Positive electrode material and preparation method thereof, negative electrode material and preparation method and application thereof

The polyanionic iron-based cathode material generated by the reaction under alginate fiber suppresses Fe-Na anti-site defects, improves sodium ion transport performance, solves the problem of limited battery performance in sodium-ion batteries, and significantly improves battery performance.

CN118841567APending Publication Date: 2024-10-25SHENZHEN TOPBAND NEW ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410939812.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing polyanionic iron-based cathode materials have limited sodium ion transport properties in sodium-ion batteries, resulting in limited battery performance.

Method used

By reacting the sodium source, iron source and phosphorus source in the presence of alginate fiber, a polyanionic iron-based cathode material is generated, and during the reaction process, the adsorption and ion exchange of the alginate fiber are used to inhibit the Fe-Na reaction. The generation of site defects improves sodium ion transport performance.

Benefits of technology

It effectively improves the sodium ion transport performance, reduces Fe-Na anti-site defects, significantly improves the overall performance of the battery, and solves the problem of insufficient sodium ion transport performance in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841567A_ABST
    Figure CN118841567A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sodium ion batteries, in particular to a positive electrode material and a preparation method thereof, and a negative electrode material and a preparation method and application thereof. The problem that in the prior art, the sodium ion transmission performance cannot be improved essentially is solved. The preparation method of the polyanion iron-based positive electrode material comprises the following steps: preparing alginic acid fibers; in the presence of alginic acid fibers, a sodium source, an iron source and a phosphorus source react to generate the polyanion iron-based positive electrode material. The preparation method is used for preparing the sodium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of sodium ion batteries, and in particular to a positive electrode material and a preparation method thereof, a negative electrode material and a preparation method and application thereof. Background Art

[0002] Compared with lithium-ion batteries, sodium-ion batteries have the following advantages: (1) Sodium salt raw materials are abundant and inexpensive. The use of iron-manganese-nickel-based positive electrode materials can reduce the raw material cost by half compared to lithium-ion battery ternary positive electrode materials; (2) Due to the characteristics of sodium salt, low-concentration electrolytes can be used (for electrolytes of the same concentration, the conductivity of sodium salts is about 20% higher than that of lithium electrolytes), thereby reducing costs; (3) Sodium ions do not form alloys with aluminum, and aluminum foil can be used as the negative electrode current collector, which can further reduce costs by about 8% and weight by about 10%.

[0003] Currently, polyanionic iron-based cathode materials are the most promising cathode materials in the field of energy storage. However, at the crystal level, this polyanionic iron-based cathode material is prone to antisite defects, which hinder the movement of sodium ions in the crystal lattice, resulting in a decrease in the transmission rate of sodium ions, which will affect the battery performance.

[0004] In the related art, the sodium ion transport performance is usually improved by improving the morphology and structure of the polyanionic iron-based positive electrode material. However, this improvement is limited to the sodium ion transport performance and cannot fundamentally improve the sodium ion transport performance, which limits the application of polyanionic iron-based positive electrode materials in sodium ion batteries. Summary of the invention

[0005] Based on this, the present application provides a positive electrode material and a preparation method thereof, a negative electrode material and a preparation method and application thereof, so as to solve the problem in the related art that the sodium ion transport performance cannot be substantially improved.

[0006] In a first aspect, a method for preparing a polyanionic iron-based positive electrode material is provided, comprising:

[0007] preparing alginate fibers;

[0008] In the presence of alginate fibers, a sodium source, an iron source and a phosphorus source are reacted to generate a polyanionic iron-based positive electrode material.

[0009] Optionally, the preparation of alginate fiber comprises:

[0010] preparing sodium alginate spinning solution;

[0011] Spraying the sodium alginate spinning solution into a calcium chloride aqueous solution through spinning to exchange ions between the sodium ions in the sodium alginate and the calcium ions in the calcium chloride to prepare the calcium alginate fibers;

[0012] The calcium alginate fiber is immersed in a hydrochloric acid solution to allow calcium ions in the calcium alginate fiber to exchange ions with hydrogen ions in the hydrochloric acid, thereby preparing the alginate fiber.

[0013] Optionally, the preparation method satisfies at least one of the following conditions:

[0014] (1) In the sodium alginate spinning solution, the mass proportion of the sodium alginate is 3% to 10%;

[0015] (2) In the calcium chloride aqueous solution, the mass proportion of calcium chloride is 3% to 10%;

[0016] (3) The concentration of the hydrochloric acid solution is 0.5 mol / L to 1.2 mol / L;

[0017] (4) The metal ions in the alginate fibers are exchanged with the hydrogen ions in the hydrochloric acid under heating, wherein the heating temperature is 50° C. to 80° C. and the heating time is 2 h to 10 h.

[0018] Optionally, the sodium source includes sodium carbonate, the iron source includes ferrous oxalate, and the phosphorus source includes one or more of phosphate and pyrophosphate;

[0019] Optionally, the phosphate is ammonium phosphate.

[0020] Optionally, the polyanionic iron-based cathode material further comprises a carbon coating layer; in the presence of alginate fibers, a sodium source, an iron source and a phosphorus source are reacted to generate a polyanionic iron-based cathode material, comprising:

[0021] The alginate fiber is immersed in a solution containing a sodium source, an iron source and a phosphorus source, and an organic carbon source is added to prepare a first mixed solution;

[0022] The first mixed solution is calcined to prepare the polyanionic iron-based positive electrode material containing the carbon coating layer.

[0023] Optionally, the preparation method satisfies at least one of the following conditions:

[0024] (1) The solvent used in the solution containing the sodium source, the iron source and the phosphorus source is a mixed solvent of water and ethanol;

[0025] (2) The organic carbon source includes glucose;

[0026] (3) The molar ratio of the sodium element in the sodium source, the iron element in the iron source and the phosphorus element in the phosphorus source is (0.7-4.0): (0.3-3.0): (0.3-3.0);

[0027] (4) The calcination is carried out under the protection of an inert gas, and the calcination temperature is 600° C. to 900° C., and the calcination time is 6 h to 12 h.

[0028] In a second aspect, a polyanionic iron-based positive electrode material is provided, which is prepared using the preparation method described in the first aspect.

