the heating rate is 4 to 6°C / min, for example, about 5°C / min;

[0062] (2) When 500°C≤temperature<800°C, the heating rate is 0.5-1.5°C / min, for example, specifically about 1°C / min;

[0063] (3) When 800°C≤temperature<1300°C, the heating rate is 0.4-0.6°C / min, for example, specifically about 0.5°C / min.

[0064] According to some embodiments of the present invention, in step S3, the cooling after calcination is natural cooling, that is, no air cooling, water cooling or the like is performed.

[0065] According to an embodiment of the third aspect of the present invention, there is provided a lithium ion battery, the lithium ion battery comprising a battery cell; the battery cell comprises a positive electrode, a negative electrode and a separator separating the positive electrode and the negative electrode;

[0066] The raw material for preparing the negative electrode includes the negative electrode active material.

[0067] Since the lithium-ion battery adopts all the technical solutions of the negative electrode active material of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment.

[0068] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±2%, for example, about 100 is actually 100±2%×100.

[0069] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values ​​2 and 3.

[0070] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0072] Figure 1 1 is the EIS spectrum of the negative electrode active materials obtained in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0073] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0074] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0075] Example 1

[0076] In this example, a negative electrode active material that can be used to prepare a lithium-ion battery is prepared. Specifically, the negative electrode active material has a core-shell structure, the core is elemental phosphorus, and the shell is a carbon layer doped with Zn, Ce and N, wherein the molar ratio of Zn to Ce is 2:1; the mass ratio of phosphorus (core) to the total negative electrode active material is 50%.

[0077] The preparation method of the negative electrode active material is as follows:

[0078] S1. The red phosphorus powder is surface treated with oxygen plasma under the following treatment conditions: oxygen pressure less than 0.01 MPa, discharge voltage of 15 kV, plasma discharge power of 650 W, and time of 2 h; thereby obtaining pre-activated red phosphorus.

[0079] S2. The pre-activated red phosphorus and part of methanol, zinc nitrate hexahydrate, and cerium nitrate hexahydrate are mixed together to obtain a solution A; and 2-methylimidazole is dispersed in the solution (remaining methanol) to obtain a solution B;

[0080] Among them, the molar ratio of zinc nitrate hexahydrate, cerium nitrate hexahydrate and 2-methylimidazole is 4:2:0.25; the mass volume ratio of zinc nitrate hexahydrate and part of methanol is 3g:40mL; the volume ratio of part of methanol and remaining methanol is 2:1; the amount of red phosphorus added after treatment ensures that the mass ratio of core / active negative electrode material is 50% (calculated without loss of C, N, P, A and B). Solution B is quickly added to solution A and stirred vigorously at room temperature (500r / min) for 24h. After washing with methanol several times, it is vacuum dried at 80℃ for 12h to obtain the precursor of the negative electrode material P@MOF-(Zn4,Ce2,N 0.5 );

[0081] S3. The precursor P@MOF-(Zn4,Ce2,N 0.5 ) calcining at high temperature in an NH3 atmosphere with an NH3 flow rate of 0.1 m / s to obtain a negative electrode active material;

[0082] The heating program of this step is as follows: when room temperature ≤ furnace temperature < 500°C, heat at a rate of 5°C / min; when 500°C ≤ furnace temperature < 800°C, heat at a rate of 1°C / min; when 800°C ≤ furnace temperature < 1300°C, heat at a rate of 0.5°C / min; when furnace temperature ≥ 1300°C, keep warm for 8 hours and then allow the material to cool naturally to room temperature.

[0083] Example 2

[0084] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0085] (1) In step S2, the molar ratio of zinc nitrate hexahydrate, cerium nitrate hexahydrate and 2-methylimidazole is 2.5:1.25:0.25;

[0086] (2) In step S3, the NH3 atmosphere flow rate is 0.06 m / s.

[0087] Example 3

[0088] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0089] (1) In step S2, the molar ratio of zinc nitrate hexahydrate, cerium nitrate hexahydrate and 2-methylimidazole is 5:2.5:0.25;

[0090] (2) In step S3, the NH3 atmosphere flow rate is 0.125 m / s.

