Atomizing core and preparation method thereof
By adding high thermal conductivity filler to the preparation method of the atomizer core and adopting hot-pressure injection molding and degreasing sintering processes, the problems of burning and taste attenuation caused by the low thermal conductivity of the existing atomizer core are solved, and a more uniform thermal field is achieved. temperature and greater taste consistency for high power and high volume applications.
Patent Information
- Application Number
- CN202410985863.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The thermal conductivity of the existing atomizing core is low, which results in the concentration of heat during atomization, which easily causes burning, bitterness and taste attenuation, reducing the consistency of the taste.
High thermal conductivity fillers, such as diamond, silicon carbide and alumina, are added to the preparation method of the atomizer core, uniformly mixed with aggregates, sintering additives and pore-forming agents, and prepared through hot-pressure injection molding and degreasing sintering processes to reduce the The sintering temperature and thermal field temperature improve the consistency of taste.
It effectively reduces the sintering temperature and the average atomization temperature, avoids burning phenomenon, improves the consistency of taste, and is suitable for high-power and large-capacity application conditions.
Smart Images

Figure CN118844684A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of atomization technology, and specifically relates to an atomization core and a preparation method thereof. Background Art
[0002] At present, the thermal conductivity of the atomizer core matrix in the atomizer core is relatively low. Although the heat is relatively concentrated during atomization and the taste burst is good, it is easy to cause burning, bitterness, and taste attenuation, which reduces the consistency of taste. Summary of the invention
[0003] In view of this, the first aspect of the present application provides a method for preparing an atomizer core, the preparation method comprising:
[0004] Providing a solute and a solvent, wherein the solute includes an aggregate, a high thermal conductivity filler, a sintering additive, and a pore-forming agent;
[0005] The solute is dried, and the dried solute and the solvent are treated with wax to obtain a mixed slurry;
[0006] Providing a heating sheet, processing the mixed slurry and the heating sheet through a hot injection molding process, so that the mixed slurry forms an atomizer core matrix embryo, and fixing the heating sheet to the atomizer core matrix embryo, to obtain an atomizer core embryo;
[0007] The atomizer core embryo is processed through a degreasing process and a sintering process to obtain an atomizer core.
[0008] The preparation method of the atomizer core provided in the first aspect of the present application is to add a high thermal conductivity filler with a high thermal conductivity coefficient to the solute so that it is fully and evenly mixed with other solute materials. First, in the sintering process, the addition of a high thermal conductivity filler can better transfer heat, thereby reducing the sintering temperature, and the inside of the atomizer core embryo can reach a preset temperature by using a lower sintering temperature. Secondly, due to the addition of a high thermal conductivity filler, the atomizer core can also better transfer the heat generated by the heating plate during operation. The temperature of the thermal field of the atomizer core is uniform, the taste is not easy to cause burning and the attenuation is small, which improves the consistency of the taste. In summary, the present application can reduce the sintering temperature, improve the consistency of taste, and is suitable for high-power and large-capacity application conditions.
[0009] Wherein, in the sintering process, the highest sintering temperature is less than 590°C.
[0010] Wherein, the high thermal conductivity filler includes at least one of diamond, silicon carbide, and aluminum oxide.
[0011] The mass of the solvent is 15%-40% of the sum of the mass of the solute and the mass of the solvent.
[0012] Wherein, by weight percentage, the solute includes 30-60 wt.% of aggregate, 5-10 wt.% of high thermal conductive filler, 10-30 wt.% of sintering additive, and 20-50 wt.% of pore former.
[0013] Wherein, the solvent comprises, by mass percentage, at least two of paraffin 5-10 wt.%, beeswax 0-5 wt.%, stearic acid 0-5 wt.%, polyethylene 0-5 wt.%, and ethylene-vinyl acetate copolymer 0-5 wt.%.
[0014] Wherein, when carrying out the wax treatment, the solvent is first melted, and then the solute is added into the melted solvent.
[0015] Wherein, when the atomization core embryo is processed through a degreasing process and a sintering process, the degreasing process and the sintering process are an integrated process.
[0016] The second aspect of the present application provides an atomizer core, which is prepared by the preparation method of the atomizer core provided by the first aspect of the present application.