[0029] Optionally, the positive electrode material in the polyanionic iron-based positive electrode material satisfies at least one of the following conditions:

[0030] (1) The proportion of Fe-Na antisite defects in the polyanionic iron-based positive electrode material is less than or equal to 0.3%;

[0031] (2) The specific surface area of ​​the positive electrode material in the polyanionic iron-based positive electrode material is 10.2 m2 / g to 52.3 m2 / g;

[0032] (3) The median particle size D50 of the positive electrode material in the polyanionic iron-based positive electrode material is 1.5 μm to 6 μm;

[0033] (4) The polyanionic iron-based positive electrode material further includes a carbon coating layer, and the mass proportion of the carbon coating layer in the polyanionic iron-based positive electrode material is 0.5% to 2%.

[0034] In a third aspect, a positive electrode plate is provided, comprising a positive electrode collector, and a positive electrode material disposed on at least one side of the positive electrode collector along its thickness direction, wherein the positive electrode material comprises the polyanionic iron-based positive electrode material as described in the second aspect.

[0035] In a fourth aspect, a method for preparing a negative electrode material is provided, comprising:

[0036] preparing a second mixed solution of a sugar carbon source and an organic nitrogen source;

[0037] The second mixed solution is carbonized in a protective gas atmosphere to prepare the negative electrode material.

[0038] Optionally, the preparation method satisfies at least one of the following conditions:

[0039] (1) The carbohydrate carbon source includes: one or more of glucose, sucrose and starch; optionally, the carbohydrate carbon source is glucose;

[0040] (2) The organic nitrogen source comprises: one or more of melamine, dicyandiamide and urea. Optionally, the organic nitrogen source is melamine;

[0041] (3) The protective gas includes at least one of nitrogen, helium, neon and argon;

[0042] (4) The temperature of the carbonization treatment is 800°C to 1500°C, and the time is 1 h to 5 h.

[0043] In a fifth aspect, a negative electrode material is provided, which is prepared using the preparation method described in the fourth aspect.

[0044] Optionally, the negative electrode material satisfies at least one of the following conditions:

[0045] (1) The interlayer spacing of the hard carbon in the negative electrode material is 0.374 nm to 0.40 nm;

[0046] (2) The median particle size D50 of the hard carbon in the negative electrode material is 4 μm to 8.0 μm.

[0047] (3) The specific surface area of ​​the hard carbon in the negative electrode material is ≤0.03 m2 / g;

[0048] (4) The ash content of the hard carbon in the negative electrode material is ≤0.1%.

[0049] In a sixth aspect, a negative electrode plate is provided, comprising a negative electrode current collector, and a negative electrode material disposed on at least one side of the negative electrode current collector along its thickness direction, wherein the negative electrode material is the negative electrode material as described in the fifth aspect.

[0050] In the seventh aspect, a sodium ion battery is provided, comprising a positive electrode plate, a negative electrode plate and a separator, wherein the positive electrode plate is the positive electrode plate as described in the third aspect, and the negative electrode plate is the negative electrode plate as described in the sixth aspect.

[0051] In an eighth aspect, a battery module is provided, comprising a plurality of batteries connected in series and / or in parallel, at least one battery being a sodium ion battery as described in the seventh aspect.

[0052] In a ninth aspect, an electrical device is provided, comprising the battery module as described in the eighth aspect.

[0053] Compared with the related art, this application has at least the following beneficial technical effects:

[0054] By reacting the sodium source, the iron source and the phosphorus source in the presence of alginate fibers, on the one hand, the sodium ions and iron ions in the reaction process can be adsorbed and fixed by utilizing the adsorption and ion exchange of metal ions by the alginate fibers. For example, the alginate fibers can form a strong complexation with the iron ions and can undergo an adsorption reaction with the sodium ions. Therefore, during the reaction, since the iron ions are complexed and fixed, the iron ions can be effectively inhibited from occupying the positions that should be occupied by the sodium ions, thereby inhibiting the generation of Fe-Na antisite defects, and further reducing the problem of decreased sodium ion transmission rate caused by Fe-Na antisite defects, thereby substantially improving the sodium ion transmission performance and thus improving the battery performance. On the other hand, the antisite defects are inhibited during the reaction process, and compared with the related art that only improves the morphology, the movement of sodium ions in the lattice can be fundamentally inhibited, thereby improving the sodium ion transmission performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 A scanning electron microscope image of a polyanionic iron-based cathode material is provided for some embodiments of the present application;

[0056] Figure 2 XRD comparison spectra of the negative electrode materials provided in Examples 1, 4, 5, 6 and 7 of the present application. DETAILED DESCRIPTION

[0057] In order to facilitate the understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0058] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0059] The present application will be further described in detail below in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly understood.

[0060] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0061] In this application, "one or several" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.

[0062] In the present application, the terms "combination thereof", "any combination thereof", "any combination thereof" and the like include all suitable combinations of any two or more of the listed items.

[0063] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0064] In the present application, reference to a numerical range includes both endpoints of the numerical range unless otherwise specified.

[0065] In the present application, the percentage content, unless otherwise specified, refers to mass percentage for solid-liquid mixing and solid-solid mixing, and volume percentage for liquid-liquid mixing.

[0066] In this application, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.

[0067] In this application, when it comes to temperature parameters, unless otherwise specified, both constant temperature treatment and treatment within a certain temperature range are permitted. The constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument.

[0068] In view of the problem that the relevant technology cannot substantially improve the sodium ion transport performance, the specific implementation of the present application is described as follows:

[0069] In a first aspect, some embodiments of the present application provide a method for preparing a polyanionic iron-based positive electrode material, the preparation method comprising:

[0070] S11), preparing alginate fibers;

[0071] S12), in the presence of alginate fibers, reacting sodium salt, iron salt and phosphate to generate a polyanionic iron-based positive electrode material.

[0072] Among them, alginate is a component of seaweed plants, which has natural biocompatibility and biodegradability. It has excellent properties of moisture absorption, moisturizing, skin affinity and heavy metal adsorption.

[0073] In the preparation method of the polyanionic iron-based positive electrode material provided in the embodiment of the present application, a sodium source, an iron source and a phosphorus source are reacted in the presence of alginate fibers. On the one hand, the sodium ions and iron ions in the reaction process can be adsorbed and fixed by utilizing the adsorption and ion exchange effect of the alginate fibers on metal ions. For example, alginate fibers can form a strong complexation with iron ions and can undergo an adsorption reaction with sodium ions. Therefore, during the reaction, since the iron ions are complexed and fixed, the iron ions can be effectively inhibited from occupying the positions that should be occupied by sodium ions, thereby inhibiting the generation of Fe-Na antisite defects, and further reducing the problem of decreased sodium ion transmission rate caused by Fe-Na antisite defects, thereby substantially improving the sodium ion transmission performance and thus improving the battery performance. On the other hand, antisite defects are inhibited during the reaction process, which can fundamentally inhibit the movement of sodium ions in the lattice and improve the sodium ion transmission performance compared with the related art that only improves the morphology.

