Antibacterial wear-resistant dental repair composite material
By modifying silica and sea urchin-type hydroxyapatite, antibacterial and wear-resistant dental repair composite materials are prepared, which solves the problems that dental repair composite resins are easy to shrink, crack, and breed bacteria, and achieve high-quality Wear resistance, antibacterial and remineralizing properties extend service life.
Patent Information
- Application Number
- CN202410921613.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-29
AI Technical Summary
Dental restoration composite resin is easy to shrink, crack, and breed bacteria during long-term use, leading to degradation of the restoration and secondary caries, making it difficult to meet the requirements for wear resistance and antibacterial properties.
By modifying silica and sea urchin-type hydroxyapatite, modified filler I and modified filler II with antibacterial functions are prepared, and used in combination, combined with matrix resin and initiator to prepare antibacterial and wear-resistant materials. Type dental restoration composite materials to improve mechanical properties and remineralization properties.
The low volume shrinkage, high wear resistance, high mechanical properties and antibacterial properties of the composite material are achieved, extending the service life, reducing the risk of secondary caries, and providing long-lasting antibacterial activity.
Smart Images

Figure BDA0004936884640000141 
Figure BDA0004936884640000151
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of medical materials, and in particular relates to an antibacterial and wear-resistant dental repair composite material and a preparation method thereof. Background Art
[0002] Dental restoration composite resins need to meet the requirements of withstanding large chewing forces without fracture and damage in a long-term oral service environment. Therefore, composite resins need to have excellent mechanical properties. Light-cured composite resins have good aesthetic properties, operating properties, mechanical properties and wear resistance. They are widely used in the field of oral restoration and have become the first choice for filling and treating posterior tooth caries. However, survey results show that the service life of composite resins is only about 10 years, and the main reasons for the failure of direct restorations are restoration fracture and secondary caries. Under the long-term effects of chewing stress and saliva, insufficient wear resistance and insufficient strength will cause the restoration to degrade, resulting in a decrease in mechanical properties. After the resin is photocured, it shrinks in volume, which will generate shrinkage stress at the bonding interface between the hard tissue of the tooth and the restoration; the oral environment changes alternately between hot and cold, the numerous bacterial flora and the resulting corrosion, as well as the different thermal expansion coefficients of the composite resin and the tooth tissue, repeated expansion and contraction and corrosion will aggravate the microcracks between the restoration and the tooth tissue, leading to restoration shedding and secondary caries.
[0003] In the past few decades, inorganic filler components in composite resins have been the focus of research and have made great progress. It has become a consensus that the addition of inorganic fillers can improve the mechanical properties of composite resins, reduce polymerization shrinkage, and enhance wear resistance. For example, inorganic fillers such as silica have excellent stability and are widely used in dental restoration materials. From the perspective of material bionics, the main component of human teeth (enamel, dentin) is hydroxyapatite (50%-95%), and the use of hydroxyapatite can promote the remineralization of dental materials. In addition, sea urchin-type hydroxyapatite is a new type of inorganic material with a spherical appearance composed of a radial whisker structure. It has a large surface area and a complex morphology. It has both the easy dispersion characteristics of spherical materials in the matrix and the various strengthening and toughening characteristics of whisker materials.
[0004] In view of the above factors, the focus of dental restoration composite resins is on low volume shrinkage, high mechanical properties, antibacterial properties, etc. Therefore, the preparation of antibacterial and wear-resistant dental restoration composite materials has received more and more attention and expectations. Summary of the invention
[0005] The purpose of the present invention is to provide an antibacterial and wear-resistant dental repair composite material and a preparation method thereof in view of the problems in the prior art that dental repair materials are prone to shrinkage, cracking, and bacterial growth. By modifying silica with a fluorine-containing ammonium salt structure, a modified filler I with antibacterial function is obtained; at the same time, the sea urchin-type hydroxyapatite is modified with a silane coupling agent to obtain a modified filler II; by compounding the modified filler I with the modified filler II, a composite material prepared by adding a matrix resin and an initiator will effectively solve the above problems, and at the same time has excellent mechanical properties and promotes the remineralization of dental repair materials. In order to achieve the above purpose, the technical solution adopted by the present invention to solve its technical problems is:
[0006] One of the purposes of the present invention is to provide a method for preparing a modified filler I, comprising the following steps:
[0007] S11, coupling reaction of silicon dioxide and aminosilane coupling agent to obtain intermediate product I;
[0008] S12, subjecting methacryloyloxyammonium bromide salt to an ion exchange reaction with fluoride to obtain an intermediate product II; and
[0009] S13, subjecting the intermediate product I and the intermediate product II to Michael addition reaction to obtain the target product, i.e., modified filler I.
[0010] Further, the silica particle size is 10-40 μm; and
[0011] The usage ratio of the silicon dioxide to the aminosilane coupling agent is 10g:0.5-1.5g.
[0012] Further,
[0013] The methacryloyloxy ammonium bromide salt and the fluoride are added in a molar ratio of bromide ion to fluoride ion of 1:1.
[0014] Further,
[0015] The intermediate product I and the intermediate product II are added in a molar ratio of amino group to methacryloyloxy group of 1:1.
[0016] Another object of the present invention is to provide a modified filler I prepared by a preparation method.
[0017] Another object of the present invention is to provide a method for preparing a modified filler II, comprising the following steps:
[0018] The sea urchin type hydroxyapatite is coupled with a silane coupling agent to obtain a target product, namely, modified filler II.
[0019] Furthermore, the sea urchin type hydroxyapatite has a particle size of 2-3 μm; and
[0020] The usage ratio of sea urchin type hydroxyapatite to silane coupling agent is 10g:0.5-2.0g.
[0021] Another object of the present invention is to provide a modified filler II prepared by a preparation method.