[0017] The atomizer core provided in the second aspect of the present application is prepared by adopting the preparation method of the atomizer core provided in the first aspect of the present application. The thermal field temperature of the atomizer core is uniform, the taste is not easy to cause burning and the attenuation is small, the consistency of the taste is improved, and it is suitable for high-power and large-capacity application conditions.
[0018] Wherein, the average atomization temperature of the atomization core is less than 245°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the implementation modes of the present application, the drawings required for use in the implementation modes of the present application will be described below.
[0020] Figure 1 This is a process flow chart of a method for preparing an atomizer core in one embodiment of the present application.
[0021] Figure 2 It is a schematic diagram of the three-dimensional structure of the atomizer core in one embodiment of the present application.
[0022] Description of labels:
[0023] Atomizer core - 1, atomizer core base - 10, heating sheet - 20. DETAILED DESCRIPTION
[0024] The following are preferred implementations of the present application. It should be noted that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
[0025] Before introducing the technical solution of the present application, the technical problems in the related technology are introduced in detail.
[0026] At present, the ceramic core matrix is mainly made of diatomaceous earth or quartz sand, glass powder, pore formers and binders, and the fillers are mostly materials that enhance the structural strength. As a result, the sintering temperature of the ceramic atomizer core is high during the preparation process, and the thermal conductivity is very low. During atomization, the heat is relatively concentrated and the taste burst is good, but it is easy to cause burning, bitterness and taste attenuation.
[0027] In view of this, in order to solve the above problems, the present application provides a method for preparing an atomizer core. Figure 1 , Figure 1 The process flow chart of the method for preparing the atomizer core in one embodiment of the present application is shown in FIG. The method for preparing the atomizer core provided in this embodiment includes S100, S200, S300, and S400. The detailed introduction of S100, S200, S300, and S400 is as follows.
[0028] S100, providing a solute and a solvent, wherein the solute includes an aggregate, a high thermal conductive filler, a sintering additive, and a pore-forming agent.
[0029] In order to prepare the atomizer core, the atomizer core matrix can be prepared first. The preparation of the atomizer core matrix is mainly composed of two types of raw materials: solute and solvent. The solute is mainly various solid powders. The solute includes aggregates, high thermal conductivity fillers, sintering additives, and pore-forming agents. The raw materials of various components can be weighed according to needs, and the above raw materials can be evenly mixed together in a certain proportion, that is, mixed. Optionally, the solute solid powder can be weighed according to the mass ratio and placed on a three-dimensional mixer for mixing.
[0030] Among them, aggregate is the main component of the atomizer core matrix, the sintering additive is mainly used to bond various aggregates together in the subsequent sintering process to make it better shaped, and the pore-forming agent is mainly used to help the atomizer core matrix to form pores. The above three components are the main components of the atomizer core matrix in the related art, and result in a very low thermal conductivity. The heat is relatively concentrated during atomization and the taste burst is good, but it is easy to cause burning, bitterness, and taste attenuation. Therefore, this embodiment adds a high thermal conductivity filler on this basis. As the name suggests, the high thermal conductivity filler is a material with a high thermal conductivity, which can effectively solve the above problems. As for how to solve them specifically, it will be described in detail below.
[0031] In this embodiment, the solute includes 30-60wt.% aggregate, 5-10wt.% high thermal conductive filler, 10-30wt.% sintering additive, and 20-50wt.% pore-forming agent by mass percentage. The formula components of this embodiment are non-toxic and harmless, economical and environmentally friendly, and an atomizer core with excellent comprehensive performance can be prepared by the above formula.
[0032] In this embodiment, the aggregate is a ceramic aggregate, so the atomizer core can also be referred to as a ceramic atomizer core, and the atomizer core substrate can also be referred to as a ceramic atomizer core substrate. Ceramic aggregates include but are not limited to at least one of quartz and diatomaceous earth. This embodiment is only schematically illustrated by the ceramic aggregate including both quartz and diatomaceous earth. At this time, the mass of quartz is 15-30Wt.%, and the mass of diatomaceous earth is 15-30Wt.%.