[0074] In summary, the embodiments of the present application can substantially improve the sodium ion transport performance, solving the problem in the related art that the sodium ion transport performance cannot be substantially improved, thereby limiting the application of polyanionic iron-based positive electrode materials in sodium ion batteries.

[0075] There is no specific limitation on the preparation method of the alginate fiber, and all preparation methods that can obtain the alginate fiber are within the protection scope of this application.

[0076] In some embodiments, preparing alginate fibers may include:

[0077] preparing sodium alginate spinning solution;

[0078] The sodium alginate spinning solution is sprayed into a calcium chloride aqueous solution through spinning to exchange sodium ions in the sodium alginate with calcium ions in the calcium chloride to prepare calcium alginate fibers;

[0079] The calcium alginate fiber is immersed in a hydrochloric acid solution to allow calcium ions in the calcium alginate fiber to exchange with hydrogen ions in the hydrochloric acid to prepare the alginate fiber.

[0080] In these embodiments, calcium chloride aqueous solution is used as coagulation liquid, and water-insoluble sodium alginate can be exchanged with calcium ions in the coagulation liquid to prepare calcium alginate fibers, and each component is safe and harmless during the entire spinning process; then, by immersing the calcium alginate fibers in a hydrochloric acid solution, the calcium alginate fibers can be converted into alginate fibers by removing metal ions in an acidic medium, and the hydrochloric acid solution is beneficial for replacing calcium ions in calcium alginate, thereby facilitating the acquisition of alginate fibers with higher purity, and facilitating the alginate fibers to more effectively fix and adsorb subsequent iron ions and sodium ions, and the hydrochloric acid solution will not introduce more impurity ions; in addition, sodium alginate can be made into a viscous solution, thereby facilitating spinning.

[0081] In some embodiments, the above preparation method satisfies at least one of the following conditions:

[0082] (1) In the sodium alginate spinning solution, the mass proportion of sodium alginate is 3%~10%;

[0083] (2) In the calcium chloride aqueous solution, the mass proportion of calcium chloride is 3%~10%;

[0084] (3) The concentration of hydrochloric acid solution is 0.5 mol / L~1.2 mol / L;

[0085] (4) The metal ions in the alginate fibers are exchanged with the hydrogen ions in the hydrochloric acid under heating at a temperature of 50°C to 80°C for a time of 2 h to 10 h.

[0086] In these embodiments, by controlling the concentration of the sodium alginate and calcium chloride, the concentration of the hydrochloric acid solution and / or the temperature and time during ion exchange, the generation of alginate fibers with higher purity can be more effectively controlled and the introduction of other impurities can be reduced.

[0087] There is no limitation on the specific selection of the above-mentioned sodium source, iron source and phosphorus source, and all raw materials that can generate polyanionic iron-based positive electrode materials are within the protection scope of this application.

[0088] In some embodiments, the sodium source includes sodium carbonate, the iron source includes ferrous oxalate, and the phosphorus source includes one or more of phosphate and pyrophosphate.

[0089] Optionally, the phosphate is ammonium phosphate.

[0090] Wherein, when the phosphorus source includes phosphate and the phosphate is ammonium phosphate, the reaction equation of the sodium source, the iron source and the phosphorus source is as shown in the following formula (1):

[0091] (NH4)3PO4+FeC2O4→FeH2P2O7

[0092] FeH2P2O7+Na2CO3→Na x Fe y (PO4)2P2 formula (1);

[0093] Wherein, in formula (1), x can be 3-8, and y can be 1-4.

[0094] When the phosphate includes pyrophosphate and the pyrophosphate is ammonium pyrophosphate, the reaction equation of the sodium source, the iron source and the phosphorus source is as shown in the following formula (2):

[0095] (NH4, H)4P2O7+FeC2O4→FeH2P2O7

[0096] FeH2P2O7+Na2CO3→Na x Fe y (PO4)2P2 formula (2);

[0097] Wherein, in formula (1), x can be 3-8, and y can be 1-4.

[0098] In some embodiments, the polyanionic iron-based cathode material may further include a carbon coating layer; in the presence of alginate fibers, reacting a sodium source, an iron source, and a phosphorus source to generate a polyanionic iron-based cathode material may include:

[0099] The alginate fiber is immersed in a solution containing a sodium source, an iron source and a phosphorus source, and an organic carbon source is added to prepare a first mixed solution;

[0100] The first mixed solution is calcined to prepare a polyanionic iron-based positive electrode material containing a carbon coating layer.

[0101] In these embodiments, the polyanionic iron-based positive electrode material also includes a carbon coating layer. At this time, the polyanionic iron-based positive electrode material containing the carbon coating layer can be directly prepared by adding an organic carbon source to a solution containing a sodium source, an iron source and a phosphorus source, and then calcining. The preparation method is simple and convenient. The carbon coating layer can improve the electronic conductivity and ionic conductivity of the polyanionic iron-based positive electrode material.

[0102] In some embodiments, the preparation method satisfies at least one of the following conditions:

[0103] (1) The solvent used in the solution containing the sodium source, the iron source and the phosphorus source is a mixed solvent of water and ethanol;

[0104] (2) Organic carbon sources include glucose;

[0105] (3) the molar ratio of the sodium element in the sodium source, the iron element in the iron source and the phosphorus element in the phosphorus source is (0.7~4.0):(0.3~3.0):(0.3~3.0);

[0106] (4) Calcination is carried out under the protection of inert gas, and the calcination temperature is 600℃~900℃, and the time is 6h~12h.