[0022] Another object of the present invention is to provide an antibacterial and wear-resistant dental repair composite material, comprising the following raw materials in percentage by weight:
[0023] Modified filler I 60-70 parts;
[0024] Modified filler II 5.0-15.0 parts;
[0025] Bisphenol A-glycidyl methacrylate 10-20 parts;
[0026] Carbamate diglycidyl methacrylate 2.0-4.0 parts;
[0027] 1.0-3.0 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0028] Triethylene glycol dimethacrylate balance;
[0029] Photoinitiator 1.0 part
[0030] Furthermore, the modified filler I is 10.0-20.0% of the mass of the modified filler II.
[0031] Furthermore, the mass percentage of the filler is 70-80%.
[0032] Another object of the present invention is to provide a method for preparing an antibacterial and wear-resistant dental repair composite material, comprising the following steps:
[0033] Protect from light, mix the modified filler I, modified filler II, bisphenol A-glycidyl methacrylate, carbamate diglycidyl methacrylate, di[2-(methacryloyloxy)ethyl]phosphate, and triethylene glycol dimethacrylate in proportion, add a photoinitiator, continue stirring, mix well, and then discharge the material to obtain a dental repair composite material with antibacterial function.
[0034] The present invention has the following beneficial effects:
[0035] (1) The present invention provides an antibacterial and wear-resistant dental repair composite material, which uses a modified filler I containing quaternary ammonium salt, fluoride ion, and long-chain structure modified silica. First, silica has excellent wear resistance, compression strength and provides a lower volume shrinkage rate; second, after the long-chain organic structure chemically modifies silica, it can be effectively dispersed to improve the mechanical properties; at the same time, it can be fully wetted and coated with the matrix resin to avoid the existence of holes; third, the quaternary ammonium salt has high efficiency and broad-spectrum antibacterial properties, and is anchored with silica and will not be released from the material; at the same time, as the material is worn during use, the newly generated contact surface still has antibacterial properties and has long-lasting antibacterial activity; in addition, due to the good wear resistance and high weight ratio of silica, it has a larger contact surface with the outside world with the help of silica as a carrier, and the antibacterial effect is better; fourth, the F element is important to the growth and development of the human body, especially in bones and teeth, and the sudden release effect of F ions is reduced through the charge adsorption of quaternary ammonium salts; in addition, the presence of F ions plays an important role in the tissue hardening of sea urchin-type hydroxyapatite.
[0036] (2) The present invention provides an antibacterial and wear-resistant dental repair composite material, which uses a modified filler II that is silane-modified sea urchin-type hydroxyapatite. First, hydroxyapatite is an inorganic material with excellent biocompatibility and is consistent with the main component of tooth enamel; second, after being compounded with the modified filler I, the small particle size structure of hydroxyapatite and the large particle size structure of the modified filler I form an effective filling, further improving the compression strength and wear resistance; third, the sea urchin-type hydroxyapatite structure forms a pinning with the matrix resin and the modified filler I wrapped by the organic chain, while improving the compression strength and wear resistance, it forms an interlocking structure with the polymer, releases stress, and improves the bonding force; fourth, the F ions in the modified filler I combine with hydroxyapatite to form fluorohydroxyapatite, which has better resistance to bone marrow absorption and better stability.
[0037] (3) The present invention provides an antibacterial and wear-resistant dental repair composite material, the formula raw materials contain di[2-(methacryloyloxy)ethyl]phosphate, which has the function of replenishing phosphorus ions and promoting remineralization, and is helpful for the repair and reinforcement of teeth. DETAILED DESCRIPTION
[0038] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0039] The purpose of the present invention is to develop an antibacterial and wear-resistant dental repair composite material with low polymerization volume shrinkage, high wear resistance, high mechanical properties, antibacterial and remineralization functions and safe and non-toxic. The idea of realization is that inorganic fillers such as silica have high wear resistance and filling a certain amount of inorganic fillers can reduce the polymerization volume shrinkage to a certain extent while improving the mechanical properties; in addition, small-particle sea urchin-type hydroxyapatite is used for compounding, and the volume shrinkage is further reduced while improving the remineralization performance of the composite material to reduce the probability of secondary caries; thirdly, quaternary ammonium salts with safe, non-toxic and highly effective antibacterial properties are used for structural design and addition to achieve the above-mentioned required effects. The theoretical basis for realization is: first, large-particle silica is used as a carrier, modified by silane coupling agent and Michael addition with methacryloyloxy ammonium fluoride salt to prepare modified filler I; small-particle sea urchin-type hydroxyapatite is modified by silane coupling agent to obtain modified filler II; second, through formula design, reactive phosphate monomers are added to supplement phosphate remineralization; further improve the remineralization performance. The antibacterial and wear-resistant dental repair composite material prepared thus has low volume shrinkage, high wear resistance, high mechanical performance, antibacterial and remineralization properties. The embodiments of the present invention are as follows:
[0040] The embodiment of the present invention provides a method for preparing a modified filler I, comprising the following steps:
[0041] S11, adding silicon dioxide and aminosilane coupling agent to an alcohol solvent, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 50-80° C. for 2-10 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain an intermediate product I;
[0042] The usage ratio of the silicon dioxide, the aminosilane coupling agent and the alcohol solvent is 10g:0.5-1.5g:80mL.
[0043] The silicon dioxide described in the following examples of the present invention has a particle size of 10-40 μm, a purity of 99.8%, a model number of YJ-958, and is purchased from Shanghai Yuanjiang Chemical Co., Ltd.
[0044] The aminosilane coupling agent may be KH901, KH902, KH540, KH550, KH602, or KH792, and preferably KH550.
[0045] The alcohol solvent may be anhydrous methanol, anhydrous ethanol, anhydrous isopropanol, etc., and anhydrous ethanol is preferred.