[0033] In this embodiment, the sintering additive includes but is not limited to low-temperature glass powder.
[0034] In this embodiment, the pore-forming agent includes but is not limited to at least one of polymethyl methacrylate, starch, polyvinyl alcohol, and polystyrene.
[0035] In this embodiment, the high thermal conductivity filler includes but is not limited to at least one of diamond, silicon carbide, and aluminum oxide. Optionally, diamond has the best effect, followed by silicon carbide, and then aluminum oxide.
[0036] S200, drying the solute, and treating the dried solute with the solvent with wax to obtain a mixed slurry.
[0037] After the solutes are mixed, the solute solid powders can be placed in a drying oven for drying to remove the moisture adsorbed in the powders. Optionally, the solute solid powders can be placed in a drying oven at 100° C. and dried for 2-4 hours.
[0038] Then, the dried solute solid powder and solvent are placed in a wax mixing machine for mixing, so that the solute solid powder is evenly dispersed in the solvent to obtain a mixed slurry for subsequent molding. The solvent is also originally solid, and can be melted into a gel after heating, which is convenient for subsequent molding. Optionally, the wax can be mixed at 80℃-140℃ for 4-6h.
[0039] Optionally, the solvent includes, but is not limited to, at least two of paraffin, beeswax, stearic acid, polyethylene, and ethylene-vinyl acetate copolymer.
[0040] In this embodiment, the solvent includes at least two of paraffin wax 5-10 wt.%, beeswax 0-5 wt.%, stearic acid 0-5 wt.%, polyethylene 0-5 wt.%, and ethylene-vinyl acetate copolymer 0-5 wt.% by mass percentage. In other words, paraffin wax is a necessary component in the solvent, and at least one of beeswax, stearic acid, polyethylene, and ethylene-vinyl acetate copolymer can be selected to match the paraffin wax.
[0041] S300, providing a heating sheet, processing the mixed slurry and the heating sheet through a hot injection molding process, so that the mixed slurry forms an atomizer core base embryo, and fixing the heating sheet to the atomizer core base embryo, to obtain an atomizer core embryo.
[0042] In related processes, a post-film printing process is usually used to form on the surface of the atomizer core substrate after the atomizer core substrate is prepared. However, in this embodiment, a heating sheet is first prepared, that is, a heating sheet with a metal etching mesh is designed in advance, and then the mixed slurry and the heating sheet are processed by a hot pressing injection molding process, and the heating sheet is directly fixed on the atomizer core substrate embryo formed by the mixed slurry. At this time, the heating sheet and the atomizer core substrate embryo can be called an atomizer core embryo.
[0043] Optionally, during the hot pressing process, the mixed slurry can be added to a hot pressing grouting machine, the designed heating sheet of the metal etching mesh is placed in the forming mold, and the hot pressing grouting machine is started to obtain a porous ceramic body with an etched metal mesh, wherein the grouting temperature is 55°C-85°C, and the forming pressure is 0.3Mpa-0.8Mpa.
[0044] S400, the atomizer core embryo is processed through a degreasing process and a sintering process to obtain an atomizer core.
[0045] The atomizer core embryo can then be degreased and sintered. During the sintering process, the pore-forming agent and solvent in the atomizer core embryo will decompose and volatilize in various forms, so that the space originally occupied by the pore-forming agent and solvent will form holes, thereby forming an atomizer core with a porous structure inside, which is convenient for the aerosol matrix to flow inside the atomizer core, and finally prepare the atomizer core. In the related technology, since the thermal conductivity of the atomizer core matrix embryo is low, a higher sintering temperature is required in order to make the inside of the atomizer core matrix embryo reach the preset temperature. For example, the existing sintering temperature is as high as 1000°C.
[0046] However, since the present embodiment adds a high thermal conductivity filler, the high thermal conductivity filler not only has a high thermal conductivity coefficient, but is also evenly dispersed in the atomizer core matrix embryo, so that the heat outside the atomizer core matrix embryo can be quickly transferred to the inside of the atomizer core matrix embryo, so a high sintering temperature is not required, and the sintering temperature can be effectively reduced. Therefore, the preparation method of the present embodiment can also be referred to as a preparation method of a high thermal conductivity, low temperature porous ceramic atomizer core. Secondly, since the atomizer core made by adding a high thermal conductivity filler can also better transfer the heat generated by the heating plate during operation, the atomizer core thermal field temperature is uniform, the taste is not easy to cause burning and the attenuation is small, which improves the consistency of the taste.
