Method for pollucite flotation, plagioclase flotation and quartz purification

By using the flotation method of TM2 and NH4F under different pH conditions, combined with sodium sulfonate and tallow amine acetate, colloid garnet was successfully separated and recovered, which solved the low recovery rate of colloid garnet and the danger of traditional reagents in the existing technology. solve the problem and achieve efficient and safe mineral recovery.

CN118847352APending Publication Date: 2024-10-29TANTALUM MINING CORPORATION OF CANADA LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410507725.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-25
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

It is difficult to efficiently recover cosmium garnet with existing technology, especially in low-grade cosmium garnet, resulting in low recovery rate and high cost of cesium. Moreover, traditional reagents such as HF are toxic and volatile, making it difficult to effectively separate cosmium garnet from other minerals. .

Method used

A flotation method using TM2 and NH4F under different pH conditions is used, combined with sodium sulfonate and tallow amine acetate, to separate cosmonite from plagioclase and quartz, and to separate lithium garnet and lithium through a multi-stage flotation process. Pyroxene, mica, feldspar and other minerals to achieve efficient recovery of garnet.

Benefits of technology

It achieves efficient recovery of cosmium garnet, improves the recovery rate of cesium, reduces production costs, avoids the use of toxic volatile reagents, and provides a safe and economical mineral recovery method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847352A_ABST
    Figure CN118847352A_ABST
Patent Text Reader

Abstract

Described herein is a process for recovering two predominantly valuable lithium minerals (amblygonite and spodumene), cesium mineral (pollucite) and quartz. The method comprises a series of direct flotation processes in combination with a reverse flotation process, intended to recover these lithium and cesium concentrates.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Priority information

[0002] This application claims priority to U.S. Provisional Patent Application No. USSN 63 / 498,996, filed on April 28, 2023, entitled “Methods for the Flotation of Cesium Garnet, Plagioclase Flotation, and Quartz Purification,” the entire contents of which are incorporated herein by reference for all purposes. Technical Field

[0003] The present application provides a method for flotation of cesium garnet, flotation of plagioclase, and purification of quartz. Background Art

[0004] Cesium brine solutions are used in the oil and gas drilling process, but cesium has become a scarce resource. The Tanco mine has the richest supply of cesium in the world; however, it is becoming increasingly difficult to obtain cesium from Tanco's ore bodies. On the other hand, cesium garnet ores are often grown with lithium ores, but lithium ores have not been processed to recover the cesium garnet, and therefore, a considerable amount of cesium garnet is discharged as tailings to the West Tailing Management Area (TMA). As will be appreciated by those skilled in the art, material from the West TMA is rejected from the mill (grinding) and generally meets the size range for flotation without the need for significant grinding.

[0005] Generally speaking, chemical engineering grade cesium garnet must be above 5% Cs2O. Due to equipment limitations in our chemical plants at Tanco, lower grade cesium garnet tends to produce more chemical plant tailings, resulting in lower cesium recovery. On the other hand, higher cesium grade cesium garnet will increase cesium salt recovery and reduce production costs.

[0006] Due to changes in the global mineral market, the West TMA contains a variety of valuable minerals, so mineral recovery research has become a priority. Specifically, the main minerals that make up the West lithium tailings are pyroxenite, spodumene, mica, feldspar, plagioclase, pyroxenite and quartz. Initially, the mineral to be recovered was pyroxenite, but as lithium prices rose, lithium ores (including pyroxenite and spodumene) became the target of recovery.

[0007] Sending low-grade cesium garnet to chemical plants is not only costly, but also results in reduced cesium recovery. For example, even with 5-9% Cs2O, the recovery is only about 80%.

[0008] Methods for extracting cesium from West TMA material have been tested for quite some time without much success, and no effective methods or reagents have been found in the literature. Specifically, the only effective reagent found was HF, where the concentration of cesium was slightly above 5%, while recovering approximately 60% of the cesium. However, HF is toxic and extremely volatile. Summary of the invention

[0009] According to a first aspect of the present invention, there is provided a method for flotation of cesium garnet, comprising:

[0010] Provide a certain amount of mineral tailings, including plagioclase, cesium garnet and quartz;

[0011] subjecting the amount of mineral tailings to flotation conditions containing TM2 and NH4F at a pH of about 2, wherein the ratio of TM2 to NH4F is about 1 part TM2 to about 2.3 parts NH4F, wherein the TM2 comprises about 1 part sodium sulfonate and about 2 parts tallow amine acetate, thereby separating plagioclase from pyrope and quartz,

[0012] Recover plagioclase;

[0013] subjecting the coleus and quartz to flotation conditions in the presence of TM2 and NH4F in a ratio of about 1 part TM2 to about 2.3 parts NH4F at a pH of about 2.35 to about 2.8, thereby separating the coleus from the quartz, and

[0014] Recovering cesium garnet.

[0015] According to another aspect of the present invention, there is provided a method for recovering pyrope from mineral tailings, comprising:

[0016] a) provide a certain amount of mineral tailings, including pyroxene, spodumene, mica, feldspar, plagioclase, pyroxene and quartz;

[0017] b) subjecting the amount of mineral tailings to flotation conditions in the presence of a pyroxenite collector at a pH of about 9 to about 9.3 to separate the mineral tailings into separated pyroxenite and mineral tailings, wherein the mineral tailings include spodumene, mica, feldspar, plagioclase, pyrope and quartz;

[0018] c) recovering lithium phosphate;

[0019] d) subjecting the mineral tailings comprising spodumene, mica, feldspar, plagioclase, pyrope and quartz to flotation conditions in the presence of a spodumene collector at a pH of about 9 to about 9.3, thereby separating the mineral tailings into separated spodumene and mineral tailings, wherein the mineral tailings comprises mica, feldspar, plagioclase, pyrope and quartz;

[0020] e) recovering the floated spodumene;

[0021] f) subjecting the mineral tailings comprising mica, feldspar, plagioclase, pyrope and quartz to flotation conditions in the presence of a mica collector at a pH of about 2.26 to about 2.3, thereby separating the mineral tailings into separated mica and mineral tailings, wherein the mineral tailings comprises feldspar, plagioclase, pyrope and quartz;