[0046] S12, adding methacryloyloxy ammonium bromide salt to deionized water A to dissolve, adding fluoride to deionized water B and placing in a constant pressure dropping funnel, stirring, slowly dropping at room temperature, continuing to stir for 1-2 hours after the addition is completed, centrifuging at 3500 rpm for 30 minutes, taking the supernatant, and vacuum drying at room temperature for 24 hours to obtain intermediate product II;
[0047] The methacryloyloxy ammonium bromide salt and the fluoride are added in a molar ratio of bromide ion to fluoride ion of 1:1;
[0048] The usage ratio of the methacryloyloxy ammonium bromide salt, deionized water A, and deionized water B is 10 g: 100 mL: 150 mL.
[0049] The methacryloyloxy ammonium bromide salt may be methacryloyloxy dodecyl pyridinium bromide, methacryloyloxy ethyl hexadecyl dimethyl ammonium bromide, or the like; and preferably methacryloyloxy dodecyl pyridinium bromide.
[0050] The fluoride is a soluble or dispersible substance, and may be silver fluoride or the like.
[0051] S13, adding intermediate product I, intermediate product II and triethylamine to N,N-dimethylformamide, stirring at 30-50°C for 2-6 hours, and distilling under reduced pressure. The concentrate is washed with deionized water C, filtered, and the insoluble matter is taken and dried under vacuum at 40°C for 8 hours to obtain the target product, i.e., modified filler I.
[0052] The intermediate product I and the intermediate product II are added in a molar ratio of amino group to methacryloyloxy group of 1:1;
[0053] The usage ratio of the intermediate product I, N,N-dimethylformamide, and deionized water C is 10 g: 300 mL: 400 mL;
[0054] The amount of triethylamine used is 1wt% of the total mass of the reactants.
[0055] The embodiment of the present invention provides a method for preparing a modified filler II, comprising the following steps:
[0056] Add sea urchin type hydroxyapatite and silane coupling agent to alcohol solvent, ultrasonically oscillate for 0.5h, stand at room temperature for 2h, react at 50-70℃ for 2-10h, filter, take insoluble matter, dry at 60℃ for 12h to obtain the target product, i.e. modified filler II.
[0057] The usage ratio of the sea urchin type hydroxyapatite to the silane coupling agent and the alcohol solvent is 10g:0.5-2.0g:100mL.
[0058] The particle size of the sea urchin-like hydroxyapatite is 2-3 μm; and the preparation method of the sea urchin-like hydroxyapatite described in the following embodiments of the present invention is prepared according to the literature (Fengwei Liu, etc.. Mechanical properties of dental resin / composite containing urchin-like hydroxyapatite, Dental Materials [J], 2014 (30): 1358-1368).
[0059] The silane coupling agent can be a vinyl silane coupling agent, a methacryloxy silane coupling agent, a mercapto silane coupling agent, etc.
[0060] The vinyl silane coupling agent may be KH151, KH171, KH172, etc., and preferably KH151.
[0061] The methacryloxysilane coupling agent may be KH570, KH571, KH670, GX572, etc.; and preferably KH570;
[0062] The mercaptosilane coupling agent may be KH580, KH590, etc., and KH590 is preferred.
[0063] The alcohol solvent may be anhydrous methanol, anhydrous ethanol, anhydrous isopropanol, etc., and anhydrous ethanol is preferred.
[0064] In the present invention, the modified filler I is a large-particle silica (micrometer level) modified by methacryloyloxy ammonium bromide, and the modified filler II is a small-particle sea urchin-type hydroxyapatite modified by silane. Due to the spherical structure of the sea urchin-type hydroxyapatite and the pinning effect of the whiskers: first, the large-particle modified filler I and the small-particle modified filler II are used in combination, which has the advantages of reducing the polymerization volume shrinkage rate, improving wear resistance, improving mechanical properties and interface bonding strength; second, the presence of fluoride ions in the modified filler I further strengthens the hardened tissue and absorbs phosphate in the environment for remineralization, effectively preventing the occurrence of secondary caries; third, the quaternary ammonium salt uses silica as a carrier, has high-efficiency dispersibility and large contact sites, has high-efficiency antibacterial properties, and can still maintain a high level of antibacterial properties after wear.
[0065] The embodiment of the present invention provides an antibacterial and wear-resistant dental repair composite material, comprising the following raw materials in percentage by weight:
[0066] Modified filler I 60-70 parts;
[0067] Modified filler II 5.0-15.0 parts;
[0068] Bisphenol A-glycidyl methacrylate 10-20 parts;
[0069] 2.0-4.0 parts of glycidyl dimethacrylate of carbamate;
[0070] 1.0-3.0 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0071] Triethylene glycol dimethacrylate balance;
[0072] Photoinitiator 1.0 part
[0073] The photoinitiator is a mixture of camphorquinone and ethyl 4-ethane-N,N-dimethylaminobenzoate; and the photoinitiator in the following embodiments of the present invention is a mixture of camphorquinone and ethyl 4-ethane-N,N-dimethylaminobenzoate in a mass ratio of 1:3.
[0074] The modified filler I accounts for 10.0-20.0% of the mass of the modified filler II.
[0075] The mass percentage of the filler is 70-80%.
[0076] The method for preparing an antibacterial and wear-resistant dental repair composite material described in the following embodiment of the present invention comprises the following steps:
[0077] Protect from light, mix the modified filler I, modified filler II, bisphenol A-glycidyl methacrylate, carbamate diglycidyl methacrylate, di[2-(methacryloyloxy)ethyl]phosphate, and triethylene glycol dimethacrylate in proportion, add a photoinitiator, continue stirring, mix well, and then discharge the material to obtain a dental repair composite material with antibacterial function.
[0078] In order to further understand the present invention, an antibacterial and wear-resistant dental repair composite material and a preparation method thereof provided by the present invention are described in detail below in conjunction with specific embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0079] Example 1
[0080] A method for preparing a modified filler I comprises the following steps:
[0081] S11, adding silica and silane coupling agent KH550 to anhydrous ethanol, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 70° C. for 5 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain intermediate product I;
[0082] The usage ratio of the silicon dioxide, the silane coupling agent KH550 and the anhydrous ethanol is 10g:1.0g:80mL.