[0047] Optionally, ultrasonic cleaning may be performed after sintering.
[0048] In summary, the preparation method provided in this embodiment is simple in process, and the atomizer core can be made mainly through weighing and mixing, drying, waxing, hot pressing molding, degreasing sintering, and ultrasonic cleaning. In addition, the porous ceramic atomizer core has a significantly lower sintering temperature due to the addition of high thermal conductivity fillers, and the obtained ceramic atomizer core has a uniform thermal field temperature, good taste consistency and small attenuation, which is suitable for high-power and large-capacity application conditions.
[0049] In this embodiment, in the sintering process, the highest sintering temperature is less than 590°C. By adopting the above embodiment of the present application for preparation, the sintering temperature can be effectively reduced, so that the highest sintering temperature in the sintering process is less than 590°C, which can effectively reduce the sintering temperature compared to the high temperature of more than 600°C and 1000°C in the related art. Optionally, the highest sintering temperature is 530°C-580°C.
[0050] In this embodiment, the mass of the solvent is 15%-40% of the sum of the mass of the solute and the mass of the solvent. When the aggregate, high thermal conductive filler, sintering additive, and pore-forming agent are weighed and mixed in a certain proportion, the solute has a mass W1. Similarly, after the solvent is weighed in a certain proportion, the solvent has a mass W2. When the wax is mixed with the solute and the solvent, the mass of the solvent can be 15%-40% of the sum of the mass of the solute and the mass of the solvent, that is, W2 / (W1+W2) is 15%-40%. When it is less than 15% or greater than 40%, the atomizer core embryo will be difficult to form during hot pressing, which will reduce the various performances of the atomizer core.
[0051] Optionally, the mass of the solvent may be 15%, 20%, 25%, 30%, 35%, or 40% of the sum of the mass of the solute and the mass of the solvent.
[0052] In this embodiment, the solvent is first melted when waxing, and then the solute is added to the melted solvent. Solvents such as paraffin wax are also solid substances at room temperature. When waxing, the solvent can be first placed in a waxing machine for heating to melt the solvent, and then the solute is added to the melted solvent, thereby improving the mixing effect of the solute and the solvent.
[0053] Optionally, the solute may be added to the melted solvent in multiple times, thereby further improving the mixing effect of the solute and the solvent.
[0054] In this embodiment, when the atomizer core embryo is processed through a degreasing process and a sintering process, the degreasing process and the sintering process are an integrated process. In the related art, in order to prevent the atomizer core matrix from deforming, the degreasing process and the sintering process are carried out separately, and the degreasing process is carried out first and then the sintering process. Since the present application adds a high thermal conductivity filler, the heat conduction is accelerated and the sintering temperature is reduced, so the degreasing process and the sintering process can be integrated into one process, that is, an integrated degreasing and sintering process, which simplifies the preparation steps and reduces the preparation cost.
[0055] Specifically, the atomizer core embryo is placed in a degreasing furnace for degreasing and sintering to obtain a porous ceramic atomizer core. The degreasing and sintering process directly places the atomizer core embryo obtained by the hot pressing process neatly on the degreasing plate, and the atomizer core embryos do not touch each other. After the placement is completed, it is directly placed in the degreasing furnace and degreasing and sintering is performed according to the set degreasing and sintering curve. The degreasing and sintering is carried out in the air. The degreasing and sintering curve is: degreasing and sintering are heated from room temperature to 150°C at a heating rate of 0.25°C / min for 10 hours, and then heated to 300°C at a rate of 0.5°C / min for 5 hours, and then heated to 450°C at a rate of 1°C / min for 2.5 hours, and kept warm for 2 hours, and then heated to the sintering temperature at a heating rate of 1°C / min for about 3 hours, and kept warm at the sintering temperature for 2 hours, and then cooled to room temperature with the furnace, and finally a high thermal conductivity and low temperature porous ceramic atomizer core can be obtained.