[0091] Example 4

[0092] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0093] (1) The mass percentage of the core in the negative electrode active material is 20%;

[0094] (2) In step S2, the amount of red phosphorus added ensures that the mass ratio of core to active negative electrode material is 20%.

[0095] Example 5

[0096] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0097] (1) The mass percentage of the core in the negative electrode active material is 80%;

[0098] (2) In step S2, the amount of red phosphorus added ensures that the mass ratio of core to active negative electrode material is 80%.

[0099] Example 6

[0100] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0101] In step S2, the pre-activated red phosphorus and part of DMF and zirconium chloride are mixed together to obtain solution A; lanthanum nitrate hexahydrate and 2-aminoterephthalic acid are dispersed in the remaining DMF to obtain solution B; wherein,

[0102] The molar ratio of zirconium chloride, lanthanum nitrate hexahydrate and 2-aminoterephthalic acid is 4:2:0.25;

[0103] The mass volume ratio of zinc nitrate hexahydrate and part of DMF is 3g:40mL;

[0104] The volume ratio of partial DMF to remaining DMF is 2:1.

[0105] The amount of red phosphorus added ensures that the mass ratio of core / active negative electrode material is 50%.

[0106] Solution B was quickly added to solution A and stirred vigorously at room temperature for 24 h. After washing with methanol several times, it was vacuum dried at 80 °C for 12 h to obtain the precursor of the negative electrode material P@MOF-(Zr4,La2,N 0.5 ).

[0107] Comparative Example 1

[0108] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0109] In step S2, cerium nitrate hexahydrate is not added.

[0110] Comparative Example 2

[0111] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0112] In step S3, the calcination atmosphere is nitrogen.

[0113] Comparative Example 3

[0114] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0115] Step S1 is not included. No phosphorus element is added in step S2 either.

[0116] Comparative Example 4

[0117] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0118] The red phosphorus powder used in the example was directly used as the negative electrode active material.

[0119] Comparative Example 5

[0120] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0121] (1) The mass percentage of the core in the negative electrode active material is 10%;

[0122] (2) In step S2, the amount of red phosphorus added ensures that the mass ratio of core to active negative electrode material is 10%.

[0123] Comparative Example 6

[0124] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0125] (1) The mass percentage of the core in the negative electrode active material is 90%;

[0126] (2) In step S2, the amount of red phosphorus added ensures that the mass ratio of core / active negative electrode material is 90%.

[0127] Comparative Example 7

[0128] In this example, a negative electrode active material is prepared, and the specific steps are as follows:

[0129] D1. The red phosphorus powder was surface treated with oxygen plasma under the following treatment conditions: oxygen pressure less than 0.01 MPa, discharge voltage of 15 kV, plasma discharge power of 650 W, and time of 2 h; thereby obtaining pre-activated red phosphorus.

[0130] D2. The pre-activated red phosphorus and part of methanol, zinc nitrate hexahydrate, and cerium nitrate hexahydrate are mixed together to obtain solution A; 2-methylimidazole is dispersed in the remaining methanol to obtain solution B; wherein the molar ratio of zinc nitrate hexahydrate, cerium nitrate hexahydrate and 2-methylimidazole is 4:2:0.25; the mass volume ratio of zinc nitrate hexahydrate and part of methanol is 3g:40mL; the volume ratio of part of methanol to the remaining methanol is 2:1.

[0131] Solution B was quickly added to solution A and stirred vigorously at room temperature for 24 h. After washing with methanol several times, it was vacuum dried at 80 °C for 12 h to obtain MOF-(Zn4,Ce2,N 0.5 );

[0132] D3. Then, the pre-activated red phosphorus (obtained in step D1) was mixed with MOF-(Zn4, Ce2, N 0.5 ) (obtained in step D2) is ground and mixed, and then calcined at high temperature under NH3 atmosphere at a flow rate of 30 mL / min to obtain a negative electrode material; the amount of red phosphorus added ensures that the mass ratio of the core / active negative electrode material is 50%.