[0083] Its infrared data is as follows: 3433cm-1 :-OH exists; 1560cm -1 : -NH peak exists; 1091cm -1 、794cm -1 :-Si-O-Si- exists.
[0084] S12, add methacryloyloxy dodecylpyridinium bromide to deionized water A to dissolve, add silver fluoride to deionized water B and place in a constant pressure dropping funnel, stir, slowly add dropwise at room temperature, continue stirring for 1.5 hours after the addition is completed, centrifuge at 3500 rpm for 30 minutes, take the supernatant, and vacuum dry at room temperature for 24 hours to obtain intermediate product II;
[0085] The methacryloyloxy dodecyl pyridinium bromide and silver fluoride are added in a molar ratio of bromide ion to fluoride ion of 1:1;
[0086] The usage ratio of the methyl methacryloyloxy dodecylpyridinium bromide, deionized water A, and deionized water B is 10 g: 100 mL: 150 mL.
[0087] Its H NMR spectrum data (only the chemical shifts with changes are marked) are as follows: 1 H NMR (500 MHz, D2O, δppm): Before reaction: 4.22 (2H, -N + -CH2-); 1.88 (2H, -N + -C-CH2-); after reaction: 4.10 (2H, -N + -CH2-); 1.75(2H, -N + -C-CH2-).
[0088] S13, adding intermediate product I, intermediate product II and triethylamine to N,N-dimethylformamide, stirring at 40°C for 5 hours, and distilling under reduced pressure. The concentrate is washed with deionized water C, filtered, and the insoluble matter is taken and dried under vacuum at 40°C for 8 hours to obtain the target product, i.e., modified filler I.
[0089] The intermediate product I and the intermediate product II are added in a molar ratio of amino group to methacryloyloxy group of 1:1;
[0090] The usage ratio of the intermediate product I, N,N-dimethylformamide, and deionized water C is 10 g: 300 mL: 400 mL;
[0091] The amount of triethylamine used is 1wt% of the total mass of the reactants.
[0092] Its infrared data is as follows: 3433cm -1 :-OH exists; 1560cm -1: -NH peak exists and weakens; 1091cm -1 、794cm -1 :-Si-O-Si- exists; 1735cm -1 :-C=O exists; 1608cm -1 、811cm -1 :-C=C- does not exist.
[0093] A method for preparing a modified filler II comprises the following steps:
[0094] Sea urchin type hydroxyapatite and silane coupling agent KH570 were added to anhydrous ethanol, ultrasonically oscillated for 0.5 h, allowed to stand at room temperature for 2 h, reacted at 60° C. for 5 h, filtered, the insoluble matter was taken, and dried at 60° C. for 12 h to obtain the target product, i.e., modified filler II.
[0095] The usage ratio of the sea urchin type hydroxyapatite, the silane coupling agent KH570 and the anhydrous ethanol is 10g:1.5g:100mL.
[0096] Its infrared data is as follows: 3438cm -1 :-OH exists; 1101cm -1 、798cm -1 ::-Si-O-Si- exists; 1735cm -1 :-C=O exists; 1608cm -1 、811cm -1 :-C=C- exists.
[0097] An antibacterial and wear-resistant dental repair composite material comprises the following raw materials in percentage by weight:
[0098] 65 parts of modified filler I;
[0099] Modified filler II 10.0 parts;
[0100] Bisphenol A-glycidyl methacrylate 15 parts;
[0101] 3.0 parts of carbamate diglycidyl methacrylate;
[0102] 2.0 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0103] Triethylene glycol dimethacrylate balance;
[0104] Photoinitiator 1.0 part
[0105] Example 2
[0106] A method for preparing a modified filler I comprises the following steps:
[0107] S11, adding silica and silane coupling agent KH550 to anhydrous ethanol, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 80° C. for 2 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain intermediate product I;
[0108] The usage ratio of the silicon dioxide, the silane coupling agent KH550 and the anhydrous ethanol is 10g:1.0g:80mL.
[0109] Its infrared data is as follows: 3433cm -1 :-OH exists; 1560cm -1 : -NH peak exists; 1091cm -1 、794cm -1 :-Si-O-Si- exists.
[0110] S12, adding methacryloyloxy dodecylpyridinium bromide to deionized water A to dissolve, adding silver fluoride to deionized water B and placing in a constant pressure dropping funnel, stirring, slowly dropping at room temperature, continuing to stir for 1 hour after the addition, centrifuging at 3500 rpm for 30 minutes, taking the supernatant, and vacuum drying at room temperature for 24 hours to obtain intermediate product II;
[0111] The methacryloyloxy dodecyl pyridinium bromide and silver fluoride are added in a molar ratio of bromide ion to fluoride ion of 1:1;
[0112] The usage ratio of the methyl methacryloyloxy dodecylpyridinium bromide, deionized water A, and deionized water B is 10 g: 100 mL: 150 mL.
[0113] Its H NMR spectrum data (only the chemical shifts with changes are marked) are as follows: 1 H NMR (500 MHz, D2O, δppm): Before reaction: 4.22 (2H, -N + -CH2-); 1.88 (2H, -N + -C-CH2-); after reaction: 4.10 (2H, -N + -CH2-); 1.75(2H, -N + -C-CH2-).
[0114] S13, add intermediate product I, intermediate product II and triethylamine to N,N-dimethylformamide, stir at 30°C for 6 hours, and then distill under reduced pressure. Wash the concentrate with deionized water C, filter, take the insoluble matter, and place it at 40°C for 8 hours to obtain the target product, i.e., modified filler I.
