Preparation method of high-flame-retardant insulating battery diaphragm
Through the combination of meta-aramid fiber and phosphorus-nitrogen polymer, combined with nano-silica and nano-titanium dioxide, a highly flame-retardant insulating battery separator is prepared, which solves the problem of low flame retardancy level of existing battery separators and achieves low-cost, high-efficiency The high flame retardant performance improves the safety performance of new energy vehicles.
Patent Information
- Application Number
- CN202411092592.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-25
AI Technical Summary
The flame retardant level of existing battery separators is low and cannot meet the needs of the new energy automobile industry for high flame retardant performance. The high cost and technology monopoly of relying on imported flame retardant insulation sheets has restricted the development of the industry.
It uses a mixed slurry of meta-aramid chopped fiber, para-aramid chopped fiber and meta-aramid fibrid fiber, and combines amino-containing phosphorus nitrogen polymer and nano diamine through wet molding and hot pressing molding processes. Silicon oxide and nano-titanium dioxide are used to prepare highly flame-retardant insulating battery separators.
Low-cost, efficient preparation of highly flame-retardant insulating battery separators has been achieved. The product has passed the UL94 flame-retardant test and reached 5VA level. It is not easy to burn and has strong flame self-extinguishing ability, which improves the safety performance of new energy vehicles.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of battery separators, and in particular to a method for preparing a highly flame-retardant insulating battery separator. Background Art
[0002] The development and application of highly flame-retardant special aramid insulation paper is an important research direction in the field of aramid paper. Traditional poly(m-phenylene isophthalamide) fiber paper (aramid 1313) has good insulation and flame-retardant properties, and has important applications in many fields such as electrical insulation, aerospace, transportation, national defense and military industry. For a long time, the main demand for aramid paper in my country has been concentrated in the field of electrical insulation, and this application scenario pays more attention to dielectric strength. With the continuous development of the new energy vehicle industry, the demand for aramid paper that can be used in power batteries continues to increase. In addition to insulation properties, it puts forward new requirements for the flame-retardant properties of aramid paper. Therefore, the development of special aramid insulation paper with high flame-retardant properties that meets the development trend of the times has become a hot topic in the field of aramid paper research.
[0003] Although traditional aramid paper has certain flame retardant properties and can be self-extinguished when away from fire, it still burns or even burns through in a continuous flame. Therefore, in the flame retardant test, the flame retardant grade of traditional aramid paper is low, and there is still a lot of room for improvement in flame retardant properties. At present, the development of highly flame-retardant special aramid insulation paper in China is still in its infancy. In the international market, similar products are called flame retardant insulation sheets, which are materials used for fire safety and electrical insulation with excellent flame retardant ability and good electrical properties. There are many types of flame retardant insulation sheets, mainly represented by the FRB series products of 3M Company in the United States. FRB is a flexible insulation product, mainly composed of inorganic materials. It can provide excellent flame retardant ability while maintaining good insulation performance. It is suitable for safety fields including electrical hazards and meets the flame retardant certification standards of UL94V-0 or UL94 5VA.
[0004] Although the performance of flame-retardant insulation sheets is relatively excellent, such products need to rely on foreign imports. Their high prices and technology monopoly will seriously restrict the development of related industries. Therefore, it is imperative to develop highly flame-retardant special aramid insulation paper with similar performance to flame-retardant insulation sheets and in compliance with the UL94 V-0 or UL94 5VA flame-retardant certification standards. This type of aramid paper can not only be used in the booming new energy vehicle industry, but its application areas can also be continuously expanded as the technology matures.
[0005] In the prior art, many battery separators containing aramid fibers have low flame retardancy. For example, the aramid-coated lithium battery separator disclosed in Chinese patent CN110391383A improves flame retardancy by combining the flame retardancy of aramid fibers and metal oxide fillers; the self-flame-retardant lithium-ion battery separator disclosed in Chinese patent CN205723721U improves flame retardancy by combining the flame retardancy of aramid fibers and the effect of accelerated cooling by microporous structures. However, the flame retardancy level still cannot exceed 5VB.
[0006] Therefore, it is necessary to improve the preparation method to solve the above problems. Summary of the invention
[0007] The main purpose of the present invention is to provide a method for preparing a highly flame-retardant insulating battery separator, which can obtain a battery separator material with high flame retardancy.