[0107] In these embodiments, a mixed solvent of water and ethanol is selected to dissolve the sodium source, iron source and phosphorus source. The solubility of pure water is limited. The addition of ethanol may improve its solubility by changing the polarity of the solvent, reducing the surface tension of the solution, etc. The addition of ethanol may also prevent or reduce the precipitation produced during the dissolution process by slowing down the precipitation rate of the solute, thereby facilitating the acquisition of a more uniform and stable solution. By using glucose as an organic carbon source, excellent electrochemical properties such as higher specific capacity, good cycle stability and rate performance are exhibited. This is mainly due to the unique structural characteristics of hard carbon materials, such as pore size, void density, etc., which are conducive to the embedding and extraction of sodium ions. Controlling the molar mass ratio of the sodium source, iron source and phosphorus source within the above range can ensure that the reactants react in an appropriate ratio, thereby avoiding excess or deficiency of a certain reactant and promoting the complete reaction. By controlling the temperature and time of calcination within the above range, the appropriate calcination temperature can promote ion rearrangement and crystallization in the positive electrode material, making the crystal structure of the material more complete. Sufficient calcination time can ensure that impurities such as carbon black and polymer in the positive electrode material are completely discharged, thereby improving the purity and crystallinity of the material.

[0108] In a second aspect, some embodiments of the present application provide a polyanionic iron-based positive electrode material prepared using the preparation method described in the first aspect.

[0109] By preparing the polyanionic iron-based positive electrode material using the preparation method as described in the first aspect, the Fe-Na antisite defects in the polyanionic iron-based positive electrode material can be reduced, thereby increasing the sodium ion transmission rate, thereby improving the battery performance of the polyanionic iron-based positive electrode material when used.

[0110] In some embodiments, the polyanionic iron-based cathode material satisfies at least one of the following conditions:

[0111] (1) The proportion of Fe-Na antisite defects in the polyanionic iron-based cathode material is less than or equal to 0.3%;

[0112] (2) The specific surface area of ​​the positive electrode material in the polyanionic iron-based positive electrode material is 10.2㎡ / g~52.3㎡ / g;

[0113] (3) The particle size of the positive electrode material in the polyanionic iron-based positive electrode material is 1.5 μm to 6 μm;

[0114] (4) The polyanionic iron-based positive electrode material further includes a carbon coating layer, and the mass proportion of the carbon coating layer in the polyanionic iron-based positive electrode material is 0.5% to 2%.

[0115] In these embodiments, the proportion of Fe-Na antisite defects in the polyanionic iron-based positive electrode material is less than or equal to 0.3%, which means that in the crystal structure of the polyanionic iron-based positive electrode material, the proportion of the number of Fe-Na antisite defects relative to the total number of atoms does not exceed 0.3%. The polyanionic iron-based positive electrode material has a relatively low Fe-Na antisite defect, which is convenient for improving the sodium ion transmission speed when used, thereby improving the battery performance. By controlling the particle size of the positive electrode material in the polyanionic iron-based positive electrode material to 1.5μm ~ 6μm, the appropriate particle size range can reduce the contact area with the electrolyte, limit the occurrence of side reactions, and thus improve the reversible capacity of the material. In the case where the polyanionic iron-based positive electrode material also includes a carbon coating layer, by controlling the mass proportion of the carbon coating layer in the polyanionic iron-based positive electrode material to 0.5% ~ 2%, the carbon coating layer, as a conductive agent, can form a conductive network on the surface of the positive electrode material, provide an electron transmission channel, and thus improve the conductive performance of the material. When the carbon coating content is appropriate, the internal resistance of the material can be significantly reduced, and the output power and charge and discharge efficiency of the battery can be improved. Too high a carbon coating content will affect the capacity.

[0116] like Figure 1 As shown, a SEM (Scanning Electron Microscope) image of a polyanionic iron-based positive electrode material provided in an embodiment of the present application is shown. From the SEM image, it can be seen that the particle size distribution of the polyanionic iron-based positive electrode material and the morphology of the prepared positive electrode material are regular, which is conducive to ion transport.

[0117] In a third aspect, some embodiments of the present application provide a positive electrode plate, comprising a positive electrode collector, and a positive electrode material arranged on at least one side of the positive electrode collector along its thickness direction, wherein the positive electrode material comprises the polyanionic iron-based positive electrode material as described in the second aspect.

[0118] Since the positive electrode material contained in the positive electrode plate provided in the third aspect includes the polyanionic iron-based positive electrode material described in the second aspect, the beneficial technical effects of the positive electrode plate provided in the third aspect are the same as the beneficial technical effects of the polyanionic iron-based positive electrode material provided in the second aspect, and will not be repeated here.

[0119] In a fourth aspect, some embodiments of the present application provide a method for preparing a negative electrode material, comprising:

[0120] preparing a second mixed solution of a sugar carbon source and an organic nitrogen source;

[0121] In a protective gas atmosphere, carbonizing the second mixed solution to prepare a negative electrode material;

[0122] The carbonization treatment temperature is 800°C to 1500°C, and the time is 1 h to 5 h.

[0123] In the preparation method of the negative electrode material provided in the embodiment of the present application, a hard carbon negative electrode material can be prepared by carbonizing a mixed solution of a suspension of a sugar carbon source and an organic nitrogen source (that is, the above-mentioned second mixed solution). The hard carbon negative electrode material prepared using the sugar carbon source has a rich pore structure and a large specific surface area, which is conducive to regulating the defects in the hard carbon negative electrode material. At the same time, during the preparation process, on the one hand, the introduction of the organic nitrogen source can produce a five-membered ring or a six-membered ring containing heteroatoms such as nitrogen atoms inside or at the edge of the carbon layer. On the other hand, by controlling the temperature of the carbonization treatment to 800°C~1500°C, topological defects can be formed in the hard carbon negative electrode material, which is different from the common defects formed in the hard carbon negative electrode material in the related art. The common defects are formed in the hard carbon negative electrode material. Introducing heteroatoms into the material and retaining them in the hard carbon negative electrode material will produce a five-membered ring or a six-membered ring containing heteroatoms inside or at the edge of the carbon layer. At the temperature of the carbonization treatment, the heteroatoms can be removed, and the multi-carbon rings from which the heteroatoms have been removed can be healed to produce carbon five-, six-, or seven-membered rings, etc., thereby changing its planar structure. On the one hand, compared with the related art in which the presence of heteroatoms reduces the reversibility of ion embedding and extraction from the negative electrode material, the interlayer spacing of carbon in the hard carbon negative electrode material can be increased, thereby maintaining the reversibility of ion embedding and extraction from the negative electrode material; on the other hand, it can also reduce the diffusion barrier of sodium ions in the hard carbon material and increase the diffusion rate of sodium ions; at the same time, topological defects can also enhance the conductivity of the hard carbon material, which is beneficial to the rapid transmission of electrons in the material.