[0022] g) recovering the floated mica;

[0023] h) subjecting the mineral tailings comprising feldspar, plagioclase, pyrope and quartz to flotation conditions in the presence of a feldspar collector at a pH of about 2.1 to about 2.2, thereby separating the mineral tailings into separated feldspar and mineral tailings, wherein the mineral tailings comprises plagioclase, pyrope and quartz;

[0024] i) recovering the flotated feldspar;

[0025] j) subjecting the amount of mineral tailings containing plagioclase, pyrope and quartz to flotation conditions containing TM2 and NH4F at a pH of about 2, wherein the ratio of TM2 to NH4F is about 1 part TM2 to about 2.3 parts NH4F, wherein the TM2 contains about 1 part sodium sulfonate and about 2 parts tallow amine acetate, thereby separating the mineral tailings into separated plagioclase and mineral tailings containing pyrope and quartz;

[0026] k) recovering the floated plagioclase;

[0027] l) subjecting the amount of mineral tailings containing pyrope and quartz to flotation conditions containing TM2 and NH4F at a pH of about 2.35 to about 2.8, wherein the ratio of TM2 to NH4F is about 1 part TM2 to about 2.3 parts NH4F, thereby separating the mineral tailings into separated pyrope and quartz; and

[0028] m) recovering the flotated cerium garnet. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is a bar graph showing the mineral abundances at West TMA. The minerals to be recovered are spodumene, pyroxenite, pyroxenite and quartz. The QEMScan work shows that quartz is the most abundant mineral, followed by pyroxenite and plagioclase.

[0030] Figure 2 is a bar graph of data from 197 drill hole samples showing the average cesium grade at West TMA to be 0.53% Cs2O. As discussed herein, Cs2O must be concentrated to feed chemical plants.

[0031] Figure 3 This is the process flow chart of West TMA multi-product reverse flotation. DETAILED DESCRIPTION

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. Although any methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention, preferred methods and materials are now described. All publications mentioned herein are incorporated herein by reference.

[0033] Described herein is a method for recovering two major valuable lithium minerals (hexadecene and spodumene), a cesium mineral (dessinite) and quartz. The method comprises a series of direct flotation processes combined with a reverse flotation process, aimed at recovering these lithium and cesium concentrates, which are described below.

[0034] Based on lithium concentrate production practices and West TMA’s 500+ test, a direct flotation method combined with reverse flotation was designed to recover lithium and cesium concentrates as described below.

[0035] According to one aspect of the present invention, there is provided a method for flotation of cesium garnet, comprising:

[0036] Provide a certain amount of mineral tailings, including plagioclase, cesium garnet and quartz;

[0037] subjecting a quantity of the mineral tailings to flotation conditions containing TM2 and NH4F in a ratio of about one part TM2 to 2.3 parts NH4F at a pH of about 2, or about 1.98 to about 2.02, wherein the TM2 comprises about 1 part sodium sulfonate and about 2 parts tallow amine acetate, thereby separating plagioclase from pyrope and quartz,

[0038] Recover plagioclase;

[0039] subjecting the pyrope and quartz to flotation conditions comprising TM2 and NH4F at a pH of about 2.35 to about 2.8, or about 2.6 to about 2.8, or about 2.35 to about 2.45, or about 2.35 to about 2.6, thereby separating the pyrope from the quartz, and

[0040] Recovering cesium garnet.

[0041] The sodium sulfonate may be sodium sulfonate SNS 457N TM .

[0042] Tallowamine acetate can be Armac T TM .

[0043] Plagioclase can be separated from chorite and quartz by subjecting the mineral tailings to at least three separate flotation stages.

[0044] The cerium garnet can be separated from the quartz in at least 2 separate flotation stages.

[0045] According to another aspect of the present invention, there is provided a method for recovering pyrope from mineral tailings, comprising:

[0046] a) provide a certain amount of mineral tailings, including pyroxene, spodumene, mica, feldspar, plagioclase, pyroxene and quartz;

[0047] b) subjecting a quantity of the mineral tailings to flotation conditions including a spodumene collector at a pH of about 9 to about 9.3 to separate the mineral tailings into separated spodumene and mineral tailings including spodumene, mica, feldspar, plagioclase, pyrope and quartz;

[0048] c) recovering lithium phosphate;

[0049] d) subjecting the mineral tailings comprising spodumene, mica, feldspar, plagioclase, pyrope and quartz to flotation conditions including a spodumene collector at a pH of about 9 to about 9.3, thereby separating the mineral tailings into separated spodumene and mineral tailings comprising mica, feldspar, plagioclase, pyrope and quartz;

[0050] e) recovering the floated spodumene;

[0051] f) subjecting the mineral tailings comprising mica, feldspar, plagioclase, pyrope and quartz to flotation conditions including a mica collector at a pH of about 2.26 to about 2.3 or about 2.3, thereby separating the mineral tailings into separated mica and mineral tailings comprising feldspar, plagioclase, pyrope and quartz;

[0052] g) recovering the floated mica;

[0053] h) subjecting the mineral tailings comprising feldspar, plagioclase, pyrope and quartz to flotation conditions including a feldspar collector at a pH of about 2.1 to about 2.2 or about 2.13 to about 2.17 to separate the mineral tailings into separated feldspar and mineral tailings comprising plagioclase, pyrope and quartz;

[0054] i) Recover the flotation feldspar

[0055] j) subjecting a quantity of mineral tailings containing plagioclase, pyrope and quartz to flotation conditions containing TM2 and NH4F at a pH of about 2, wherein the ratio of TM2 to NH4F is about 1 part TM2 to about 2.3 parts NH4F, wherein the TM2 contains about 1 part sodium sulfonate and about 2 parts tallow amine acetate, thereby separating the mineral tailings into separated plagioclase and mineral tailings containing pyrope and quartz;

[0056] k) recovering the floated plagioclase;

[0057] l) subjecting a quantity of mineral tailings containing pyrope and quartz to flotation conditions containing TM2 and NH4F at a pH of about 2.4 to about 2.8 or about 2.6 to about 2.8, wherein the ratio of TM2 to NH4F is about 1 part TM2 to about 2.3 parts NH4F, thereby separating the mineral tailings into separated pyrope and quartz; and

[0058] m) recovering the flotated cerium garnet.