[0115] The intermediate product I and the intermediate product II are added in a molar ratio of amino group to methacryloyloxy group of 1:1;
[0116] The usage ratio of the intermediate product I, N,N-dimethylformamide, and deionized water C is 10 g: 300 mL: 400 mL;
[0117] The amount of triethylamine used is 1wt% of the total mass of the reactants.
[0118] Its infrared data is as follows: 3433cm -1 :-OH exists; 1560cm -1 : -NH peak exists and weakens; 1091cm -1 、794cm -1 :-Si-O-Si- exists; 1735cm -1 :-C=O exists; 1608cm -1 、811cm -1 :-C=C- does not exist.
[0119] A method for preparing a modified filler II comprises the following steps:
[0120] Sea urchin type hydroxyapatite and silane coupling agent KH570 were added to anhydrous ethanol, ultrasonically oscillated for 0.5 h, allowed to stand at room temperature for 2 h, reacted at 50° C. for 10 h, filtered, the insoluble matter was taken, and dried at 60° C. for 12 h to obtain the target product, i.e., modified filler II.
[0121] The usage ratio of the sea urchin type hydroxyapatite, the silane coupling agent KH570 and the anhydrous ethanol is 10g:1.5g:100mL.
[0122] Its infrared data is as follows: 3438cm -1 :-OH exists; 1101cm -1 、798cm -1 ::-Si-O-Si- exists; 1735cm -1 :-C=O exists; 1608cm -1 、811cm -1 :-C=C- exists.
[0123] An antibacterial and wear-resistant dental repair composite material comprises the following raw materials in percentage by weight:
[0124] 60 parts of modified filler I;
[0125] Modified filler II 9.0 parts;
[0126] Bisphenol A-glycidyl methacrylate 20 parts;
[0127] 4.0 parts of glycidyl dimethacrylate of carbamate;
[0128] 1.5 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0129] Triethylene glycol dimethacrylate balance;
[0130] Photoinitiator 1.0 part
[0131] Example 3
[0132] A method for preparing a modified filler I comprises the following steps:
[0133] S11, adding silica and silane coupling agent KH550 to anhydrous ethanol, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 50° C. for 10 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain intermediate product I;
[0134] The usage ratio of the silicon dioxide, the silane coupling agent KH550 and the anhydrous ethanol is 10g:1.0g:80mL.
[0135] Its infrared data is as follows: 3433cm -1 :-OH exists; 1560cm -1 : -NH peak exists; 1091cm -1 、794cm -1 :-Si-O-Si- exists.
[0136] S12, adding methacryloyloxy dodecylpyridinium bromide to deionized water A to dissolve, adding silver fluoride to deionized water B and placing in a constant pressure dropping funnel, stirring, slowly dropping at room temperature, continuing to stir for 2 hours after the addition, centrifuging at 3500 rpm for 30 minutes, taking the supernatant, and vacuum drying at room temperature for 24 hours to obtain an intermediate product II;
[0137] The methacryloyloxy dodecyl pyridinium bromide and silver fluoride are added in a molar ratio of bromide ion to fluoride ion of 1:1;
[0138] The usage ratio of the methyl methacryloyloxy dodecylpyridinium bromide, deionized water A, and deionized water B is 10 g: 100 mL: 150 mL.
[0139] Its H NMR spectrum data (only the chemical shifts with changes are marked) are as follows: 1 H NMR (500 MHz, D2O, δppm): Before reaction: 4.22 (2H, -N + -CH2-); 1.88 (2H, -N + -C-CH2-); after reaction: 4.10 (2H, -N + -CH2-); 1.75(2H, -N + -C-CH2-).
[0140] S13, adding intermediate product I, intermediate product II and triethylamine to N,N-dimethylformamide, stirring at 50°C for 2 hours, and distilling under reduced pressure. The concentrate is washed with deionized water C, filtered, and the insoluble matter is taken and dried under vacuum at 40°C for 8 hours to obtain the target product, i.e., modified filler I.
[0141] The intermediate product I and the intermediate product II are added in a molar ratio of amino group to methacryloyloxy group of 1:1;
[0142] The usage ratio of the intermediate product I, N,N-dimethylformamide, and deionized water C is 10 g: 300 mL: 400 mL;
[0143] The amount of triethylamine used is 1wt% of the total mass of the reactants.
[0144] Its infrared data is as follows: 3433cm -1 :-OH exists; 1560cm -1 : -NH peak exists and weakens; 1091cm -1 、794cm -1 :-Si-O-Si- exists; 1735cm -1 :-C=O exists; 1608cm -1 、811cm -1 :-C=C- does not exist.
[0145] A method for preparing a modified filler II comprises the following steps:
[0146] Sea urchin type hydroxyapatite and silane coupling agent KH570 were added to anhydrous ethanol, ultrasonically oscillated for 0.5 h, allowed to stand at room temperature for 2 h, reacted at 70° C. for 2 h, filtered, the insoluble matter was taken, and dried at 60° C. for 12 h to obtain the target product, i.e., modified filler II.
[0147] The usage ratio of the sea urchin type hydroxyapatite, the silane coupling agent KH570 and the anhydrous ethanol is 10g:1.5g:100mL.
[0148] Its infrared data is as follows: 3438cm -1 :-OH exists; 1101cm -1 、798cm -1 ::-Si-O-Si- exists; 1735cm -1 :-C=O exists; 1608cm -1 、811cm -1 :-C=C- exists.
[0149] An antibacterial and wear-resistant dental repair composite material comprises the following raw materials in percentage by weight:
[0150] 70 parts of modified filler I;
[0151] Modified filler II 10.5 parts;
[0152] Bisphenol A-glycidyl methacrylate 10 parts;
[0153] 2.0 parts of glycidyl carbamate dimethacrylate;
[0154] 2.5 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0155] Triethylene glycol dimethacrylate balance;
[0156] Photoinitiator 1.0 part
[0157] Example 4
[0158] The rest is the same as in Example 1, except that:
[0159] In a method for preparing a modified filler I, the usage ratio of silicon dioxide, silane coupling agent KH550 and anhydrous ethanol is 10g:0.5g:80mL.