[0008] The present invention achieves the above-mentioned object through the following technical scheme: A method for preparing a highly flame-retardant insulating battery separator, comprising the steps of:
[0009] S1. Slurry preparation: dispersing meta-aramid chopped fibers, para-aramid chopped fibers and meta-aramid fibrids in water, adding a dispersant and stirring the mixture to obtain aramid fiber mixed slurry;
[0010] S2, wet forming: the aramid fiber mixed slurry is subjected to wet papermaking, and after water filtering, pressing and vacuum drying, aramid base paper is obtained;
[0011] S3, preparation of flame retardant solution: adding amino-containing phosphorus-nitrogen polymer, nano-silicon dioxide and nano-titanium dioxide into deionized water to prepare a flame retardant solution;
[0012] S4, impregnation treatment: impregnating the aramid base paper in the flame retardant solution, taking it out and drying it to obtain a semi-finished aramid paper;
[0013] S5, hot pressing molding: subjecting the semi-finished aramid paper to hot pressing treatment to obtain a highly flame-retardant insulating battery separator.
[0014] Specifically, the length of the meta-aramid chopped fibers and the para-aramid chopped fibers is 3-6 mm, the linear density is 2-5 dtex, the addition amount of the meta-aramid chopped fibers is 10-50wt%, the addition amount of the para-aramid chopped fibers is 10-50wt%, and the addition amount of the meta-aramid fibrid is 40-50wt%.
[0015] Specifically, the dispersant is carboxymethyl cellulose and cationic polyacrylamide, and the concentration of the dispersant in the aramid fiber mixed slurry is 0.2-0.6wt%.
[0016] Specifically, the basis weight of the aramid base paper is 50-100 g / m 2 .
[0017] Specifically, the pressing pressure in step S2 is 0.4 MPa, the pressing time is 2-5 min, the vacuum pressure during drying is -0.09 MPa, the drying temperature is 90-120° C., and the drying time is 10-15 min.
[0018] Specifically, the concentration of the flame retardant solution is 10-20wt%.
[0019] Specifically, the immersion time in step S4 is 3-5 minutes, the drying temperature is 80-100° C., and the drying time is 10-20 minutes.
[0020] Specifically, the hot pressing temperature in step S5 is 160-220° C., the hot pressing pressure is 6-15 MPa, and the hot pressing time is 3-5 min.
[0021] The beneficial effects of the technical solution of the present invention are:
[0022] 1. The technical solution of the present invention provides a simple, effective, mature and low-cost papermaking process for preparing highly flame-retardant insulating battery separators. The reagents used are all conventional medicines, which are non-toxic and low-priced.
[0023] 2. The product of the present invention can not only reflect the performance advantages of each raw material itself, but also use aramid short fibers and phosphorus nitrogen polymer as bonding materials to enhance the bonding force between fibers, and nano-silicon dioxide and nano-titanium dioxide can be filled in the pores of the fibers to improve the overall mechanical properties of the aramid paper.
[0024] 3. The product of the present invention can pass the UL94 flame retardant grade test and has a flame retardant grade of 5VA. It is not easy to burn and has a strong flame self-extinguishing ability. It can prevent the occurrence of combustion problems caused by thermal runaway of lithium batteries during use, thereby improving the safety performance of new energy vehicles. It has great potential to become a new generation of new energy vehicle power battery coating materials. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below with reference to specific embodiments.
[0026] Example 1
[0027] S1. Slurry preparation: according to the quantitative 100g / m 2Carry out fiber proportioning, take 20 parts by mass of meta-aramid short fibers, 30 parts by mass of para-aramid short fibers and 50 parts by mass of meta-aramid precipitated fibers, the length of meta-aramid short fibers and para-aramid short fibers are 3-6 mm, the linear density is 2-5 dtex, disperse and stir in water for 15000 r, then add CMC (carboxymethyl cellulose) with a mass concentration of 0.5% and CPAM (cationic polyacrylamide) with a mass concentration of 0.2%, continue stirring for 20000 r, and obtain aramid fiber mixed slurry.
[0028] S2, wet forming: pour the mixed slurry dispersed in step S1 into the forming barrel of the sheet making machine, and obtain wet paper sheets after filtering. Press the wet paper sheets at a pressure of 0.4 MPa for 4 minutes, and then put them into a vacuum dryer for drying. The vacuum pressure is -0.09 MPa, the drying temperature is 90°C, and the drying time is 10 minutes to obtain aramid base paper.
[0029] S3. Preparation of flame retardant solution: 20 parts by mass of amino-containing phosphorus-nitrogen polymer, 5 parts by mass of nano-silicon dioxide and 5 parts by mass of nano-titanium dioxide are added to 200 parts by mass of deionized water to prepare a flame retardant solution and pour it into a tray.