[0059] The lithium phosphate collector may include any lithium phosphate collector known in the art, for example, (1) about 2 parts M and about 5 servings 727 accelerator mixture; (2) Talon A150 TM or (3) PolyfloatFA27 TM .

[0060] Aristonate M is a medium molecular weight, low foaming oil-soluble sodium alkyl aryl sulfonate; 727 Accelerator is a mixture of fatty acids, sulfonated compounds and glycol ethers.

[0061] In some embodiments, a lithium phosphate bubbler is added together with the lithium phosphate collector. The lithium phosphate bubbler can be any suitable lithium phosphate bubbler known in the art, such as W31.

[0062] W31 is a (2-methoxymethylethoxy)propanol mixture.

[0063] The spodumene collector may be any suitable spodumene collector known in the art, for example, A mixture of 727 accelerators or different spodumene collectors such as Talon A150 or Polyfloat FA27 as described above.

[0064] The spodumene bubbler may be added together with the spodumene collector. The spodumene bubbler may be any suitable spodumene bubbler known in the art, such as W31.

[0065] In some embodiments, between steps (e) and (f), the mineral tailings are decanted to remove the alkaline solution and re-slurried in an acidic solution.

[0066] The mica collector may include any suitable mica collector known in the art, for example, a mica collector comprising about 3 parts Duomeen About 2.5 servings of Armac T TM and about 0.5 parts Armeen C TM mixture.

[0067] Duomeen It is a mixture of amines, N-C16-C18-alkyl-(even number, C18 unsaturated)propane-1,3-diamine di[(9Z)-octadec-9-enoate].

[0068] Armeen C TM Made from cocoamine.

[0069] The feldspar collector may be any suitable feldspar collector known in the art, for example, comprising about 3 parts of Duomeen About 2.5 servings of Armac T TM and about 0.5 parts Armeen C TM mixture.

[0070] In some embodiments, between steps (a) and (b), the mineral tailings are subjected to an acid wash and an alkaline wash.

[0071] In some embodiments, between steps (a) and (b), the mineral tailings are subjected to an acid wash at a pH of about 2 and an alkaline wash at a pH of about 11.

[0072] The sodium sulfonate may be sodium sulfonate SNS 457N TM .

[0073] Tallowamine acetate can be Armac T TM .

[0074] Plagioclase can be separated from chorite and quartz by subjecting the mineral tailings to at least three separate flotation stages.

[0075] The cerium garnet can be separated from the quartz in at least 2 separate flotation stages.

[0076] As those skilled in the art are aware, tailings size is an important consideration in the flotation process. For example, minerals with finer sizes are more easily suspended in solution and attached to collector bubbles, which is necessary for flotation. As discussed herein, tests have been conducted with different size ranges and have shown that the finer size ranges (-212 or -300 μm) have higher recoveries than the coarser range (-425 μm). Since obtaining finer material means grinding, which in turn means energy consumption and maintenance costs, the material is typically used with the coarsest grind possible.

[0077] Figure 1The approximate percentages of the different size ranges of the TWA material are shown. It can be seen that the combined sample is about 3% pyrope, about 8% spodumene, about 4% muscovite, about 42% quartz, about 14% feldspar, about 27% plagioclase, and about 2% pyrophyllite, with trace amounts of silicates, pyroxenites, oxides, calcite, calcium phosphates, and other materials.

[0078] By size, tailings larger than 300 μm are about 2% pyroxene, about 7% spodumene, about 5% muscovite, about 40% quartz, about 18% feldspar and about 27% plagioclase, as well as trace amounts of pyroxenite, silicates, fluopyrite, oxides, calcite, calcium phosphate and other materials.

[0079] from Figure 1 It can be seen that the 300-212 μm tailings contain about 2% of cerium garnet, about 7% of spodumene, about 6% of muscovite, about 40% of quartz, about 15% of feldspar, about 29% of plagioclase and about 1% of pyroxenite, and contain trace amounts of silicates, fluopyrite, oxides, calcite, calcium phosphate and other materials.

[0080] The 212-150 μm tailings are about 4% pyroxene, about 11% spodumene, about 5% muscovite, about 39% quartz, about 12% feldspar, about 26% plagioclase and about 3% pyroxenite, and contain trace amounts of silicates, fluopyrite, oxides, calcite, calcium phosphate and other materials.

[0081] Tailings smaller than 150 μm are about 4% pyroxene, about 12% spodumene, about 6% muscovite, about 32% quartz, about 12% feldspar, about 27% plagioclase and about 2% pyroxenite, and contain trace amounts of silicates, fluopyrite, oxides, calcite, calcium phosphate and other materials.

[0082] The chemical formula of plagioclase is Na(AlSi3O8), with Na(11%Na2O) as the main component; the chemical formula of feldspar is K(AlSi3O8), with K2O accounting for 12.6%. Feldspar contains rubidium, while plagioclase contains almost none. In each flotation, we checked 8 elemental analyses to analyze the minerals: Li, Na, K, Rb, Cs, Fe, Si and P.

[0083] As used herein, "about" or "approximately" for numerical values ​​refers to the base value plus or minus 10%. For example, "about 100" means "90-110 (inclusive)".

[0084] Flotation is based on the surface chemistry of minerals. Minerals are usually wettable but will not float unless a hydrophobic collector is used, which consists of an organic compound that creates gas bubbles that can attach to suitable minerals.

[0085] The most complex part of flotation is the selection of reagents, which can be divided into three groups: collectors, frothers, and modifiers. Modifiers can be further subdivided into activators, depressants, pH adjusters, and dispersants. While the general mechanism of flotation is understood, the specific surface reactions are not necessarily easy to predict or understand. For example, it may be known that the reagent for the desired mineral must be a cationic collector, but a suitable cationic collector needs to not attract other negatively charged minerals.