[0160] Example 5
[0161] The rest is the same as in Example 1, except that:
[0162] In a method for preparing a modified filler I, the amount ratio of silicon dioxide, silane coupling agent KH550, and anhydrous ethanol is 10g:1.5g:80mL.
[0163] Example 6
[0164] The rest is the same as in Example 1, except that:
[0165] In a method for preparing a modified filler II, the usage ratio of the sea urchin type hydroxyapatite to the silane coupling agent KH570 and anhydrous ethanol is 10 g:0.5 g:100 mL.
[0166] Example 7
[0167] The rest is the same as in Example 1, except that:
[0168] In a method for preparing a modified filler II, the usage ratio of the sea urchin type hydroxyapatite to the silane coupling agent KH570 and anhydrous ethanol is 10 g:2.0 g:100 mL.
[0169] Example 8
[0170] The rest is the same as in Example 1, except that:
[0171] In a method for preparing a modified filler II, the silane coupling agent KH570 is replaced by KH151.
[0172] Example 9
[0173] The rest is the same as in Example 1, except that:
[0174] In a method for preparing a modified filler II, the silane coupling agent KH570 is replaced by KH590.
[0175] Example 10
[0176] The rest is the same as in Example 1, except that:
[0177] An antibacterial and wear-resistant dental repair composite material comprises the following raw materials in percentage by weight:
[0178] 65 parts of modified filler I;
[0179] Modified filler II 6.5 parts;
[0180] Bisphenol A-glycidyl methacrylate 15 parts;
[0181] 3.0 parts of carbamate diglycidyl methacrylate;
[0182] 2.0 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0183] Triethylene glycol dimethacrylate balance;
[0184] Photoinitiator 1.0 part
[0185] Embodiment 11
[0186] The rest is the same as in Example 1, except that:
[0187] An antibacterial and wear-resistant dental repair composite material comprises the following raw materials in percentage by weight:
[0188] 65 parts of modified filler I;
[0189] Modified filler II 13.0 parts;
[0190] Bisphenol A-glycidyl methacrylate 15 parts;
[0191] 3.0 parts of carbamate diglycidyl methacrylate;
[0192] 2.0 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0193] Triethylene glycol dimethacrylate balance;
[0194] Photoinitiator 1.0 part
[0195] Example 12
[0196] The rest is the same as in Example 1, except that:
[0197] An antibacterial and wear-resistant dental repair composite material comprises the following raw materials in percentage by weight:
[0198] 60 parts of modified filler I;
[0199] Modified filler II 15.0 parts;
[0200] Bisphenol A-glycidyl methacrylate 15 parts;
[0201] 3.0 parts of carbamate diglycidyl methacrylate;
[0202] 2.0 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0203] Triethylene glycol dimethacrylate balance;
[0204] Photoinitiator 1.0 part
[0205] Embodiment 13
[0206] The rest is the same as in Example 1, except that:
[0207] An antibacterial and wear-resistant dental repair composite material comprises the following raw materials in percentage by weight:
[0208] 70 parts of modified filler I;
[0209] Modified filler II 5.0 parts;
[0210] Bisphenol A-glycidyl methacrylate 15 parts;
[0211] 3.0 parts of carbamate diglycidyl methacrylate;
[0212] 2.0 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0213] Triethylene glycol dimethacrylate balance;
[0214] Photoinitiator 1.0 part
[0215] Embodiment 14
[0216] The rest is the same as in Example 1, except that:
[0217] An antibacterial and wear-resistant dental repair composite material comprises the following raw materials in percentage by weight:
[0218] 65 parts of modified filler I;
[0219] Modified filler II 10.0 parts;
[0220] Bisphenol A-glycidyl methacrylate 15 parts;
[0221] 3.0 parts of carbamate diglycidyl methacrylate;
[0222] 1.0 part of di[2-(methacryloyloxy)ethyl]phosphate;
[0223] Triethylene glycol dimethacrylate balance;
[0224] Photoinitiator 1.0 part
[0225] Embodiment 15
[0226] The rest is the same as in Example 1, except that:
[0227] An antibacterial and wear-resistant dental repair composite material comprises the following raw materials in percentage by weight:
[0228] 65 parts of modified filler I;
[0229] Modified filler II 10.0 parts;
[0230] Bisphenol A-glycidyl methacrylate 15 parts;
[0231] 3.0 parts of carbamate diglycidyl methacrylate;
[0232] 3.0 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0233] Triethylene glycol dimethacrylate balance;
[0234] Photoinitiator 1.0 part
[0235] Comparative Examples 1-9 are compared with Example 1:
[0236] Comparative Example 1
[0237] The rest is the same as in Example 1, except that:
[0238] An antibacterial and wear-resistant dental repair composite material comprises the following raw materials in percentage by weight:
[0239] 75 parts of modified filler I;
[0240] Bisphenol A-glycidyl methacrylate 15 parts;
[0241] 3.0 parts of carbamate diglycidyl methacrylate;
[0242] 2.0 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0243] Triethylene glycol dimethacrylate balance;
[0244] Photoinitiator 1.0 part
[0245] Comparative Example 2
[0246] The rest is the same as in Example 1, except that:
[0247] An antibacterial and wear-resistant dental repair composite material comprises the following raw materials in percentage by weight:
[0248] Modified filler II 75.0 parts;
[0249] Bisphenol A-glycidyl methacrylate 15 parts;
[0250] 3.0 parts of carbamate diglycidyl methacrylate;
[0251] 2.0 parts of di[2-(methacryloyloxy)ethyl]phosphate;
[0252] Triethylene glycol dimethacrylate balance;
[0253] Photoinitiator 1.0 part
[0254] Comparative Example 3
[0255] The rest is the same as in Example 1, except that:
[0256] The modified filler I is the intermediate product I in Example 1.