[0030] S4, impregnation treatment: the aramid base paper prepared in step S2 is immersed in a flame retardant solution for 3 minutes, and then placed in an oven and dried at 90° C. for 10 minutes to obtain a semi-finished aramid paper.
[0031] S5, hot pressing treatment: put the semi-finished aramid paper prepared in step S4 into a hot pressing roller for hot pressing treatment, the hot pressing temperature is 200°C, the hot pressing time is 3 minutes, after the hot pressing is completed, wait for it to cool to room temperature to obtain a highly flame-retardant insulating battery separator.
[0032] Example 2
[0033] S1. Slurry preparation: according to the quantitative 100g / m 2 Carry out fiber proportioning, take 20 parts by mass of meta-aramid chopped fibers, 20 parts by mass of para-aramid chopped fibers and 60 parts by mass of meta-aramid precipitated fibers, the length of meta-aramid chopped fibers and para-aramid chopped fibers are 3-6 mm, the linear density is 2-5 dtex, dissolve and stir in water for 15000 r, then add CMC with a mass concentration of 0.5% and CPAM with a mass concentration of 0.2%, continue stirring for 20000 r, and obtain aramid fiber mixed slurry.
[0034] S2, wet forming: pour the mixed slurry dispersed in step S1 into the forming barrel of the sheet making machine, and obtain wet paper sheets after filtering. Press the wet paper sheets at a pressure of 0.4 MPa for 4 minutes, and then put them into a vacuum dryer for drying. The vacuum pressure is -0.09 MPa, the drying temperature is 90°C, and the drying time is 10 minutes to obtain aramid base paper.
[0035] S3. Preparation of flame retardant solution: 20 parts by mass of amino-containing phosphorus-nitrogen polymer, 5 parts by mass of nano-silicon dioxide and 5 parts by mass of nano-titanium dioxide are added to 200 parts by mass of deionized water to prepare a flame retardant solution and pour it into a tray.
[0036] S4, impregnation treatment: the aramid base paper prepared in step S2 is immersed in a flame retardant solution for 3 minutes, and then placed in an oven and dried at 90° C. for 10 minutes to obtain a semi-finished aramid paper.
[0037] S5, hot pressing treatment: put the semi-finished aramid paper prepared in step S4 into a hot pressing roller for hot pressing treatment, the hot pressing temperature is 200°C, the hot pressing time is 3 minutes, after the hot pressing is completed, wait for it to cool to room temperature to obtain a highly flame-retardant insulating battery separator.
[0038] Example 3
[0039] S1. Slurry preparation: according to the quantitative 100g / m 2 Carry out fiber proportioning, take 20 parts by mass of meta-aramid short fibers, 30 parts by mass of para-aramid short fibers and 50 parts by mass of meta-aramid precipitated fibers, the length of meta-aramid short fibers and para-aramid short fibers are 3-6 mm, the linear density is 2-5 dtex, dissolve and stir in water for 15000 r, then add CMC with a mass concentration of 0.5% and CPAM with a mass concentration of 0.2%, continue stirring for 20000 r, and obtain aramid fiber mixed slurry.
[0040] S2, wet forming: pour the mixed slurry dispersed in step S1 into the forming barrel of the sheet making machine, and obtain wet paper sheets after filtering. Press the wet paper sheets at a pressure of 0.4 MPa for 4 minutes, and then put them into a vacuum dryer for drying. The vacuum pressure is -0.09 MPa, the drying temperature is 90°C, and the drying time is 10 minutes to obtain aramid base paper.
[0041] S3. Preparation of flame retardant solution: 10 parts by mass of amino-containing phosphorus-nitrogen polymer, 5 parts by mass of nano-silicon dioxide and 5 parts by mass of nano-titanium dioxide are added to 200 parts by mass of deionized water to prepare a flame retardant solution and pour it into a tray.
[0042] S4, impregnation treatment: the aramid base paper prepared in step S2 is immersed in a flame retardant solution for 3 minutes, and then placed in an oven and dried at 90° C. for 10 minutes to obtain a semi-finished aramid paper.
[0043] S5, hot pressing treatment: put the semi-finished aramid paper prepared in step S4 into a hot pressing roller for hot pressing treatment, the hot pressing temperature is 200°C, the hot pressing time is 3 minutes, after the hot pressing is completed, wait for it to cool to room temperature to obtain a highly flame-retardant insulating battery separator.