[0133] The heating and cooling process of calcination in this step is the same as that in Example 1.

[0134] Comparative Example 8

[0135] This example prepares a negative electrode active material, which is different from Example 1 in that:

[0136] In step S2, zinc nitrate hexahydrate is not added.

[0137] Test Case

[0138] This example tests the performance of the negative electrode active materials obtained in the examples and comparative examples, and the test method is as follows:

[0139] Preparation of negative electrode sheet:

[0140] The negative electrode active material, conductive agent (SP and CNT mixed in a mass ratio of 0.45:0.05) and binder (SBR and PAALi mixed in a mass ratio of 0.5:1.8) prepared in the embodiment and comparative example were mixed in a weight ratio of 97.7:1.1:1.2 to prepare an anode active material slurry, which was evenly coated on the negative electrode current collector, and then cold pressed and stripped to obtain an anode electrode sheet. Preparation of positive electrode sheet:

[0141] The positive electrode active material NCM523, the conductive agent acetylene black, and the binder PVDF are mixed in a mass ratio of 97:2:1, and the solvent NMP is added, and stirred under the action of a vacuum mixer until the system is uniform to obtain a positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, dried at room temperature, and then transferred to an oven for further drying, and then cold pressed and cut to obtain a positive electrode sheet.

[0142] Preparation of electrolyte:

[0143] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried lithium salt LiPF6 is dissolved in the mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0144] Separation film: A polyethylene film is selected as the separation film.

[0145] Preparation of lithium-ion batteries:

[0146] The positive electrode sheet, separator and negative electrode sheet are wound, injected with liquid, packaged and formed to produce a soft-pack battery with a design capacity of 5000mAh, a design 1C=5000mA and an N / P value of 1.05.

[0147] Lithium plating performance test (using the above soft pack battery):

[0148] RT2.8C / 0.7C lithium plating: ① Charge to 4.5V at 2.8C constant current and constant voltage, cut-off rate 0.025C, and leave for 5min; ② Discharge to 3V at 0.7C constant current, and leave for 5min; ③ Repeat steps ① to ② for a total of 49 times; ④ Charge to 4.5V at 2.8C constant current and constant voltage, cut-off rate 0.025C, and leave for 5min; ⑤ Disassemble the interface;

[0149] RT2.6C / 0.7C lithium precipitation: ① Charge to 4.5V at 2.6C constant current and constant voltage, cut-off rate 0.025C, and leave for 5min; ② Discharge to 3V at 0.7C constant current, and leave for 5min; ③ Repeat steps ① to ② for a total of 49 times; ④ Charge to 4.5V at 2.6C constant current and constant voltage, cut-off rate 0.025C, and leave for 5min; ⑤ Disassemble the interface;

[0150] RT2.4C / 0.7C lithium precipitation: ① Charge to 4.5V at 2.4C constant current and constant voltage, cut-off rate 0.025C, and leave for 5min; ② Discharge to 3V at 0.7C constant current, and leave for 5min; ③ Repeat steps ① to ② for a total of 49 times; ④ Charge to 4.5V at 2.4C constant current and constant voltage, cut-off rate 0.025C, and leave for 5min; ⑤ Disassemble the interface;

[0151] RT2.6C / 0.7C lithium precipitation: ① Charge to 4.5V at 2.2C constant current and constant voltage, cut-off rate 0.025C, and leave for 5min; ② Discharge to 3V at 0.7C constant current, and leave for 5min; Repeat steps ① to ② for a total of 49 times; ④ Charge to 4.5V at 2.2C constant current and constant voltage, cut-off rate 0.025C, and leave for 5min; ⑤ Disassemble the interface;

[0152] Cycle retention rate test (using the above soft pack battery):