[0257] Comparative Example 4
[0258] The rest is the same as in Example 1, except that:
[0259] A method for preparing a modified filler I comprises the following steps:
[0260] S11, adding silica and silane coupling agent KH550 to anhydrous ethanol, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 70° C. for 5 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain intermediate product I;
[0261] The usage ratio of the silicon dioxide, the silane coupling agent KH550 and the anhydrous ethanol is 10g:1.0g:80mL.
[0262] S12, adding the intermediate product I, methacryloyloxy dodecylpyridinium bromide and triethylamine to N,N-dimethylformamide, stirring at 40°C for 5 hours, and distilling under reduced pressure. The concentrate is washed with deionized water C, filtered, and the insoluble matter is taken and dried under vacuum at 40°C for 8 hours to obtain the target product, i.e., the modified filler I.
[0263] The intermediate product I and methacryloyloxy dodecyl pyridinium bromide are added in a molar ratio of amino group to methacryloyloxy group of 1:1;
[0264] The usage ratio of the intermediate product I, N,N-dimethylformamide, and deionized water C is 10 g: 300 mL: 400 mL;
[0265] The amount of triethylamine used is 1wt% of the total mass of the reactants.
[0266] Comparative Example 5
[0267] The rest is the same as in Example 1, except that:
[0268] In a method for preparing a modified filler I, the intermediate product I and the intermediate product II described in Example 1 are physically blended in a molar ratio of amino group to methacryloyloxy group of 1:1.
[0269] Comparative Example 6
[0270] The rest is the same as in Example 1, except that:
[0271] replacing the sea urchin-type hydroxyapatite with spherical hydroxyapatite;
[0272] The spherical hydroxyapatite has an average particle size of 2-10 μm and is purchased from Beijing Dekedaojin Technology Co., Ltd.
[0273] Comparative Example 7
[0274] The rest is the same as in Example 1, except that:
[0275] The invention discloses an antibacterial and wear-resistant dental repair composite material in which di[2-(methacryloyloxy)ethyl]phosphate is not added into the raw materials.
[0276] Comparative Example 8
[0277] The rest is the same as in Example 1, except that:
[0278] In an antibacterial and wear-resistant dental repair composite material, the mass percentage of the filler is 65%.
[0279] Comparative Example 9
[0280] The rest is the same as in Example 1, except that:
[0281] In an antibacterial and wear-resistant dental repair composite material, the mass percentage of the filler is 85%.
[0282] The physical properties of the antibacterial and wear-resistant dental repair composite materials prepared in the examples of the present invention and the comparative examples were measured respectively. The results are shown in Table 1.
[0283] Table 1 Physical test performance of each embodiment
[0284]
[0285]
[0286] First, it can be observed from Examples 1-15 that the antibacterial and wear-resistant dental repair composite material of the present invention has excellent antibacterial properties, wear resistance, low polymerization shrinkage and remineralization performance.
[0287] Second, it can be observed from Example 1 and Comparative Examples 1-2 that the homemade modified filler I of the present invention has excellent wear resistance and antibacterial properties; the modified filler II has the function of promoting remineralization; and the modified filler I and the modified filler II compound also have excellent mechanical properties, etc.; it can be observed from Example 1 and Comparative Examples 3-5 that the quaternary ammonium salt structure in the homemade modified filler I of the present invention has excellent antibacterial effect; the F ion has excellent performance in promoting remineralization and the quaternary ammonium salt fluoride ion structure is bonded to silica, using silica as a carrier, and It has a greater chance of contact with the outside world, and has better antibacterial properties; it can be observed from Example 1 and Comparative Example 6 that the sea urchin-type hydroxyapatite used in the present invention has higher mechanical properties and wear resistance; it can be observed from Example 1 and Comparative Example 7 that the phosphate monomer in the present invention can promote the remineralization of hydroxyapatite and improve dental restorability; it can be observed from Example 1 and Comparative Examples 8-9 that the filler resin ratio in the present invention can greatly exert its excellent antibacterial properties, wear resistance, low polymerization shrinkage and remineralization properties within a suitable range.
[0288] In summary, the antibacterial and wear-resistant dental repair composite material of the present invention achieves the effect of low polymerization volume shrinkage by adding appropriate fillers, and at the same time has excellent antibacterial properties, wear resistance, mechanical properties and safety.
[0289] The test method is as follows:
[0290] (1) Wear resistance: A stainless steel mold was used to prepare a composite resin sample with a size of 10 mm in diameter and 6 mm in height. The sample was cured in three layers, each layer was 2 mm, and each layer was cured for 40 seconds. Three samples were prepared for each composite resin formula. The cured sample was placed in deionized water at 37°C and cured for 24 hours in the dark. Then, the wear resistance test was carried out according to the industry standard YY / T0113-2015. After the abrasive was pre-grinded 150 times, the sample was taken out, cleaned and blown dry, and weighed to obtain m1. Then the abrasive was rubbed 1500 times, the sample was taken out, cleaned and blown dry, and weighed to obtain m2. The sample density ρ was then measured. The volume wear of the composite resin can be calculated (unit: mm 3 ). The wear loss of the composite resin of each formula was taken as the average value of the test results of three specimens.
[0291] Volume wear = (m2-m1) / ρ.