[0124] In some embodiments, the above preparation method satisfies at least one of the following conditions:

[0125] (1) The carbohydrate carbon source includes: one or more of glucose, sucrose and starch; optionally, the carbohydrate carbon source is glucose;

[0126] (2) The organic nitrogen source includes: one or more of melamine, dicyandiamide and urea, and optionally, the organic nitrogen source is melamine;

[0127] (3) The protective gas includes at least one of nitrogen, helium, neon and argon.

[0128] In these embodiments, by selecting one or more of melamine, dicyandiamide and urea as the organic nitrogen source, the stability and controllability of the nitrogen source can be utilized to perform nitrogen doping under nitrogen protection, which can further reduce the interference of oxygen and ensure the accuracy and effectiveness of nitrogen doping.

[0129] In a fifth aspect, some embodiments of the present application provide a negative electrode material prepared using the preparation method described in the fourth aspect.

[0130] By adopting the preparation method as described in the fourth aspect to prepare the negative electrode material, topological defects can be formed in the hard carbon negative electrode material. Compared with the ordinary defects formed in the hard carbon negative electrode material in the related art, the topological defects are formed after the removal of heteroatoms, and the multi-carbon rings heal to produce carbon five-, six-, and seven-membered rings, etc., which change its planar structure. On the one hand, the interlayer spacing of carbon in the hard carbon negative electrode material can be increased, and on the other hand, the distance for the insertion and extraction of sodium ions can be shortened. Compared with the ordinary defects formed in the hard carbon negative electrode material in the related art, the topological defects can maintain the electrochemical properties of the hard carbon negative electrode material to a large extent.

[0131] In some embodiments, the negative electrode material satisfies at least one of the following conditions:

[0132] (1) The interlayer spacing of the hard carbon in the negative electrode material is 0.374 nm to 0.40 nm;

[0133] (2) The median particle size D50 of the hard carbon in the negative electrode material is 4 μm to 8.0 μm;

[0134] (3) The specific surface area of ​​the hard carbon in the negative electrode material is ≤0.03 m2 / g;

[0135] (4) The ash content of the hard carbon in the negative electrode material is ≤0.1%.

[0136] In these embodiments, the interlayer spacing of carbon in the negative electrode material is relatively large, which can maintain the reversibility of ion insertion and extraction and improve battery performance. The particle size in the negative electrode material is controlled at 4μm ~ 8.0μm. The smaller particle size can shorten the diffusion path of ions and improve the rate performance. The specific surface area in the negative electrode material is controlled at ≤3%㎡ / g because the increase in specific surface area can increase the adsorption amount of lithium ions on the one hand, and on the other hand, the high specific surface area will increase the side reactions during the SEI formation process, affecting the formation of the SEI film and resulting in poor cycle stability. Therefore, appropriate specific surface area control is beneficial to improving battery performance.

[0137] In a sixth aspect, some embodiments of the present application provide a negative electrode plate, comprising a negative electrode current collector, and a negative electrode material disposed on at least one side of the negative electrode current collector along its thickness direction, wherein the negative electrode material is the negative electrode material as described in the fifth aspect.

[0138] Since the negative electrode material contained in the negative electrode plate provided in the sixth aspect includes the negative electrode material described in the fifth aspect, the beneficial technical effects of the negative electrode plate provided in the sixth aspect are the same as the beneficial technical effects of the negative electrode material provided in the second aspect, and will not be repeated here.

[0139] In the seventh aspect, some embodiments of the present application provide a sodium ion battery, comprising a positive electrode plate, a negative electrode plate and a separator, wherein the positive electrode plate is the positive electrode plate as described in the third aspect, and the negative electrode plate is the negative electrode plate as described in the sixth aspect.

[0140] Since the sodium ion battery described in the seventh aspect includes the positive electrode sheet described in the third aspect and the negative electrode sheet described in the sixth aspect, the sodium ion battery described in the seventh aspect has the dual beneficial technical effects of the positive electrode sheet described in the third aspect and the negative electrode sheet described in the sixth aspect. The specific effect description can be found in the description of the third aspect and the sixth aspect, which will not be repeated here.

[0141] In an eighth aspect, some embodiments of the present application provide a battery module comprising a plurality of batteries connected in series and / or in parallel, at least one battery being a sodium ion battery as described in the seventh aspect.

[0142] Since the battery module described in the eighth aspect includes the sodium ion battery described in the seventh aspect, the beneficial technical effects of the battery module described in the eighth aspect can be found in the description of the beneficial technical effects of the sodium ion battery described in the seventh aspect above, and will not be repeated here.

[0143] In a ninth aspect, some embodiments of the present application provide an electrical device comprising a battery module as described in the eighth aspect.

[0144] Since the electrical device described in the ninth aspect includes the battery module described in the eighth aspect, the beneficial technical effects of the battery module described in the ninth aspect can be found in the description of the beneficial technical effects of the sodium ion battery described in the eighth aspect above, and will not be repeated here.

[0145] The above introduces the specific implementation methods of the present application. In order to objectively illustrate the technical effects produced by the present application, the following examples and comparative examples will be used for description.

[0146] In the following examples and comparative examples, all raw materials can be purchased in commercial form, and in order to maintain the reliability of the experiment, the raw materials used in the following examples and comparative examples have the same physical and chemical parameters or are processed in the same way.

[0147] Example 1

[0148] The preparation method of the sodium ion battery provided in Example 1 is as follows:

[0149] Step 1), preparation of polyanionic iron-based positive electrode material:

[0150] Step 11), weighing 5% sodium alginate solution and spraying it into a coagulation bath containing 5% CaCl2 through a spinner to obtain calcium alginate fibers;

[0151] Step 12), the obtained calcium alginate fiber is immersed in 1M HCl solution for Ca 2+ and H + The exchange of , protonated calcium alginate fibers was obtained;

[0152] Step 13), soaking the protonated calcium alginate fiber in a water-ethanol solution of 40% sodium carbonate, 30% ferrous oxalate, and 30% ammonium phosphate, adding 1% glucose to obtain a mixed solution, wherein the molar ratio of sodium carbonate, ferrous oxalate, and ammonium phosphate is 1.88:1.80:1.0;

[0153] Step 14), calcining the mixed solution obtained in step 13) at 700° C. in a N2 atmosphere for 8 hours to obtain a carbon-coated polyanionic sodium ion positive electrode material with low antisite defects;

[0154] Step 2), preparation of hard carbon negative electrode material:

[0155] Step 21), dispersing the melamine-containing solution in tetrahydrofuran to obtain a suspension;

[0156] Step 22), glucose is dissolved in tetrahydrofuran, the supernatant is removed and added to the suspension of the above (4), after stirring and drying, it is carbonized at 1100°C for 4h under argon protection and then cooled to obtain a sodium-ion hard carbon negative electrode material with high topological defects.