[0044] Example 4
[0045] S1. Slurry preparation: according to the quantitative 60g / m 2 Carry out fiber proportioning, take 20 parts by mass of meta-aramid short fibers, 30 parts by mass of para-aramid short fibers and 50 parts by mass of meta-aramid precipitated fibers, the length of meta-aramid short fibers and para-aramid short fibers are 3-6 mm, the linear density is 2-5 dtex, dissolve and stir in water for 15000 r, then add CMC with a mass concentration of 0.5% and CPAM with a mass concentration of 0.2%, continue stirring for 20000 r, and obtain aramid fiber mixed slurry.
[0046] S2, wet forming: pour the mixed slurry dispersed in step S1 into the forming barrel of the sheet making machine, and obtain wet paper sheets after filtering. Press the wet paper sheets at a pressure of 0.4 MPa for 4 minutes, and then put them into a vacuum dryer for drying. The vacuum pressure is -0.09 MPa, the drying temperature is 90°C, and the drying time is 10 minutes to obtain aramid base paper.
[0047] S3. Preparation of flame retardant solution: 20 parts by mass of amino-containing phosphorus-nitrogen polymer, 5 parts by mass of nano-silicon dioxide and 5 parts by mass of nano-titanium dioxide are added to 200 parts by mass of deionized water to prepare a flame retardant solution and pour it into a tray.
[0048] S4, impregnation treatment: the aramid base paper prepared in step S2 is immersed in a flame retardant solution for 3 minutes, and then placed in an oven and dried at 90° C. for 10 minutes to obtain a semi-finished aramid paper.
[0049] S5, hot pressing treatment: put the semi-finished aramid paper prepared in step S4 into a hot pressing roller for hot pressing treatment, the hot pressing temperature is 200°C, the hot pressing time is 3 minutes, after the hot pressing is completed, wait for it to cool to room temperature to obtain a highly flame-retardant insulating battery separator.
[0050] The technical solution of the present invention provides a simple, effective, mature and low-cost papermaking process for preparing highly flame-retardant insulating battery separators. The reagents used are all conventional medicines, which are non-toxic and low-priced.
[0051] The main raw materials used in this process include a variety of aramid fibers (meta-aramid chopped fibers, para-aramid chopped fibers and meta-aramid precipitated fibers), amino-containing phosphorus-nitrogen polymers (obtained by the reaction of tetrakis(hydroxymethyl)phosphonium sulfate and ammonia water), and inorganic oxides (nano-silicon dioxide and nano-titanium dioxide). These substances are all excellent flame retardants, but their flame retardant principles are slightly different:
[0052] ① The molecular structure of aramid fiber includes stable aromatic rings, which are not easy to burn; the thermal conductivity coefficient is low, making it difficult for heat to diffuse; aramid fiber is easily carbonized at high temperatures, releasing carbon dioxide and water vapor, thereby forming a protective layer that isolates oxygen.
[0053] ② When thermally decomposed at high temperature, phosphorus-nitrogen polymers will form a porous carbon layer that isolates oxygen; the decomposition will produce non-combustible gases (such as carbon dioxide, nitrogen, etc.), thereby diluting the concentration of combustible gases and reducing the combustion rate; the decomposition reaction will absorb a large amount of heat, reduce the surface temperature of the material, and delay the combustion process; certain active groups (such as PO·, N·, etc.) produced by the decomposition of phosphorus-nitrogen polymers can capture free radicals in the combustion process, interrupt the combustion chain reaction, and play a chemical inhibition role.
[0054] ③Inorganic oxides themselves cannot burn, but only absorb heat and form an inorganic oxide film on the surface to prevent the spread of flames.
[0055] Comparative Examples 1-9 were prepared as follows and compared with Examples 1-4.
[0056] Comparative Example 1
[0057] Other conditions are the same as those in Example 1, except that the chopped fibers in step S1 are all meta-aramid fibers.
[0058] Comparative Example 2
[0059] Other conditions are the same as those in Example 1, except that the chopped fibers in step S1 are all para-aramid fibers.
[0060] Comparative Example 3
[0061] The other conditions are the same as those in Example 1, except that the immersion treatment in step S3 is omitted.
[0062] Comparative Example 4
[0063] The other conditions are the same as those in Example 1, except that the flame retardant solution in step S3 is composed only of phosphorus-nitrogen polymer, without nano-silicon dioxide and nano-titanium dioxide.
[0064] Comparative Example 5
[0065] The other conditions are the same as those in Example 1, except that the flame retardant solution in step S3 is composed only of nano-silicon dioxide, without phosphorus nitrogen polymer and nano-titanium dioxide.