[0153] ① Charge the battery to 4.5V at 0.5C at 25℃, with a cut-off current of 0.05C, and leave it for 5min; ② Measure the discharge capacity of the battery at this time, recorded as Dbefore; ③ Discharge the battery to 3V at 0.8C, and leave it for 5min; ④ Charge the battery to 4.5V at 1.5C, with a cut-off current of 0.05C, and leave it for 5min; ⑤ Repeat the above steps ③ to ④ 300 times, and then measure the discharge capacity of the battery at this time, recorded as Dafter; Calculate the cycle retention rate = Dafter / Dbefore*100%;

[0154] Cyclic thickness change rate test (using the above soft pack battery):

[0155] ① Charge the battery to 4.5V at 0.5C at 25℃, with a cut-off current of 0.05C, and leave it for 5min; ② Measure the thickness of the battery at this time, recorded as dbefore; ③ Discharge the battery to 3V at 0.8C, and leave it for 5min; ④ Charge the battery to 4.5V at 1.5C, with a cut-off current of 0.05C, and leave it for 5min; ⑤ Repeat the above steps ③ to ④ 300 times, and then measure the thickness of the battery at this time, recorded as dbefore; Calculate the cycle thickness expansion rate = (dbefore-dbefore) / dbefore*100%;

[0156] EIS test (using the above soft pack battery):

[0157] The battery cell was placed in a 25±3℃ constant temperature box for 2h, and tested using an electrochemical workstation. The test started at a frequency of 10000HZ, a cutoff frequency of 0.03HZ, and an amplitude (uA) = (10 / R)*1000000, where R is the internal resistance of the battery cell (mΩ). After the test, the EIS raw data of Potential, current, Frequency, Zre, and Zim (Z) were saved, and then a spectrum was drawn based on the data.

[0158] Gram Capacity Test:

[0159] Assemble the button battery for testing. The positive and negative electrodes and separator of the button battery are the same as those of the soft-pack battery. The model of the button battery is 2025. First, discharge the battery to 5mV with a constant current of 0.1mA and let it stand for 10 minutes. Then discharge it to 5mV with a constant current of 0.05mA and let it stand for 10 minutes. Then charge it to 2.0V with a constant current of 0.1mA and record the charging capacity.

[0160] Negative electrode coating appearance test: Use visual inspection to see whether the surface of the negative electrode is flat and whether there are black spots, so as to judge the hydrophilicity of the obtained negative electrode active material and the uniformity of its dispersion in water. Among them, the test result of "occasionally" means that 1 to 2 defects appear on every 2 negative electrode sheets; if the density of defect points is less than this range, it is recorded as no black spots or convex points; a large number of defects means that there are defects on each negative electrode sheet, and the number is greater than 20.

[0161] The results of the above tests are shown in Tables 1 to 2 and Figure 1 shown.

[0162] Table 1: Negative electrode rate lithium deposition in some specific implementation methods

[0163] Example 1 Example 2 Example 3 Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 8 2.8C No lithium precipitation Slight lithium deposition Slight lithium deposition Slight lithium deposition Severe lithium deposition Moderate lithium precipitation Severe lithium deposition 2.6C No lithium precipitation No lithium precipitation No lithium precipitation No lithium precipitation Lithium Separation Slight lithium deposition Lithium Separation 2.4C No lithium precipitation No lithium precipitation No lithium precipitation No lithium precipitation Slight lithium deposition No lithium precipitation Slight lithium deposition 2.2C No lithium precipitation No lithium precipitation No lithium precipitation No lithium precipitation No lithium precipitation No lithium precipitation No lithium precipitation

[0164] The results in Table 1 show that by adjusting the ratio of metal element A, metal element B and N element, the lithium precipitation of the negative electrode sheet made of the obtained negative electrode active material during the charge and discharge process can be adjusted to a certain extent. Within the ratio range provided by the present invention, the obtained negative electrode active material will not precipitate lithium when used at a rate of 2.6C (or below). Further optimization within the range provided by the present invention can even obtain a negative electrode active material that does not precipitate lithium when used at 2.8C.