[0157] Step 3) Preparation of positive electrode sheet:

[0158] The positive electrode material prepared in step 1) is used as the positive electrode active material, and is dissolved in N-methylpyrrolidone in a ratio of 96% of the positive electrode active material (based on the mass of the positive electrode), 2% of PVDF (based on the mass of the positive electrode), 1% of the conductive carbon black (based on the mass of the positive electrode) and 1% of the carbon nanotubes (based on the mass of the positive electrode). The mixture is stirred and dispersed in a blender under vacuum to prepare a uniform bubble-free slurry, which is evenly coated on an aluminum foil to prepare a positive electrode sheet.

[0159] Step 4), preparation of negative electrode sheet:

[0160] The negative electrode material prepared in step 2) is used as the negative electrode active material, wherein the D50 of the hard carbon in the negative electrode active material is 7.3 um and the specific surface area is 3.5 m 2 / g. 94% of negative electrode active material (based on negative electrode mass), 1.5% of sodium carboxymethyl cellulose (based on positive electrode mass), 2% of conductive carbon black (based on positive electrode mass) and 2.5% of styrene-butadiene latex (based on negative electrode mass) were dissolved in deionized water, stirred and dispersed in a blender under vacuum to prepare a uniform slurry without bubbles, which was evenly coated on aluminum foil to prepare a negative electrode sheet.

[0161] Step 5), packaging and formation:

[0162] Step 51), the positive electrode sheet and the separator prepared in step 3) and the negative electrode sheet prepared in step 4) are stacked to form a battery cell, the battery cell has tabs on the same side, the tabs are welded together with the current collector using an ultrasonic welding machine, and then encapsulated with an aluminum-plastic film;

[0163] Step 52), after the battery cell is baked, the electrolyte is injected into the battery cell, and after chemical composition, a 4Ah lithium-ion battery is prepared, wherein the solute of the electrolyte is sodium hexafluorophosphate, the solvent is a mixed solvent of EC (ethylene carbonate), PC (propylene carbonate), EMC (ethyl methyl carbonate) and DMC (dimethyl carbonate), and the additives are FEC (fluoroethylene carbonate) and DTD (ethylene sulfate).

[0164] Example 2

[0165] The method for preparing the sodium ion battery provided in Example 2 is substantially the same as the method for preparing the sodium ion battery provided in Example 1, except that:

[0166] In step 11), the concentration of the sodium alginate solution is 3%, and the concentration of CaCl2 in the coagulation bath is 3%;

[0167] In step 12), the concentration of the HCl solution is 0.8 mol;

[0168] In step 13), the molar ratio of sodium carbonate, ferrous oxalate and ammonium phosphate is 3:2:2, the concentrations of sodium carbonate, ferrous oxalate and ammonium phosphate are 30%, 34% and 28% respectively, and the concentration of glucose is 1%;

[0169] In step 14), the calcination temperature is 850° C. and the calcination time is 7 h.

[0170] Example 3

[0171] The method for preparing a sodium ion battery provided in Example 3 is substantially the same as the method for preparing a sodium ion battery provided in Example 1, except that:

[0172] In step 11), the concentration of the sodium alginate solution is 10%, and the concentration of CaCl2 in the coagulation bath is 10%;

[0173] In step 12), the concentration of the HCl solution is 1.2 mol;

[0174] In step 13), the molar ratio of sodium carbonate, ferrous oxalate and ammonium phosphate is 1:1:1; the concentrations of sodium carbonate, ferrous oxalate and ammonium phosphate are 24%, 41% and 34% respectively, and the concentration of glucose is 1%;

[0175] In step 14), the calcination temperature is 900° C. and the calcination time is 6 h.

[0176] Example 4

[0177] The method for preparing a sodium ion battery provided in Example 4 is substantially the same as the method for preparing a sodium ion battery provided in Example 1, except that:

[0178] In step 22), the carbonization temperature is 800°C.

[0179] Example 5

[0180] The method for preparing a sodium ion battery provided in Example 5 is substantially the same as the method for preparing a sodium ion battery provided in Example 1, except that:

[0181] In step 22), the carbonization temperature is 900°C.

[0182] Example 6

[0183] The method for preparing a sodium ion battery provided in Example 6 is substantially the same as the method for preparing a sodium ion battery provided in Example 1, except that:

[0184] In step 22), the carbonization temperature is 1000°C.

[0185] Example 7

[0186] The method for preparing a sodium ion battery provided in Example 7 is substantially the same as the method for preparing a sodium ion battery provided in Example 1, except that:

[0187] In step 22), the carbonization temperature is 1200°C.

[0188] Example 8

[0189] The method for preparing a sodium ion battery provided in Example 8 is substantially the same as the method for preparing a sodium ion battery provided in Example 1, except that:

[0190] In step 21), melamine is replaced by dicyandiamide.

[0191] Example 9

[0192] The method for preparing a sodium ion battery provided in Example 9 is substantially the same as the method for preparing a sodium ion battery provided in Example 8, except that:

[0193] In step 22), glucose is replaced by sucrose.

[0194] Example 10

[0195] The method for preparing a sodium ion battery provided in Example 10 is substantially the same as the method for preparing a sodium ion battery provided in Example 8, except that:

[0196] In step 22), glucose is replaced by starch.

[0197] Embodiment 11

[0198] The method for preparing a sodium ion battery provided in Example 11 is substantially the same as the method for preparing a sodium ion battery provided in Example 1, except that:

[0199] In step 21), melamine is replaced by urea.

[0200] Example 12

[0201] The method for preparing the sodium ion battery provided in Example 12 is substantially the same as the method for preparing the sodium ion battery provided in Example 11, except that:

[0202] In step 22), glucose is replaced by sucrose.

[0203] Example 13

[0204] The method for preparing the sodium ion battery provided in Example 13 is substantially the same as the method for preparing the sodium ion battery provided in Example 11, except that:

[0205] In step 22), glucose is replaced by starch.

[0206] Embodiment 14

[0207] The method for preparing a sodium ion battery provided in Example 14 is substantially the same as the method for preparing a sodium ion battery provided in Example 7, except that:

[0208] In step 2), only glucose is dissolved in tetrahydrofuran, stirred and dried, and then carbonized at 1200° C. under argon protection and then cooled to obtain a hard carbon negative electrode material.