[0056] Please refer to Figure 2 , Figure 2 Schematic diagram of the three-dimensional structure of an atomizer core in one embodiment of the present application. This embodiment also provides an atomizer core 1, which is prepared by the preparation method of the atomizer core 1 provided in the above embodiment of the present application.
[0057] The atomizer core 1 provided in this embodiment is prepared by adopting the preparation method of the atomizer core 1 provided in the above embodiment of the present application. The atomizer core 1 has a uniform thermal field temperature, is not easy to cause burning in taste, and has small attenuation, thereby improving the consistency of taste and being suitable for high-power and large-capacity application conditions.
[0058] In this embodiment, the average atomization temperature of the atomizer core 1 is less than 245°C. The addition of high thermal conductivity fillers allows the heat of the heating sheet 20 to be quickly transferred to all parts of the atomizer core substrate 10 when it is working, avoiding the problem of excessively high local temperature of the atomizer core 1, and reducing the average atomization temperature of the atomizer core 1. Optionally, the average atomization temperature of the atomizer core 1 is 215°C-230°C.
[0059] In addition, the present application also provides three specific embodiments of the preparation method of the atomizer core, and a comparative example of an atomizer core prepared without using a high thermal conductive filler, the specific contents are as follows:
[0060] Embodiment 1:
[0061] The preparation method of the high thermal conductivity and low temperature porous ceramic atomizer core of this embodiment is as follows:
[0062] (1) According to the mass percentage, 34% of quartz, 15% of diatomaceous earth, 3% of diamond powder, 18% of low-temperature glass powder and 30% of 50 μm polystyrene pore-forming agent were weighed and put into a three-dimensional mixer for mixing for 2 hours. After mixing evenly, a premix was formed. The mixed powder was placed in a drying oven at 100°C and dried for 4 hours.
[0063] (2) According to the mass percentage, 74% of the dried premix, 18% of paraffin, 4% of beeswax and 4% of stearic acid were put into a wax mixer and waxed at 80° C. for 4 hours to obtain a mixed slurry.
[0064] (3) Pour the mixed slurry with wax into a hot press grouting machine, place the designed metal etched mesh in the molding mold, start the hot press grouting machine, and obtain a porous ceramic atomized core embryo with an etched metal mesh. The process parameters are: grouting temperature 70°C, molding pressure 0.4Mpa.
[0065] (4) The porous ceramic atomizer core blanks are neatly arranged in a sagger without contact between the atomizer core blanks. The arranged degreasing trays are then directly placed in a degreasing sintering furnace. The degreasing sintering is carried out at a heating rate of 0.25°C / min from room temperature to 150°C, kept warm for 1 hour, then heated to 300°C at a rate of 0.5°C / min, and then heated to 450°C at a rate of 1°C / min, kept warm for 2 hours, then heated to 530°C at a heating rate of 1°C / min, kept warm at 530°C for 2 hours, and then cooled to room temperature with the furnace to obtain a high thermal conductivity, low-temperature porous ceramic atomizer core.
[0066] (5) The performance parameters of the high thermal conductivity and low temperature porous ceramic atomizer core are as follows, where the average atomization temperature uses a test e-liquid with PG:VG=5:5 and maintains a constant power of 9W.
[0067]
[0068] Embodiment 2:
[0069] The preparation method of the high thermal conductivity and low temperature porous ceramic atomizer core of this embodiment is as follows:
[0070] (1) According to the mass percentage, 34% of quartz, 15% of diatomaceous earth, 3% of silicon carbide, 18% of low-temperature glass powder and 30% of 50 μm polystyrene pore-forming agent were weighed and put into a three-dimensional mixer for mixing for 2 hours. After mixing evenly, a premix was formed. The mixed powder was placed in a drying oven at 100°C and dried for 4 hours.
[0071] (2) According to the mass percentage, 74% of the dried premix, 18% of paraffin, 4% of beeswax and 4% of stearic acid were put into a wax mixer and waxed at 80° C. for 4 hours to obtain a mixed slurry.