[0086] Each collector has unique properties (such as, but not limited to, charge and / or attraction of different organic groups) that may attract a particular mineral or group of minerals, as described herein.

[0087] Tailings are often composed of geologically co-existing minerals with similar flotation characteristics, which makes the separation of individual minerals difficult. Specifically, when one desired mineral is floated, other minerals may be entrained with the desired mineral.

[0088] However, it is important to note that while these minerals may have similar flotation characteristics, they are, after all, different minerals. Therefore, the flotation kinetics of two or more coexisting minerals are different, allowing their separation if suitable reagents are used.

[0089] For example, for the same collector, pyroxenite floats first, while spodumene takes longer to attach to the collector. Due to this difference in their respective flotation kinetics, pyroxenite and spodumene can be separated under a suitable collector.

[0090] Differences in mineral flotation kinetics are another important property used in flotation. As is known to those skilled in the art, if minerals have different points of zero charge (PZC, or isoelectric points), they will have different floating kinetics.

[0091] For example, for oxide minerals, the surface potential determining ions are hydrogen ions and hydroxide ions. Therefore, the surface potential of oxide minerals is greatly affected by the pH environment of the mineral. This means that at a certain pH value, the surface charge of the mineral is zero. The pH value at which the surface charge is zero is crucial to its surface electrical attraction potential. As known to those skilled in the art, at any pH value greater than this value, the surface of the mineral will be negatively charged, and at any pH value below this value, the surface of the mineral will be positively charged. For example, when the surface of the mineral is negatively charged, the mineral can be attached to a suitable positively charged hydrophobic collector.

[0092] In general, the PZC of TMA tailings is at low pH values. For example, spodumene has a PZC at pH = 2 (Filippov et al., 2019); quartz has a PZC of 3 and iron oxide has a PZC of 6.7. For example, above the PZC, as the pH increases, the surfaces of all of these minerals may become negatively charged, but the rate and extent of the charge change will depend on the respective PZCs and / or their respective change profiles. This means that the degree of attraction for a particular collecting agent may be different for two different minerals, even if the two minerals can be floated by the same reagent. As will be appreciated by those skilled in the art, this means that in some embodiments, control of the pH and dosage of the reagents is important for the recovery of a particular mineral.

[0093] It can be seen that since flotation is within a certain size range and the flotation machine is mixing and generating air to create physical movement to separate the minerals, these physical characteristics need to be considered.

[0094] During and after the attachment between the mineral and the collector, which can generally be described as (a) mixing and conditioning and (b) flotation, mixing tanks and / or flotation cells are used for separation and / or classification.

[0095] For example, flotation cells can be used to produce bubbles of uniform size that have a certain degree of surface attraction and floatability. During the flotation process, the flotation or settling of mineral particles depends largely on mechanical settling and slurry parameters.

[0096] In conclusion, the flotation results depend largely on the reagents used and the flotation conditions (flotation cell, agitation / wind speed, temperature and pH value, etc.). Previously, the reagents and conditions used for the flotation of spodumene, mica and feldspar were already very mature; however, no practical method for the flotation of cesium garnet has been found.

[0097] As discussed in more detail below, it has been determined and / or demonstrated that the combination of collectors, frothers and modifiers used in the process described below can achieve good selectivity and good recovery of the mineral to be floated.

[0098] Specifically, as mentioned above, the most concentrated cesium content developed from the West TMA was slightly above 5% Cs2O, resulting in a recovery of approximately 60% of the cesium. This was achieved with HF, which, as mentioned above, is a volatile / highly toxic reagent.

[0099] In the existing process, after lithium concentrate is removed as a product, mica and feldspar are removed as tails, and the main remaining minerals are pyrope, plagioclase, quartz, etc., which are not easy to separate and account for about 70% by weight. For technicians in this field, this is one of the reasons why pyrope cannot be concentrated. Specifically, the difficulty lies in the similarity of mineralogy. However, through extensive literature review and subsequent "trial and error" testing, we unexpectedly developed a reagent mixture and optimized reaction conditions, thereby completely removing plagioclase, a single-grade pyrope product with a recovery rate of 65%, a 16% Cs2O grade, and a relatively pure quartz product, while the content of other elements (such as lithium) is low, and other elements such as K, Na, Rb, Fe, Cs and P. In addition, the developed reagent mixture has no obvious safety impact on the mineral processing operation.

[0100] For example, as discussed herein, we have developed a non-HF and low toxicity reagent that, for example, can concentrate even low-grade (1.55%) cesium garnet up to over 16% Cs2O with over 65% cesium recovery. That is, as discussed herein, for example, the process concentrates cesium garnet at least 10-fold regardless of the starting concentration.

[0101] To compare the results of the different reagents, all tests were completed using the Denver D12 flotation cell.

[0102] The newly established treatment procedures were developed from more than 500 tests conducted by Tanco in the past. Figure 3 As shown, the West TMA process consists of 7 steps:

[0103] 1. Screening and cleaning of TMA sand

[0104] 2. Flotation and recovery of lithium phosphate

[0105] 3. Spodumene flotation and recovery

[0106] 4. Mica flotation and removal

[0107] 5. Feldspar flotation and removal

[0108] 6. Plagioclase flotation and removal

[0109] 7. Flotation of garnet and recovery of garnet and quartz

[0110] For each step, we modified the experimental conditions according to best practices. At each step from feed to concentrate, we filter, dry and check samples to determine lithium, sodium, potassium, rubidium, iron, silicon, phosphorus and cesium, from which we indirectly assess the loss or gain of minerals at each stage, as described below. In this way, we gradually developed our current methods and reagents. Typically, we check the following concentrates / tails:

[0111] Slime from raw material acid / alkaline detergents and decantants after spodumene flotation

[0112] · Lithium phosphate, from the flotation of lithium phosphate

[0113] Spodumene, from spodumene flotation

[0114] Mica, from single-stage mica flotation

[0115] Feldspar from 4-stage feldspar flotation

[0116] Plagioclase from level 3 plagioclase flotation

[0117] ·Cesium garnet from 2nd level cesium garnet flotation

[0118] Quartz, from the tailings of garnet flotation

[0119] As discussed herein, in some embodiments, the feed is first subjected to an acid wash and then to an alkaline wash.