[0209] Embodiment 15

[0210] The method for preparing a sodium ion battery provided in Example 15 is substantially the same as the method for preparing a sodium ion battery provided in Example 7, except that:

[0211] In step 1), sodium alginate is not used to prepare alginic acid. Only 40 parts of sodium carbonate, 30 parts of ferrous oxalate and 30 parts of ammonium phosphate are weighed, added into 5000 mL of deionized water-ethanol solution (water: ethanol = 1: 1) and stirred for half an hour to obtain a uniformly mixed solution, and 1% glucose is added to obtain a mixed solution; then the mixed solution is calcined under a N2 atmosphere (calcination is divided into pre-calcination and calcination, pre-calcination at 300°C, 4h, then heated to 600°C and calcined for 6h) to obtain a carbon-coated polyanionic sodium ion positive electrode material.

[0212] Comparative Example 1

[0213] The preparation method of the sodium ion battery provided in Comparative Example 1 is the same as the preparation method of the sodium ion battery provided in Example 7, except that:

[0214] In step 1), sodium alginate is not used to prepare alginic acid. Only 40 parts of sodium carbonate, 30 parts of ferrous oxalate and 30 parts of ammonium phosphate are weighed, added into 5000 mL of deionized water-ethanol solution (water: ethanol = 1: 1) and stirred for half an hour to obtain a uniformly mixed solution, and 1% glucose is added to obtain a mixed solution; then the mixed solution is calcined under N2 atmosphere (calcination is divided into pre-calcination and calcination, pre-calcination at 300°C for 4h, then the temperature is raised to 600°C and calcined for 6h) to obtain a carbon-coated polyanionic sodium ion positive electrode material;

[0215] In step 2), only glucose is dissolved in tetrahydrofuran, stirred and dried, and then carbonized at 1200° C. under argon protection and then cooled to obtain a hard carbon negative electrode material.

[0216] Test Case

[0217] 1. XRD test was performed on the negative electrode materials prepared at different carbonization treatment temperatures provided in Examples 1, 4, 5, 6 and 7, and the test results were as follows: Figure 2 shown.

[0218] Depend on Figure 2 It can be seen that the main diffraction peaks are usually located at 2θ angles of about 26° and 44°, which are the positions of the (002) peak and the (004) peak respectively. The interplanar spacing (also known as interlayer spacing) of the (002) peak is represented by d002, which is given by Figure 2 It can be seen that the interlayer spacing varies with temperature.

[0219] 2. The interlayer spacing of the hard carbon of the negative electrode materials prepared at different carbonization treatment temperatures provided in Examples 1, 4, 5, 6 and 7 was tested, and the test results were shown in Table 1 below:

[0220] Table 1

[0221]

[0222] Among them, the test method of the interlayer spacing of hard carbon in Table 1 is as follows: The test method of interlayer spacing of hard carbon mainly relies on X-ray diffraction (XRD) analysis. In the XRD spectrum of hard carbon materials, one or more diffraction peaks related to the carbon interlayer spacing are usually observed. There is a certain relationship between the position of these diffraction peaks (i.e., the diffraction angle) and the carbon interlayer spacing, which can be described by the Bragg's Law: 2dsinθ=nλ, where (d) is the average interlayer spacing of the carbon layer, (sinθ) is the angle between the incident angle of the X-ray and the diffraction peak, (λ) is the wavelength of the X-ray, and (n) is the diffraction order (usually an integer). Through this equation, we can calculate the interlayer spacing of the hard carbon material based on the position of the diffraction peak.

[0223] As shown in Table 1, by controlling the temperature of the carbonization treatment in the range of 800~1200℃, the interlayer spacing of the hard carbon can be increased, thereby facilitating the insertion and extraction of sodium ions.

[0224] 3. The rate discharge performance of the sodium ion batteries provided in Examples 1 to 15 and Comparative Example 1 was tested. The test results are shown in Table 2 below. The test method is as follows:

[0225] (1) Charge the experimental cell at 25°C ±3 at a constant current and constant voltage rate of 0.5C to 4.0V, with a cut-off current of 0.02C;

[0226] (2) Leave for 30 minutes;

[0227] (3) At 25℃±3, discharge at a constant current of 1C to 2.0V, and record the capacity at this time as D1;

[0228] (4) Leave for 30 minutes;

[0229] (5) Charge at a constant current and constant voltage rate of 1C to 4.0V, with a cut-off voltage of 0.02C;

[0230] (6) Leave for 30 minutes;

[0231] (7) Discharge at a constant current of 0.5C to 2.0V, and record the capacity at this time as D2;

[0232] (8) Leave for 30 minutes;

[0233] (9) Charge at a constant current and constant voltage rate of 1C to 4.0V, with a cut-off voltage of 0.02C;

[0234] (10) Leave for 30 minutes;

[0235] (11) Discharge at a constant current of 5C to 2.0V, and record the capacity at this time as D3;

[0236] (12) Leave for 30 minutes;

[0237] (13) Charge at a constant current and constant voltage rate of 1C to 4.0V, with a cut-off voltage of 0.02C;

[0238] (14) Leave for 30 minutes;

[0239] (15) Discharge at a constant current of 10C to 2.0V, and record the capacity at this time as D4;

[0240] The discharge rate capacity retention rate is calculated using the formula D=Dx / D1*100%, where x is 1~4.

[0241] 4. The room temperature cycle performance of the sodium ion batteries provided in Examples 1 to 15 and Comparative Example 1 was tested. The test results are shown in Table 2 below. The test method is as follows:

[0242] (1) Charge the experimental cell at 25°C ±3 at a constant current and constant voltage rate of 0.5C to 4.0V, with a cut-off current of 0.02C;

[0243] (2) Leave for 30 minutes;

[0244] (3) At 25℃±3, discharge at a constant current of 1C to 2.0V, and record the capacity D1 at this time;

[0245] (4) Leave for 30 minutes;

[0246] (5) Repeat (1) to (4) above and record the number of cycles and the final discharge capacity as Dy, where y is 500.

[0247] Among them, the cycle capacity retention rate is calculated using the formula D=Dy / D1*100%.