[0072] (3) Pour the mixed slurry with wax into a hot press grouting machine, place the designed metal etched mesh in the molding mold, start the hot press grouting machine, and obtain a porous ceramic atomizer core blank with an etched metal mesh. The process parameters are: grouting temperature 70°C, molding pressure 0.4Mpa.
[0073] (4) The porous ceramic atomizer core blanks are neatly arranged in a sagger without contact between the atomizer core blanks. Then the arranged degreasing tray is directly placed in a degreasing sintering furnace. The degreasing sintering is carried out at a heating rate of 0.25℃ / min from room temperature to 150℃, kept warm for 1h, then heated to 300℃ at a rate of 0.5℃ / min, and then heated to 450℃ at a rate of 1℃ / min, kept warm for 2h, then heated to 560℃ at a heating rate of 1℃ / min, kept warm at 560℃ for 2h, and then cooled to room temperature with the furnace to obtain a high thermal conductivity and low temperature porous ceramic atomizer core.
[0074] (5) The performance parameters of the high thermal conductivity and low temperature porous ceramic atomizer core are as follows, where the average atomization temperature uses a test e-liquid with PG:VG=5:5 and maintains a constant power of 9W.
[0075]
[0076] Embodiment 3:
[0077] The preparation method of the high thermal conductivity and low temperature porous ceramic atomizer core of this embodiment is as follows:
[0078] (1) According to the mass percentage, 34% of quartz, 15% of diatomaceous earth, 3% of alumina, 18% of low-temperature glass powder and 30% of 50 μm polystyrene pore-forming agent were weighed and put into a three-dimensional mixer and mixed for 2 h. After mixing evenly, a premix was formed. The mixed powder was placed in a drying oven at 100°C and dried for 4 h.
[0079] (2) According to the mass percentage, 74% of the dried premix, 18% of paraffin, 4% of beeswax and 4% of stearic acid were put into a wax mixer and waxed at 80° C. for 4 hours to obtain a mixed slurry.
[0080] (3) Pour the mixed slurry with wax into a hot press grouting machine, place the designed metal etched mesh in the molding mold, start the hot press grouting machine, and obtain a porous ceramic atomizer core blank with an etched metal mesh. The process parameters are: grouting temperature 70°C, molding pressure 0.4Mpa.
[0081] (4) The porous ceramic atomizer core blanks are neatly arranged in a sagger without contact between the atomizer core blanks. The arranged degreasing trays are then directly placed in a degreasing sintering furnace. The degreasing sintering is carried out at a heating rate of 0.25°C / min from room temperature to 150°C, kept warm for 1 hour, then heated to 300°C at a rate of 0.5°C / min, and then heated to 450°C at a rate of 1°C / min, kept warm for 2 hours, then heated to 580°C at a heating rate of 1°C / min, kept warm at 580°C for 2 hours, and then cooled to room temperature with the furnace to obtain a high thermal conductivity and low temperature porous ceramic atomizer core.
[0082] (5) The performance parameters of the high thermal conductivity and low temperature porous ceramic atomizer core are as follows, where the average atomization temperature uses a test e-liquid with PG:VG=5:5 and maintains a constant power of 9W.
[0083]
[0084] Comparative Example:
[0085] The preparation method of the high thermal conductivity and low temperature porous ceramic atomizer core of this embodiment is as follows:
[0086] (1) According to the mass percentage, 37% of quartz, 15% of diatomaceous earth, 18% of low-temperature glass powder and 30% of 50 μm polystyrene pore-forming agent were weighed and put into a three-dimensional mixer and mixed for 2 hours. After mixing evenly, a premix was formed. The mixed powder was placed in a drying oven at 100°C and dried for 4 hours.
[0087] (2) According to the mass percentage, 74% of the dried premix, 18% of paraffin, 4% of beeswax and 4% of stearic acid were put into a wax mixer and waxed at 80° C. for 4 hours to obtain a mixed slurry.
[0088] (3) Pour the mixed slurry with wax into a hot press grouting machine, place the designed metal etched mesh in the molding mold, start the hot press grouting machine, and obtain a porous ceramic atomizer core blank with an etched metal mesh. The process parameters are: grouting temperature 70°C, molding pressure 0.4Mpa.