[0292] (2) Polymerization volume shrinkage:
[0293] Density of resin before polymerization (D r ) determination
[0294] Pour the prepared resin into a 10ml density bottle with known weight, weigh it, pour out the resin, clean the density bottle, dry it, then pour in the resin again, weigh it, repeat the operation 5 times, and take the arithmetic mean of the five times to get the resin weight M r Use the same density bottle, fill it with distilled water and weigh it, pour out the water and dry it, then fill it with water and weigh it again, repeat the operation 5 times, and take the arithmetic mean of the five times to get the weight of water M w . Density of resin before polymerization D r Calculated by formula (3-2):
[0295] D r =(M r / M w )×D(T)
[0296] Where D(T) is the density of water at the measurement temperature;
[0297] Density of the resin after polymerization (D s ) determination
[0298] The resin was injected into a 25 mm × 2 mm × 2 mm mold. Five samples were prepared for each resin system. After 5 minutes of illumination, the samples were taken out and the density D of the samples was measured using a density tester. s ;
[0299] Calculation of polymerization shrinkage
[0300] Polymerization shrinkage (S%) is measured by D r and D s According to the following formula:
[0301] S%=(D s -D r ) / D s ×100%.
[0302] (3) Antibacterial rate: The antibacterial rate of dental composite resin was quantitatively analyzed according to the standard "ASTM E2180-07 (2012)". The sample to be tested was immersed in deionized water, placed in a 37°C constant temperature water bath oscillating box, and tested again after 15 days. The same sample after the test was cut, all the surface layers were removed, and the above operation was repeated for retesting.
[0303] (4) Mechanical properties:
[0304] Bending strength, compressive strength: The sample preparation method and test steps of the mechanical properties of composite resin refer to ISO 4049-2009. The resin specimen after curing and demoulding was polished flat with silicon carbide sandpaper and placed at room temperature for 72 hours. The bending strength and compressive strength were tested using an electronic universal material testing machine.
[0305] (5) Remineralization performance:
[0306] First, prepare 1.5 times the simulated body fluid: according to the formula described in the following literature, weigh a certain amount of NaCl, NaHCO3, Na2SO4, KCl, K2HPO4·3H2O, MgCl2·6H2O and CaCl2·2H2O and add them in batches in order to 37°C deionized water. After the previous drug is dissolved, add the next drug and adjust the pH to 7.4 with Tris-HCl. (Literature: FUZENG R, RENLONG X, XIANG G, et al. Characterization and structural analysis of zinc-substituted hydroxyapatites [Jl. Acta Biomaterialia, 2009, 5 (8): 3141-3149.)
[0307] Remineralization experiment: Add the composite resin disc to 10mL1.5SBF, shake in a constant temperature water bath at 37℃ (65rpm), replace 1.5SBF every day, take out the resin disc after 12h, wash with water and dry. Use SEM to characterize the surface morphology of the dried resin disc; weigh and record the mass change and make a comprehensive evaluation (dissolution rate> remineralization rate, that is, the mass decreases, mainly demineralization, recorded as "1"; dissolution rate=remineralization rate, that is, the mass remains unchanged, demineralization and remineralization reach a balance or no reaction occurs, recorded as "2"; dissolution rate<remineralization rate, that is, the mass increases, mainly remineralization, recorded as "3"; dissolution rate<<remineralization rate, that is, the mass increases significantly, mainly remineralization, recorded as "4").
[0308] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing a modified filler I, characterized in that: The following steps are involved: S11, coupling reaction of silicon dioxide and aminosilane coupling agent to obtain intermediate product I; S12, subjecting methacryloyloxyammonium bromide salt to an ion exchange reaction with fluoride to obtain an intermediate product II; and S13, subjecting the intermediate product I and the intermediate product II to Michael addition reaction to obtain the target product, i.e., modified filler I.
2. The preparation method according to claim 1, characterized in that: The silica particle size is 10-40 μm; and The usage ratio of the silicon dioxide to the aminosilane coupling agent is 10g:0.5-1.5g.
3. The preparation method according to claim 1, characterized in that: The methacryloyloxy ammonium bromide salt and the fluoride are added in a molar ratio of bromide ion to fluoride ion of 1:
1.
4. The preparation method according to claim 1, characterized in that: The intermediate product I and the intermediate product II are added in a molar ratio of amino group to methacryloyloxy group of 1:
1.
5. A modified filler I prepared by the preparation method as described in any one of claims 1 to 4.
6. A method for preparing a modified filler II, characterized in that: The following steps are involved: The sea urchin type hydroxyapatite is coupled with a silane coupling agent to obtain a target product, namely, modified filler II.
7. The preparation method according to claim 6, characterized in that: The particle size of the sea urchin type hydroxyapatite is 2-3 μm; and The usage ratio of sea urchin type hydroxyapatite to silane coupling agent is 10g:0.5-2.0g.
8. A modified filler II prepared by the preparation method according to claim 6 or 7.
9. An antibacterial and wear-resistant dental repair composite material, characterized in that: The following raw materials are included in percentage by weight: Modified filler I 60-70 parts; Modified filler II 5.0-15.0 parts; Bisphenol A-glycidyl methacrylate 10-20 parts; 2.0-4.0 parts of glycidyl dimethacrylate of carbamate; 1.0-3.0 parts of di[2-(methacryloyloxy)ethyl]phosphate; Triethylene glycol dimethacrylate balance; Photoinitiator 1.0 part 10. The antibacterial and wear-resistant dental repair composite material according to claim 9, characterized in that: The modified filler I accounts for 10.0-20.0% of the mass of the modified filler II.
11. The antibacterial and wear-resistant dental repair composite material according to claim 9, characterized in that: The mass percentage of the filler is 70-80%.
12. A method for preparing an antibacterial and wear-resistant dental repair composite material, characterized in that: The following steps are involved: Protect from light, mix the modified filler I, modified filler II, bisphenol A-glycidyl methacrylate, carbamate diglycidyl methacrylate, di[2-(methacryloyloxy)ethyl]phosphate, and triethylene glycol dimethacrylate in proportion, add a photoinitiator, continue stirring, mix well, and then discharge the material to obtain a dental repair composite material with antibacterial function.
Citation Information
Cited By
Dental resin-based ceramic composite material and preparation method thereof
CN120549779A