[0248] Table 2

[0249]

[0250] It can be seen from Table 2 that when the polyanionic iron-based positive electrode material provided in the embodiment of the present application is used as the positive electrode active material, the discharge capacity retention rate and the cycle capacity retention rate of the battery are greatly improved. When the hard carbon negative electrode material provided in the embodiment of the present application is used as the negative electrode active material, the discharge capacity retention rate and the cycle capacity retention rate of the battery are also greatly improved. When the polyanionic iron-based positive electrode material provided in the embodiment of the present application is used as the positive electrode active material and the hard carbon negative electrode material provided in the embodiment of the present application is used as the negative electrode active material at the same time, the improvement effect of the discharge capacity retention rate and the cycle capacity retention rate of the battery is the most obvious.

[0251] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0252] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A method for preparing a polyanionic iron-based positive electrode material, characterized in that: include: preparing alginate fibers; In the presence of the alginate fibers, a sodium source, an iron source and a phosphorus source are reacted to generate a polyanionic iron-based positive electrode material.

2. The preparation method according to claim 1, characterized in that: The method for preparing alginate fiber comprises: preparing sodium alginate spinning solution; Spraying the sodium alginate spinning solution into a calcium chloride aqueous solution through spinning to exchange ions between the sodium ions in the sodium alginate and the calcium ions in the calcium chloride to prepare the calcium alginate fibers; The calcium alginate fiber is immersed in a hydrochloric acid solution to allow calcium ions in the calcium alginate fiber to exchange ions with hydrogen ions in the hydrochloric acid, thereby preparing the alginate fiber.

3. The preparation method according to claim 2, characterized in that: The preparation method satisfies at least one of the following conditions: (1) In the sodium alginate spinning solution, the mass proportion of the sodium alginate is 3% to 10%; (2) In the calcium chloride aqueous solution, the mass proportion of calcium chloride is 3% to 10%; (3) The concentration of the hydrochloric acid solution is 0.5 mol / L to 1.2 mol / L; (4) The calcium ions in the calcium alginate fibers are exchanged with the hydrogen ions in the hydrochloric acid under heating, wherein the heating temperature is 50° C. to 80° C. and the heating time is 2 h to 10 h.

4. The preparation method according to any one of claims 1 to 3, characterized in that The sodium source includes sodium carbonate, the iron source includes ferrous oxalate, and the phosphorus source includes one or more of phosphate and pyrophosphate; Optionally, the phosphate is ammonium phosphate.

5. The preparation method according to any one of claims 1 to 3, characterized in that The polyanionic iron-based positive electrode material further includes a carbon coating layer; in the presence of alginate fibers, a sodium source, an iron source and a phosphorus source are reacted to generate a polyanionic iron-based positive electrode material, including: The alginate fiber is immersed in a solution containing a sodium source, an iron source and a phosphorus source, and an organic carbon source is added to prepare a first mixed solution; The first mixed solution is calcined to prepare the polyanionic iron-based positive electrode material containing the carbon coating layer.

6. The preparation method according to claim 5, characterized in that: The preparation method satisfies at least one of the following conditions: (1) The solvent used in the solution containing the sodium source, the iron source and the phosphorus source is a mixed solvent of water and ethanol; (2) The organic carbon source includes glucose; (3) the molar ratio of the sodium element in the sodium source, the iron element in the iron source and the phosphorus element in the phosphorus source is (0.7-4.0): (0.3-3.0): (0.3-3.0); (4) The calcination is carried out under the protection of an inert gas, and the calcination temperature is 600° C. to 900° C., and the calcination time is 6 h to 12 h.

7. A polyanionic iron-based positive electrode material, characterized in that: The method is prepared according to any one of claims 1 to 6.

8. The polyanionic iron-based positive electrode material according to claim 7, characterized in that: The positive electrode material in the polyanionic iron-based positive electrode material satisfies at least one of the following conditions: (1) The proportion of Fe-Na antisite defects in the polyanionic iron-based positive electrode material is less than or equal to 0.3%; (2) The specific surface area of ​​the polyanionic iron-based positive electrode material is 10.2 m2 / g~52.3 m2 / g; (3) The median particle size D50 of the polyanionic iron-based positive electrode material is 1.5 μm to 6 μm; (4) The polyanionic iron-based positive electrode material further includes a carbon coating layer, and the mass proportion of the carbon coating layer in the polyanionic iron-based positive electrode material is 0.5% to 2%.

9. A positive electrode sheet, characterized in that: It comprises a positive electrode current collector and a positive electrode material arranged on at least one side of the positive electrode current collector along the thickness direction thereof, wherein the positive electrode material comprises the polyanionic iron-based positive electrode material as described in any one of claims 7 to 8.

10. A method for preparing a negative electrode material, characterized in that: include: preparing a second mixed solution of a sugar carbon source and an organic nitrogen source; In a protective gas atmosphere, carbonizing the second mixed solution to prepare the negative electrode material; Wherein, the temperature of the carbonization treatment is 800°C~1500°C, and the time is 1 h~5 h.

11. The preparation method according to claim 10, characterized in that: The preparation method satisfies at least one of the following conditions: (1) The carbohydrate carbon source includes: one or more of glucose, sucrose and starch; optionally, the carbohydrate carbon source is glucose; (2) The organic nitrogen source comprises: one or more of melamine, dicyandiamide and urea. Optionally, the organic nitrogen source is melamine; (3) The protective gas includes at least one of nitrogen, helium, neon and argon.

12. A negative electrode material, characterized in that: The method is described in any one of claims 10 to 11.

13. The negative electrode material according to claim 12, characterized in that: The negative electrode material satisfies at least one of the following conditions: (1) The interlayer spacing of the hard carbon in the negative electrode material is 0.374 nm to 0.40 nm; (2) The median particle size D50 of the hard carbon in the negative electrode material is 4 μm to 8.0 μm; (3) The specific surface area of ​​the hard carbon in the negative electrode material is ≤0.03 m2 / g; (4) The ash content of the hard carbon in the negative electrode material is ≤0.1%.

14. A negative electrode plate, characterized in that: It comprises a negative electrode current collector and a negative electrode material arranged on at least one side of the negative electrode current collector along the thickness direction thereof, wherein the negative electrode material is the negative electrode material according to any one of claims 12 to 13.

15. A sodium ion battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the positive electrode sheet is the positive electrode sheet as claimed in claim 9, and the negative electrode sheet is the negative electrode sheet as claimed in claim 14.

16. A battery module, characterized in that: It comprises a plurality of batteries connected in series and / or in parallel, and at least one battery is the sodium ion battery as claimed in claim 15.

17. An electrical device, characterized in that: Comprising the battery module as claimed in claim 16.