[0089] (4) The porous ceramic atomizer core blanks are neatly arranged in a sagger without contact between the atomizer core blanks. The arranged degreasing trays are then directly placed in a degreasing sintering furnace. The degreasing sintering is carried out at a heating rate of 0.25°C / min from room temperature to 150°C, kept warm for 1 hour, then heated to 300°C at a rate of 0.5°C / min, and then heated to 450°C at a rate of 1°C / min, kept warm for 2 hours, then heated to 580°C at a heating rate of 1°C / min, kept warm at 580°C for 2 hours, and then cooled to room temperature with the furnace to obtain a high thermal conductivity and low temperature porous ceramic atomizer core.
[0090] (5) The performance parameters of the high thermal conductivity and low temperature porous ceramic atomizer core are as follows, where the average atomization temperature uses a test e-liquid with PG:VG=5:5 and maintains a constant power of 9W.
[0091]
[0092] Through Examples 1-3 and the comparative examples, it can be seen that the preparation method provided by the present application can effectively reduce the temperature of the embryo body desintering and the average temperature during atomization, so that the taste consistency is good and the attenuation is small. At the same time, a high porosity and pore size can be maintained. The atomizer core and the preparation method provided by the present application have a uniform thermal field temperature of the atomizer core, the taste is not easy to cause burning and the attenuation is small, which improves the consistency of the taste and is suitable for high-power and large-capacity application conditions.
[0093] In the description of the present application, it is necessary to understand that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like to indicate orientations or positional relationships are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0094] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions.
[0095] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be connected, detachably connected, or integrated. It can be mechanically connected or electrically connected. It can be directly connected or indirectly connected through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances.
[0096] The above describes the contents provided by the implementation methods of the present application in detail, and describes and illustrates the principles and implementation methods of the present application. These descriptions are only used to help understand the method and its core ideas of the present application. However, the contents of this specification should not be construed as limiting the present application, and those skilled in the art may make various changes and modifications to the present application without departing from the spirit and scope of the present application. These modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents.
Claims
1. A method for preparing an atomizer core, characterized in that: The preparation method comprises: Providing a solute and a solvent, wherein the solute includes an aggregate, a high thermal conductive filler, a sintering additive, and a pore-forming agent; The solute is dried, and the dried solute and the solvent are treated with wax to obtain a mixed slurry; Providing a heating sheet, processing the mixed slurry and the heating sheet through a hot injection molding process, so that the mixed slurry forms an atomizer core matrix embryo, and fixing the heating sheet to the atomizer core matrix embryo, to obtain an atomizer core embryo; The atomizer core embryo is processed through a degreasing process and a sintering process to obtain an atomizer core.
2. The preparation method according to claim 1, characterized in that In the sintering process, the maximum sintering temperature is less than 590°C.
3. The preparation method according to claim 1, characterized in that: The high thermal conductivity filler includes at least one of diamond, silicon carbide, and aluminum oxide.
4. The preparation method according to claim 1, characterized in that: The mass of the solvent is 15%-40% of the sum of the mass of the solute and the mass of the solvent.
5. The preparation method according to claim 1, characterized in that: In terms of mass percentage, the solute includes 30-60 wt.% of aggregate, 5-10 wt.% of high thermal conductivity filler, 10-30 wt.% of sintering additive, and 20-50 wt.% of pore former.
6. The preparation method according to claim 1, characterized in that: In terms of mass percentage, the solvent includes at least two of paraffin 5-10 wt.%, beeswax 0-5 wt.%, stearic acid 0-5 wt.%, polyethylene 0-5 wt.%, and ethylene-vinyl acetate copolymer 0-5 wt.%.
7. The preparation method according to claim 1, characterized in that: When the wax treatment is performed, the solvent is first melted, and then the solute is added to the melted solvent.
8. The preparation method according to claim 1, characterized in that: When the atomization core embryo is processed through a degreasing process and a sintering process, the degreasing process and the sintering process are an integrated process.
9. An atomizer core, characterized in that: The atomizer core is prepared by the atomizer core preparation method according to any one of claims 1 to 8.
10. The atomizer core according to claim 9, characterized in that: The average atomization temperature of the atomization core is less than 245°C.