[0120] For each procedure, the following sections describe the methods (old / new) and reagents (old / new). Particular attention should be paid to the methods and reagents in steps 6 and 7. The inclusion of cesium has already been fully considered when applying reagents (such as spodumene, spodumene, mica, feldspar and plagioclase) in the early flotation stages.

[0121] 1. Screening and washing of TMA sand

[0122] Mineral size is related to the degree of mineral release. We tested multiple size ranges (in μm) of West TMA sand: +425, -425-+212 and -212, which showed different characteristics. For most tests, we used a mineral size of -425 μm, weighing 2.2 kg. The flotation cell used was a 4 liter square Denver type flotation machine. We used an impeller speed of 1450 rpm and a temperature range of 17 to 20 ° C.

[0123] We previously conditioned the sand with NaOH at a pH of about 11 for 10 minutes, then dumped the slime onto the sand line and used a magnetic bar to remove magnetic material from the tailings.

[0124] We currently wash the screened feed using dilute acid (H2SO4, pH≈2) and alkaline (NaOH, pH≈11) solutions for 10 minutes each, achieving higher recoveries of lithium and cesium compared to tests with alkaline wash (conditioning) alone.

[0125] Because tailings are used, processing can be complicated by contaminants such as dirt, old collectors, overly fine gangue minerals, etc. However, we use H2SO4 to clean the mineral surface followed by an alkaline wash. Surprisingly, we found that both the cesium and lithium mineral recoveries and grades were improved. While not wishing to be bound to a particular theory or hypothesis, it may be that through both the acid wash and the alkaline wash, the organic material is dissolved and the fine slime is better dispersed, resulting in improved removal during the desludging process. That is, the acid wash removes organic contaminants that cannot be dissolved by the alkaline wash alone. In addition, the additional acid wash removes more of the fine material (slimes) covering the mineral surface, providing a cleaner mineral surface for subsequent processing.

[0126] After each wash, the slime was poured into buckets (in an alkaline environment) along with the decantate from spodumene flotation and samples were filtered / dried for testing as slime samples, as described above.

[0127] In one embodiment of the present invention, this stage includes:

[0128] 1) Screening and separation of tailings to remove unwanted debris, such as organic materials;

[0129] 2) Sizing the tailings, for example, by flotation machines and / or grinders, to achieve a desired size, for example, less than 300 μm;

[0130] 3) desludging the material as described above (Desludging 1) to remove fine minerals and gangue from the surface of the tailings and prepare the tailings for flotation;

[0131] 4) As described above, use an abrasive scrubber to scrub the particle surface in both acid and alkaline washes to dissolve any chemical residues on the tailings surface;

[0132] 5) removing any magnetic material, for example, using a magnetic separator; and

[0133] 6) A second desludging (Desludging 2) is performed to remove dissolved residues.

[0134] Specifically, an initial screening step, for example using a 0.5 mm screen, separates the organic material from the tailings.

[0135] As will be appreciated by those skilled in the art, the magnetic material may be, for example, residual steel from a previous grinding operation. This material may be removed using a high intensity magnetic separator or a low intensity magnetic separator (eg, a 2000 Gauss magnetic separator).

[0136] In some embodiments, the mineral size is reduced to below 300 μm for flotation using a flotation mill mill set to 300 μm. In some embodiments, mineral tailings above 300 μm are fed to a ball mill.

[0137] In some embodiments, the tailings are acid washed using a low pH abrasive scrubber for about 10 minutes.

[0138] In some embodiments, the tailings are alkaline washed using a high pH abrasive scrubber for about 10 minutes.

[0139] The mixture may be deslimed using a cyclone or hydrocyclone. As will be appreciated by those skilled in the art, this removes any residue dissolved from the surface of the tailings and also removes any fine particles.

[0140] 2. Lithium aluminum sulfate flotation and recovery

[0141] At this stage, we follow our traditional method to recover lithium phosphate. Specifically, the reagent mixture ( M: 727 Promoter, about 2 parts to about 5 parts by weight, about 121 g / t) is used for lithium phosphate flotation, after 3 minutes of adjustment and 1 minute of collecting the floated concentrate. The pH value after adjustment is about 9 to about 9.3, which is the same as spodumene flotation. In some embodiments, a lithium phosphate bubbler is added, such as W31. All other conditions (such as temperature and impeller speed) were the same throughout the tests.

[0142] Heliosphene is easier to float than spodumene (using the same reagents). The main elements in heliosphene are phosphorus and lithium.

[0143] In some embodiments, the weight percentage of the lithium apatite is 12-19%, and the main oxides are Li (3.3-4.3% assay, 58-71% recovery) and P (5.8-7.7% assay, 82-94% recovery).

[0144] 3. Spodumene flotation recovery

[0145] Based on the flotation reaction kinetics, we used the same conditions, reagents and methods mentioned above to recover spodumene after the flotation of lithiasite.

[0146] As can be seen, spodumene contains much less phosphorus than spodumene, but has comparable lithium content. Compared to other reagent mixtures for lithium flotation, this reagent mixture entrains less cesium in the flotation of spodumene and spodumene, while still providing good lithium recoveries.

[0147] In some embodiments, the weight percent of spodumene is 10-16%, and the major oxide is Li (1.0-2.2% assay, 13-20% recovery).

[0148] In some embodiments, the material is deslimed again after spodumene flotation, which has two purposes: desliming and reducing reagent interactions. Initially, we performed this step because lithium concentrate production is carried out at high pH (about 9 to about 9.3), while the rest of the flotation is carried out under acidic conditions. By desliming, reagent residues and slime can be removed simultaneously. As will be understood by those skilled in the art, in full-scale production, this can be achieved by other means, for example, using a hydrocyclone or a thickener, if appropriate.