[0066] Comparative Example 6
[0067] The other conditions are the same as those in Example 1, except that the flame retardant solution in step S3 is composed only of nano-titanium dioxide, without phosphorus nitrogen polymer and nano-silicon dioxide.
[0068] Comparative Example 7
[0069] The other conditions are the same as those in Example 1, except that the flame retardant solution in step S3 is composed only of phosphorus nitrogen polymer and nano-silicon dioxide, without nano-titanium dioxide.
[0070] Comparative Example 8
[0071] The other conditions are the same as those in Example 1, except that the flame retardant solution in step S3 is composed only of phosphorus nitrogen polymer and nano-titanium dioxide, without nano-silicon dioxide.
[0072] Comparative Example 9
[0073] The other conditions are the same as those in Example 1, except that the flame retardant solution in step S3 is composed only of nano-silicon dioxide and nano-titanium dioxide, and contains no phosphorus-nitrogen polymer.
[0074] The test method is as follows and the results are shown in Table 1.
[0075] Flame retardant grade: UL94 flame retardant grade test standard.
[0076] Heat resistance: GB / T 11026.1-2003 "Heat resistance of electrical insulating materials Part 1: Aging procedures and evaluation of test results".
[0077] Tensile strength and elongation at break: GB / T 12914-2018 "Determination of tensile strength of paper and paperboard - Constant rate of tension (20 mm / min)".
[0078] Thermal shrinkage: GB / T 20629.2-2013 "Non-cellulose paper for electrical use Part 2: Test method".
[0079] Table 1 Performance indexes of high flame retardant insulating battery separators
[0080]
[0081] Note: According to the UL94 flame retardant grade test standard, the specific flame retardant grades from low to high are HB, V-2, V-1, V-0, 5VB, and 5VA.
[0082] Table 1 shows the influence of each component on the overall performance of the product:
[0083] ① From the mechanical properties, it can be compared that the best mechanical property is in control example 2, slightly higher than in embodiments 1-4, control example 1 has very poor tensile strength and thermal stability, control examples 3-6 and control example 9 have good tensile strength but poor thermal stability, and control examples 7 and 8 have high thermal stability.
[0084] The reason for the above results is that there is only meta-aramid fiber in control example 1, and its structural characteristics are that the groups on the aromatic ring are in a meta-position relationship. After polymerization, the molecule presents a multi-turn structure, with large internal gaps and easy rotation of the bond position, so it is easier to be stretched and more easily deformed by heat. After the polymerization of para-aramid, the molecule presents a linear structure, which is easy to stack, and the molecular structure is stable, and it is not easy to be stretched and deformed by heat. After mixing multiple aramid fibers, the mechanical properties are between the two. Because the polymerization principle of aramid fiber is the process of amino-NH2 and carboxyl-COOH dehydration condensation to form peptide bond-CONH-, in the case of incomplete reaction, there will still be free carboxyl groups on the fiber surface, and there will be free amino groups on the phosphorus nitrogen polymer, which can be dehydrated and polymerized again with the carboxyl groups on the aramid fiber at a temperature not exceeding 100°C, so that there are fewer free radicals on the aramid fiber, more crosslinking is produced, and the decomposition difficulty is increased, so the thermal stability can be improved.
[0085] ② From the flame retardant performance, it can be compared that the worst flame retardant performance is the product without impregnation treatment (Control Example 3), the lower ones are the products in which the flame retardant solution contains only one component (Control Examples 4-6) and the flame retardant solution contains nano-silicon dioxide and nano-titanium dioxide (Control Example 9), the higher ones are the products lacking nano-titanium dioxide or nano-silicon dioxide (Control Examples 7 and Control Examples 8), and the highest is the embodiment.
[0086] The reasons for the above results are: nano-titanium dioxide is a larger molecule, and nano-silicon dioxide is a smaller molecule, so the molecules of nano-silicon dioxide can occupy the gaps of nano-titanium dioxide, produce a coordination effect, and help improve the flame retardant properties; aramid base paper is made of triple aramid fibers, and the reaction of the three fibers will produce tiny holes in the fiber structure, which can be filled with small molecules, and nitrogen-phosphorus polymers are macromolecular materials that can react with the free radicals of aramid fibers, so the reaction of phosphorus-nitrogen polymers with aramid fibers not only improves the tensile properties of the product, but also locks nano-silicon dioxide and nano-titanium dioxide in the holes of aramid fibers, so phosphorus-nitrogen polymers can help improve the filling rate of the aramid base paper surface and reduce free radicals, thereby reflecting better flame retardant properties.