[0165] In the EIS spectrum, the first semicircle is the impedance R of lithium ions passing through the solid electrolyte. SEI , the second semicircle is the charge transfer impedance R CT The larger the radius, the greater the corresponding impedance, which is not conducive to the transfer of lithium ions and charges. It can be seen from the spectrum that in Example 1, the two added metal elements will have a synergistic effect, greatly reducing R SEI and R CT ; This indicates that the shell has high electrical conductivity and high lithium ion transfer efficiency.

[0166] Table 2 Electrochemical properties of negative electrode active materials obtained in Examples and Comparative Examples

[0167] Serial number Gram capacity mAh / g Thickness expansion rate Capacity retention rate Coating appearance Example 1 1263 15.8% 91.6% No black spots or convex spots Example 2 1250 16.3% 90.2% Occasionally black spots or convex spots appear Example 3 1262 16.5% 90.7% No black spots or convex spots Example 4 758 13.2% 92.4% No black spots or convex spots Example 5 1455 18.7% 89.9% No black spots or convex spots Example 6 1262 19.1% 86.6% No black spots or convex spots Comparative Example 1 1258 21.5% 83.1% A lot of black spots and convex spots appear Comparative Example 2 1257 18.5% 86.8% Occasionally black spots or convex spots appear Comparative Example 3 323 8.9% 92.4% No black spots or convex spots Comparative Example 4 1850 45.9% 61.9% A lot of black spots and convex spots appear Comparative Example 5 589 12.8% 92.9% No black spots or convex spots Comparative Example 6 1687 25.7% 80.1% No black spots or convex spots Comparative Example 7 1255 30.5% 72.8% No black spots or convex spots Comparative Example 8 1260 23.3% 80.6% There are a lot of black spots and convex spots

[0168] By comparing the results of Examples 1 to 3 and Comparative Examples 1 to 2, it can be seen that the ratio of Zn, Ce, and nitrogen-containing ligands, as well as the flow rate of ammonia during calcination, will affect the gram capacity, pole piece expansion, and capacity retention rate of the material, but if they are within the range specified in the present invention, relatively excellent electrochemical performance will be obtained. Further, in Example 2, the flow rate of ammonia during calcination is small, and the N content in the shell of the obtained negative electrode active material is low, so its hydrophilicity and dispersibility in water are reduced to a certain extent, and uneven black spots and convex spots occasionally appear.

[0169] Comparison of Example 1 and Comparative Examples 1-2 also shows that in the negative electrode active material provided by the present invention, there is an obvious synergistic effect among the elements A, B and N, and none of them can be missing. Specifically, in Comparative Example 1, element B is not doped, and in Comparative Example 2, the N content is low, which affects the hydrophilicity and conductivity of the shell, and further affects the electrochemical performance.

[0170] By comparing the test results of Examples 1, 4, 5 and Comparative Examples 3 to 6, it can be seen that the mass percentage of the core in the overall negative electrode active material can greatly affect its specific capacity. Specifically, increasing the proportion of the core can increase the gram specific capacity to a certain extent. Too little phosphorus content is not ideal for the gram capacity. However, if the obtained negative electrode active material contains too much phosphorus, it is not conducive to reducing the volume change ratio during the battery charge and discharge cycle.

[0171] By comparing the test results of Example 1 and Comparative Example 7, it can be seen that simply mixing the core-shell (i.e., red phosphorus and MOF) of the embodiment and then calcining it cannot alleviate the expansion of red phosphorus, and the capacity retention rate is not ideal. This also shows that in the negative electrode active material provided by the present invention, the core-shell structure, or the special preparation process, plays an important role in the electrochemical performance of the negative electrode active material.