[0149] 4. Mica flotation and removal

[0150] Mica flotation is carried out under acidic conditions, so in this step, we use, for example, a hydrocyclone to decant the alkaline solution (part of the slime) to remove unused reactants after spodumene flotation, and re-slurry the tailings in an acidic environment (pH = about 2.26 to about 2.30) for 10 minutes. The flotation reagent formulation was previously used for West TMA recovery testing. The mixture was prepared by mixing Tomy (cationic alkyl diamine with a nonpolar fatty tail), Armac T TM (tallowamine acetate) and Armeen C TM (Coconut amine) (about 3 to about 2.5 to about 0.5 weight) and other reagents are suspended in DI (deionized) water for several hours, prepared at about 50°C, until the mixture is uniform. The application rate is about 82 grams / ton. After conditioning the mixture for 3 minutes, the mica concentrate is floated.

[0151] As discussed in this article, micas are more easily floated than feldspar using the same reagents. Micas include muscovite and lepidolite; the difference is that muscovite does not contain lithium, while lepidolite does. Both lepidolite and feldspar are dominated by potassium and rubidium.

[0152] In some embodiments, the weight percentage of mica is 3-4%, and the main oxides are Li (1.0-1.4% assay, 4-5% recovery), Rb (1.5-1.9% assay, 12-21% recovery) and K (5.8-7.3% assay, 10-21% recovery).

[0153] 5. Feldspar flotation and removal

[0154] The 4-stage feldspar flotation process is the same as the mica flotation and uses the same reagent mixture, but the dosage per stage is lower (about 68 g / t) and the pH is about 2.1 to about 2.2 or about 2.13 to about 2.17 (compared to pH 2.3 for the 500+ test). As with the other stages, each stage is conditioned for 3 minutes with one minute of concentrate collection.

[0155] At this stage, slightly reduced pH was shown to significantly reduce cesium inclusions while still providing good recoveries of the potassium- and rubidium-dominated feldspars.

[0156] In some embodiments, the collector TM3 includes Duomeen TDO, Armac T, and Armeen C in a ratio of about 3 to about 2.5 to about 0.5 or 3:2.5:0.5. Using the dosages we used, it was found that after four stages of feldspar removal, no detectable amount of TM3 remained, which means there is no need to worry about any effect of the collector on subsequent steps.

[0157] This is important because in previous tailings flotation testing at Tanco, in order to avoid reagent interactions when flotating cesium garnet, the feldspar tails had to be heat treated at 500°C to eliminate the collector used previously. However, surprisingly, we can see that we did not have to perform any active steps to eliminate TM3 from the reaction mixture. While not wishing to be bound by a particular theory or hypothesis, it is thought that because the mineral is initially thoroughly cleaned and subsequently maintained in a dynamic environment, the reagents do not have as much time to adhere to the mineral. As one skilled in the art will appreciate, the selectivity of the reagents used in this process greatly helps to reduce these undesirable reactions.

[0158] In some embodiments, the feldspar weight percentage is 11-19% and the major oxide is K (2.6-3.1% assay, 14-36% recovery).

[0159] 6. Plagioclase flotation and removal

[0160] The reagent mixture applied at this stage was originally designed for flotation of pyrope with remarkable results: one often sees 98% to 100% of the cesium float and separate from the quartz tail (also very clean), but at a lower grade. Experiments have shown that separating plagioclase from pyrope is much more difficult than separating plagioclase from quartz. In pursuit of the optimum pH for pyrope flotation, we have found that at lower pH values ​​of about 2, such as about 1.98 to about 2.02, rather than the 2.2 or 2.3 previously used, more plagioclase floats than pyrope; however, at pH values ​​of about 2, almost no material floats. At the same time, we have found that the dosage of the reagents also affects the separation of plagioclase and pyrope, as will be explained below.

[0161] Reagents

[0162] Two reagents are used in plagioclase flotation: TM2, a mixture of sodium sulfonate SNS 457N and Armac T in a ratio of 1:2 by weight, mixed with deionized water at 50 °C for several hours until the mixture is homogeneous; and ammonium fluoride (NH4F), a modifier of the surface charge variation of the mineral. The TM2 reagent is based on a mixture of feldspar collectors (Bulatovic 2014), in which sodium petroleum sulfonate (anionic collector) is used to flot albite. Specifically, sodium sulfonate SNS 457N (Additiv Chemie Luers) is also an anionic collector, and the entire mixture carries a positive charge due to the cationic nature of Armac T (tallowamine acetate, Nouryon) and the mixing ratio used. However, the pH used for the reaction is considered unfavorable for the flotation of plagioclase and pyrope. It is important to note that if plagioclase and pyrope are floated together, they are difficult to separate, which means that the grade of any pyrope recovered will be greatly reduced.

[0163] Furthermore, TM2 alone will not float cerium garnet and requires ammonium fluoride. Specifically, ammonium fluoride is introduced because we want to suppress quartz, and this salt-containing fluoride ion is non-volatile under normal operating conditions (especially in water). This property can be related to the following equation (at high temperatures) (Dyachenko 2022):

[0164] SiO2+6NH4F→(NH4)2SiF6+2H2O+4NH3

[0165] However, at room temperature and under relatively mild conditions, only low levels of surface reactions are expected. As with the other reactions mentioned above, dosage is a critical parameter. Specifically, when we applied an excessive dosage, pyrope was found to be depressed by quartz. However, when we tried to suppress quartz using a low dosage, we found that pyrope was floating.

[0166] We tested different pH values ​​and checked the cesium capture at each pH and finally decided that a pH of about 2 should be used.

[0167] It is important to note that the fluoride salt NH4F is not volatile in water, especially in a low pH environment. Due to its inherent acidity and the low dosage (g / t) used in this application, it is unlikely that HF ​​will be generated during flotation under normal operating conditions.

[0168] dose

[0169] As mentioned above, we initially developed this reagent combination to flot pyrope, but we found that under more acidic conditions, and at lower dosages than used for pyrope, sodium-dominated plagioclase flots with little or no pyrope inclusion.