[0087] In summary, this aramid paper can not only reflect the performance advantages of each raw material itself, but also use aramid short fibers and phosphorus nitrogen polymer as bonding materials to enhance the bonding force between fibers, and nano-silicon dioxide and nano-titanium dioxide can be filled in the pores of the fibers to improve the overall mechanical properties of the aramid paper. The product can pass the UL94 flame retardant grade test, has a flame retardant grade of 5VA, is not easy to burn, and has a strong flame self-extinguishing ability. It can prevent the occurrence of combustion problems when lithium batteries are thermally runaway during use, thereby improving the safety performance of new energy vehicles, and has great potential to become a new generation of new energy vehicle power battery coating materials.
[0088] The above are only some embodiments of the present invention. For ordinary operators in this field, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing a highly flame-retardant insulating battery separator, characterized in that the steps include: S1. Slurry preparation: dispersing meta-aramid chopped fibers, para-aramid chopped fibers and meta-aramid fibrids in water, adding a dispersant and stirring the mixture to obtain aramid fiber mixed slurry; S2, wet forming: the aramid fiber mixed slurry is subjected to wet papermaking, and after water filtering, pressing and vacuum drying, aramid base paper is obtained; S3, preparation of flame retardant solution: adding amino-containing phosphorus-nitrogen polymer, nano-silicon dioxide and nano-titanium dioxide into deionized water to prepare a flame retardant solution; S4, impregnation treatment: impregnating the aramid base paper in the flame retardant solution, taking it out and drying it to obtain a semi-finished aramid paper; S5, hot pressing molding: subjecting the semi-finished aramid paper to hot pressing treatment to obtain a highly flame-retardant insulating battery separator.
2. The method for preparing a highly flame-retardant insulating battery separator according to claim 1, characterized in that: The length of the meta-aramid chopped fibers and the para-aramid chopped fibers is 3-6 mm, and the linear density is 2-5 dtex. The addition amount of the meta-aramid chopped fibers is 10-50 wt%, the addition amount of the para-aramid chopped fibers is 10-50 wt%, and the addition amount of the meta-aramid fibrids is 40-50 wt%.
3. The method for preparing the highly flame-retardant insulating battery separator according to claim 1, characterized in that: The dispersant is carboxymethyl cellulose and cationic polyacrylamide, and the concentration of the dispersant in the aramid fiber mixed slurry is 0.2-0.6wt%.
4. The method for preparing a highly flame-retardant insulating battery separator according to claim 1, characterized in that: The basis weight of the aramid base paper is 50-100 g / m 2 .
5. The method for preparing a highly flame-retardant insulating battery separator according to claim 1, characterized in that: The pressing pressure in step S2 is 0.4 MPa, the pressing time is 2-5 min, the vacuum pressure during drying is -0.09 MPa, the drying temperature is 90-120° C., and the drying time is 10-15 min.
6. The method for preparing a highly flame-retardant insulating battery separator according to claim 1, characterized in that: The concentration of the flame retardant solution is 10-20 wt %.
7. The method for preparing a highly flame-retardant insulating battery separator according to claim 1, characterized in that: The immersion time in step S4 is 3-5 minutes, the drying temperature is 80-100° C., and the drying time is 10-20 minutes.
8. The method for preparing a highly flame-retardant insulating battery separator according to claim 1, characterized in that: The hot pressing temperature in step S5 is 160-220° C., the hot pressing pressure is 6-15 MPa, and the hot pressing time is 3-5 min.
Citation Information
Patent Citations
Preparation method of aramid fiber coated lithium battery diaphragm
CN110391383A
From fire -retardant lithium ion battery diaphragm
CN205723721U
Preparation method of para-aramid and meta-aramid electrical insulation paper
CN106223129A
Phosphorus-nitrogen containing polymer modified silicon dioxide nanoparticle and preparation method and application thereof
CN106832413A
Polyhydroxy benzene ring phosphorus-nitrogen type flame retardant, manufacturing method and application thereof in flame retardant polyurethane hard bubble material
CN108285523A
Cited By
High-flame-retardant aramid paper and preparation method thereof
CN121228560A
Cellulose-based sodium ion diaphragm with double-layer structure and preparation method of cellulose-based sodium ion diaphragm
CN121566055A
A cellulose-based sodium ion separator with a double-layer structure and its preparation method
CN121566055B