[0172] By comparing the results of Example 1, Comparative Examples 1 and 8, it can be seen that the absence of element A or element B will lead to lithium precipitation, which means that these two elements not only improve the overall conductivity, but also establish a synergistic effect with MOF to enhance the storage capacity of lithium (MOFs cannot be formed in Comparative Example 8), which is beneficial to improving the charging and high and low temperature discharge performance of the battery cell, and the formation of Zn-P bonds can serve as a charge and lithium ion transfer channel to prevent lithium ions from staying on the shell and not in the core, which is beneficial to fading and rate charge and discharge;

[0173] By comparing the results of Example 1 and Example 6, it can be seen that the combination of Zn and Ce has greater advantages in charging and cycling performance than the combination of Zr and La. This is because Zn and Ce have greater electronegativity, which can store electrons, avoid lithium precipitation, and improve the overall conductivity. However, it should be noted that within the scope provided by the present invention, changing the combination of metal element A and metal element B will bring about slight changes in performance, but the resulting negative electrode active materials all have relatively excellent overall performance.

[0174] The coating appearance problem will have a great impact on the capacity and cycle life of the battery. The generation of black spots and convex spots will affect the conductivity of the battery, hinder the electron transfer between the electrode materials, reduce the performance of the battery, and inhibit the lithium ion diffusion of the electrode materials. Comparing Example 1 and Example 2, Comparative Examples 1, 2, 4, and 8, the shell contains the calcined product of MOFs and is doped with heavy rare earth elements B and N. Compared with materials without MOFs or no rare earth element (element B) doping or reduced N content, the synergistic effect of the three greatly improves the hydrophilicity, which is mainly manifested in the obvious reduction of black spots and convex spots on the coating appearance; the coating appearance is also significantly improved by changing the doping amount.

[0175] In summary, the negative electrode active material provided by the present invention can greatly improve its conductivity and effectively increase its capacity, thereby greatly improving the cycle expansion rate, first efficiency and capacity retention rate of lithium-ion secondary batteries. Due to the above excellent performance, lithium-ion batteries including the negative electrode active material provided by the present invention are expected to have broad application prospects in the fields of energy storage, power, etc.

[0176] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A negative electrode active material, characterized in that: The negative electrode active material includes a core and a shell surrounding the core; The core includes elemental phosphorus; the core accounts for 20 to 80% of the mass percentage of the negative electrode active material; The shell is a carbon layer doped with metal element A, metal element B and N; the metal element A includes at least one of Zr, Zn, Co and Fe; the metal element B includes at least one of Ce, La and Pr.

2. The negative electrode active material according to claim 1, characterized in that The metal element A is Zn; and / or the metal element B is Ce.

3. The negative electrode active material according to claim 1 or 2, characterized in that: The core accounts for 40-60% of the mass of the negative electrode active material.

4. A method for preparing a negative electrode active material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: S1. preactivating the elemental phosphorus; S2. The product of step S1, salt A containing the metal element A, salt B containing the metal element B and a N-containing ligand are mixed in a solvent to obtain a precursor; S3. calcining the precursor in an atmosphere containing ammonia.

5. The preparation method according to claim 4, characterized in that: In step S1, the elemental phosphorus includes at least one of red phosphorus, black phosphorus, blue phosphorus and purple phosphorus; and / or the pre-activation method includes at least one of acid oxidation treatment, plasma treatment and chemical grafting treatment.

6. The preparation method according to claim 4, characterized in that: In step S2, the salt A includes at least one of chloride, nitrate and acetate; and / or the salt B includes at least one of chloride, nitrate and acetate.

7. The preparation method according to claim 6, characterized in that: In step S2, the molar ratio of salt A to salt B is 1.8-2.2:

1.

8. The preparation method according to claim 4, characterized in that: In step S2, the solvent includes at least one of N,N-dimethylformamide, water and methanol; and / or, in step S2, the N-containing ligand includes at least one of dimethylimidazole, diaminoterephthalic acid and urea.

9. The preparation method according to claim 4, characterized in that: In step S3, the maximum calcination temperature is ≥1300°C; and / or, in step S3, the flow rate of the atmosphere is 0.05-0.13 m / s.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises a battery cell; the battery cell comprises a positive electrode, a negative electrode and a separator separating the positive electrode and the negative electrode; The raw material for preparing the negative electrode includes the negative electrode active material as claimed in any one of claims 1 to 3.