[0170] The flotation of plagioclase is divided into 3 stages, with the dosage being:

[0171] stage TM2(g / t) <![CDATA[NH4F(g / t) <!-- 10 -->]]> 1 73 169 2 66 152 3 59 137

[0172] Alternatively, 4 stages of flotation may be used, with the dosage being:

[0173] stage TM2(g / t) <![CDATA[NH4F(g / t)]]> 1 59 137 2 47 109 3 38 87 4 30 70

[0174] It is important to note that while dosages may vary depending on the attributes / properties of the tailings, TM2 and NH4F are always in direct proportion by weight: about 1 to about 2.3, or 1:2.3.

[0175] At each stage, the slurry pH was controlled at about 2, the reagent adjustment time was 3 minutes, and the concentrate collection time was 1 minute. At this pH, cesium garnet usually does not float. The dose applied was based on the estimated dry weight of the stage, which was 0.43 of the dose that could capture all cesium at this dry weight. Therefore, in the second stage, the estimated weight loss was 10%. It was found that when this ratio was adopted, the chance of cesium flotation was smaller, which may be attributed to the different specific gravity between plagioclase and cesium garnet (cesium garnet is heavier). According to Stokes' law, when particles exist in the same size range, heavier particles (such as cesium garnet) have a greater sedimentation velocity. For too much collecting agent (higher dose), cesium garnet may also float and therefore be lost in the plagioclase capture stage. That is, as mentioned above, at the same estimated dose, the cesium recovery rate is different under the same weight supply due to different particle size distribution.

[0176] As will be appreciated by those skilled in the art, in some embodiments, at least three stages of plagioclase flotation are required, depending on the size of the tailings and the distribution of the minerals. Specifically, since a significant weight percentage of the tailings is plagioclase, the advantage of using a large amount of water or a lower pulp density is to enhance the weight difference between plagioclase and other heavier minerals, thereby better settling the other minerals and thus more clearly separating the plagioclase.

[0177] Additionally, as plagioclase is removed at each flotation stage, less plagioclase remains, and therefore less TM2 and NH4F are used to float the plagioclase without entraining chorite (especially in the smaller size range). Specifically, as discussed herein, the entrainment of chorite within the plagioclase also increases when larger volumes of collector are used. Notably, for example, by reducing the pH from 2.3 to 2.2, the amount of cesium entrainment is reduced from about 10% to about 5% without a significant change in yield. In fact, lowering the pH to around 2.15 further reduces entrainment by an average of 0.5%.

[0178] In some embodiments, the weight percent of plagioclase is 14-24%, and the major oxide is sodium (6.2-7.7% assay, 22-53% recovery).

[0179] 7. Flotation of garnet and recovery of garnet and quartz

[0180] Since the dry material is estimated to be half of the feed in the cesium garnet flotation stage, the maximum dose applied is:

[0181] stage TM2(g / t) <![CDATA[NH4F(g / t)]]> 1 118 273 2 118 273

[0182] For feeds below 212 μm, the dosage ensures that all of the cesium or pyrope is captured and only trace or very small amounts of elements other than silicon are left in the quartz. When flotating pyrope, we have found that pH values ​​of about 2.35 to about 2.8, or about 2.4 to about 2.8, or about 2.6 to about 2.8, or 2.35 to about 2.45, or about 2.35 to about 2.6 are more favorable for pyrope flotation than at lower pH values.

[0183] Although TM2 is a mixture commonly used in mineral processing, the application of NH4F is not common, but after general analysis, its impact seems to be easily controlled. On the other hand, the application of NH4F can be reduced because there is almost no cesium to collect in the second stage of the flotation of the cesium garnet.

[0184] Plagioclase is lighter than pyrope (specific gravities 2.62 and 2.79, respectively), which makes it possible to separate them in the same size range using the same reagents. However, as mentioned above, dosage is an important parameter because initially the collecting agent only produces enough bubbles to float the plagioclase. That is, pyrope flotation also requires increased dosage and longer conditioning times compared to plagioclase flotation.

[0185] In addition, pH is also an important parameter, as evidenced by the fact that pyrope cannot float at lower pH values ​​(2), while plagioclase can float. Furthermore, although pyrope has a higher PZC pH than plagioclase, pyrope and plagioclase can float together in the presence of excess collector. Therefore, in order to separate these two minerals, it is necessary to exploit chemical and physical differences in the flotation process.

[0186] In some embodiments, the weight percentage of cerium garnet is 4-6% during the first stage flotation and 2-3% during the second stage flotation. The main oxide is cesium (4.1-12.4% assay percentage, 15-46% recovery for the first stage flotation; 4.4-15.7% assay percentage, 21-47% recovery for the second stage flotation).

[0187] In some embodiments, the remaining quartz is 20-25% by weight. The main oxide of quartz is silicon (96-100% assay, 23-26% recovery). As will be appreciated by those skilled in the art, quartz of this purity represents a potentially marketable product.

[0188] General comments on workmanship

[0189] The process design provides a non-HF method to concentrate cesium garnet with minimal operational and / or environmental impact due to low reagent dosage. In addition, cesium assays on concentrated cesium garnet showed double the amount of cesium recovered by HF flotation.

[0190] The possibility of enriching cesium garnet not only provides a solution for the extraction of cesium in the Western TMA, but also helps to enrich low-grade ores, thereby reducing processing costs in chemical plants.

[0191] With this process for processing Western TMA, we have 4 products: pyroxenite, spodumene, pyroxenite and quartz, which expands the economic potential. In addition, this flotation process is more economical than the traditional acid leaching method for producing quartz.

[0192] For example, by removing most of the plagioclase, cesium garnet can be enriched to high-cesium assays and associated only with quartz, which does not consume the acid; thus, a purer cesium salt can be produced.

[0193] Furthermore, in the current process design, the cesium entrainment in each step is taken into account by adjusting the pH value, reagent type and dosage, so that the concentration and recovery rate of cesium in the process are maximized.

[0194] While the preferred embodiment of the invention has been described above, it will be recognized and understood that various modifications may be made therein and the appended claims are intended to cover all such modifications which may fall within the spirit and scope of the invention.

[0195] References:

[0196] Bulatovic, Srdjan M. 2014. Handbook of Flotation Reagents: Chemistry, Theory and Practice: Volume 3: Flotation of Industrial Minerals. 1st edition. Elsevier.

[0197] Dyachenko, Alexander. 2022. Ammonium Fluorides in Mineral Processing. IntechOpen.

[0198] Filippov, Lev, Saeed Farrokhpay, Lichau Lyo, and Inna Filippova. 2019. ‘Spodumene Flotation Mechanism’. Minerals 9(6):372. doi:10.3390 / min9060372.

Claims

1. A method for flotation of cesium garnet, comprising: Provide a certain amount of mineral tailings, including plagioclase, cesium garnet and quartz; subjecting the amount of mineral tailings to flotation conditions containing TM2 and NH4F at a pH of about 2, wherein the ratio of TM2 to NH4F is about 1 part TM2 to about 2.3 parts NH4F, wherein the TM2 comprises about 1 part sodium sulfonate and about 2 parts tallow amine acetate, thereby separating plagioclase from pyrope and quartz, Recover plagioclase; subjecting the coleus and quartz to flotation conditions in the presence of TM2 and NH4F in a ratio of about 1 part TM2 to about 2.3 parts NH4F at a pH of about 2.35 to about 2.8, thereby separating the coleus from the quartz, and Recovering cesium garnet.

2. The method according to claim 1, characterized in that: The sodium sulfonate is sodium sulfonate SNS 457 N TM .

3. The method according to claim 1, characterized in that: The tallow amine acetate is Armac T TM .

4. The method according to claim 1, characterized in that: The plagioclase is separated from the chorite and quartz by subjecting the mineral tailings to at least three separate flotation stages.

5. The representation according to claim 1, characterized in that The paragonite is separated from the quartz in at least 2 separate flotation stages.

6. A method for recovering pyrope from mineral tailings, comprising: a) provide a certain amount of mineral tailings, including pyroxene, spodumene, mica, feldspar, plagioclase, pyroxene and quartz; b) subjecting the amount of mineral tailings to flotation conditions in the presence of a pyroxenite collector at a pH of about 9 to about 9.3 to separate the mineral tailings into separated pyroxenite and mineral tailings, wherein the mineral tailings include spodumene, mica, feldspar, plagioclase, pyrope and quartz; c) recovering lithium phosphate; d) subjecting the mineral tailings comprising spodumene, mica, feldspar, plagioclase, pyrope and quartz to flotation conditions in the presence of a spodumene collector at a pH of about 9 to about 9.3, thereby separating the mineral tailings into separated spodumene and mineral tailings, wherein the mineral tailings comprises mica, feldspar, plagioclase, pyrope and quartz; e) recovering the floated spodumene; f) subjecting the mineral tailings comprising mica, feldspar, plagioclase, pyrope and quartz to flotation conditions in the presence of a mica collector at a pH of about 2.26 to about 2.3, thereby separating the mineral tailings into separated mica and mineral tailings, wherein the mineral tailings comprises feldspar, plagioclase, pyrope and quartz; g) recovering the floated mica; h) subjecting the mineral tailings comprising feldspar, plagioclase, pyrope and quartz to flotation conditions in the presence of a feldspar collector at a pH of about 2.1 to about 2.2, thereby separating the mineral tailings into separated feldspar and mineral tailings, wherein the mineral tailings comprises plagioclase, pyrope and quartz; i) recovering the flotated feldspar; j) subjecting the amount of mineral tailings containing plagioclase, pyrope and quartz to flotation conditions containing TM2 and NH4F at a pH of about 2, wherein the ratio of TM2 to NH4F is about 1 part TM2 to about 2.3 parts NH4F, wherein the TM2 contains about 1 part sodium sulfonate and about 2 parts tallow amine acetate, thereby separating the mineral tailings into separated plagioclase and mineral tailings containing pyrope and quartz; k) recovering the floated plagioclase; l) subjecting the amount of mineral tailings containing pyrope and quartz to flotation conditions containing TM2 and NH4F at a pH of about 2.35 to about 2.8, wherein the ratio of TM2 to NH4F is about 1 part TM2 to about 2.3 parts NH4F, thereby separating the mineral tailings into separated pyrope and quartz; and m) recovering the flotated cerium garnet.

7. The method according to claim 6, characterized in that The lithium phosphate collector is M: 727 accelerator mixture, weight ratio of about 2 to about 5.

8. The method according to claim 6, characterized in that The ferrite bubbler is added together with the ferrite collector.

9. The method according to claim 8, characterized in that Lithium aluminum sulfate bubbler is W31.

10. The method according to claim 6, characterized in that Spodumene collector Spodumene collector is 727 accelerator mixture, weight ratio of about 2 to about 5.

11. The method according to claim 6, characterized in that The spodumene bubbler is added together with the spodumene collector.

12. The method according to claim 11, characterized in that Spodumene bubbler is W31.

13. The method according to claim 6, characterized in that Between steps (e) and (f), the mineral tailings are decanted to remove the alkaline solution and re-slurried in an acidic solution.

14. The method according to claim 6, characterized in that The mica collector comprises a mixture of about 3 parts Duomeen About 2.5 servings of Armac T TM and about 0.5 parts Armeen C TM .

15. The method according to claim 6, characterized in that The feldspar collector comprises a mixture of about 3 parts Duomeen About 2.5 servings of Armac T TM and about 0.5 parts Armeen C TM .

16. The method according to claim 6, characterized in that Between steps (a) and (b), the mineral tailings are subjected to an acid wash and then an alkaline wash.

17. The method according to claim 6, characterized in that Between steps (a) and (b), the mineral tailings are subjected to an acid wash at a pH of about 2 and then to an alkaline wash at a pH of about 11.

18. The method according to claim 6, characterized in that The sodium sulfonate is sodium sulfonate SNS 457 N TM .

19. The method according to claim 6, characterized in that Tallowamine acetate is Armac T TM .

20. The method according to claim 6, characterized in that Plagioclase is separated from chorite and quartz by subjecting the mineral tailings to at least three separate flotation stages.

21. The method according to claim 6, characterized in that The cerium garnet is separated from the quartz in at least 2 separate flotation stages.