Preparation method for improving torque expression precision of orthodontic square wire
Through drawing-rolling tandem processing and mirror polishing technology, the problem of insufficient accuracy in orthodontic square wire torque expression is solved, achieving more stable tooth correction force and more precise tooth movement.
Patent Information
- Application Number
- CN202410871863.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-29
AI Technical Summary
The existing orthodontic square wire preparation method is difficult to control the torque expression accuracy, resulting in unstable tooth correction force and affecting the treatment effect.
Using drawing-rolling tandem processing and mirror polishing technology, by determining the deformation amount of the drawing fire and the deformation amount of the drawing pass, the edge curvature radius of the orthodontic square wire is controlled to ensure the accuracy of torque expression, and through mirror polishing Remove the scale and maintain the consistency of the edge curvature.
It improves the torque expression accuracy of the orthodontic square wire in the groove of the orthodontic bracket, establishes a stable orthodontic mechanics system, controls the movement of the teeth more accurately, and enhances the orthodontic effect.
Smart Images

Figure CN118847745A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of orthodontic square wires, and in particular to a preparation method for improving the torque expression accuracy of orthodontic square wires. Background Art
[0002] In orthodontic treatment, torque force is an important means to control the movement of teeth in three dimensions, and the expression of torque force is mainly achieved clinically by orthodontic square wires. The cross-section of the orthodontic square wire is square. When it is tied into the groove of the orthodontic bracket, which is also square, the height dimension of the orthodontic square wire is between 0.40 and 0.54 mm, and the width of the common orthodontic bracket groove is 0.56 to 0.58 mm. The height dimension of the orthodontic square wire is smaller than the width dimension of the orthodontic bracket groove, and there is a gap between the two. Therefore, the orthodontic square wire uses the torsion of its square cross-section to generate a pair of couples on the orthodontic bracket, thereby indirectly applying correction force and torque to the teeth, thereby achieving three-dimensional control of the root and crown.
[0003] Furthermore, the height of the orthodontic square wire is smaller than the size of the orthodontic bracket groove. When the orthodontic square wire is tied into the orthodontic bracket groove, a gap will be generated between the two, which is the clearance angle. The torque expression of the orthodontic square wire is the torque angle after eliminating the clearance angle with the orthodontic bracket. The size of the clearance angle directly affects the torque expression of the orthodontic square wire.
[0004] Furthermore, the edge bevel of orthodontic square wire refers to the fact that during the preparation and production of orthodontic square wire, due to the influence of material properties and production process, the four edges of the orthodontic square wire are not right angles, but have a certain curvature. This arc is the edge bevel of the orthodontic square wire. Gu Min et al. measured and analyzed the clearance angles of several commonly used orthodontic square wires and concluded that the clearance angle of nickel-titanium square wire is significantly larger than that of stainless steel square wire. The difference has an obvious corresponding relationship with the difference in the edge bevels of the two. The edge bevel of nickel-titanium square wire> stainless steel square wire. Sebanc et al. also found that the edge bevel of TMA wire> stainless steel square wire> nickel-chromium alloy wire. Gu Min et al. measured and analyzed using the intercept measurement method and concluded that in a 0.022-inch bracket, a stainless steel square wire with a width of 0.025 inches loses about 4° of torque for every 0.001-inch reduction, while a nickel-titanium square wire with a width of 0.025 inches loses about 6° of torque for every 0.001-inch reduction.
[0005] Therefore, it is necessary to improve the existing orthodontic square wire preparation method, reduce the arc radius of the four edges of the orthodontic square wire, make the edge bevel of the orthodontic square wire of the same material and different cross-sectional sizes consistent, improve the torque expression accuracy of the orthodontic square wire in the orthodontic bracket groove, provide clinicians with a stable orthodontic mechanical system, help clinicians determine a reasonable torque angle, and thus improve the orthodontic treatment effect. Summary of the invention
[0006] In order to solve the problem that it is difficult to control the torque expression accuracy of the orthodontic square wire in the groove of the orthodontic bracket in the existing orthodontic square wire preparation method, the present invention provides a preparation method for improving the torque expression accuracy of the orthodontic square wire.
[0007] The present invention is achieved by adopting the following technical solutions:
[0008] A preparation method for improving the torque expression accuracy of orthodontic square wire, the method comprising the following steps:
[0009] Step S1: determining the deformation amount of the orthodontic square wire after drawing;
[0010] Step S2: determining the starting round wire diameter of the orthodontic square wire before drawing according to the target cross-sectional area of the orthodontic square wire;
[0011] Step S3: determining the deformation amount of the orthodontic square wire during each drawing pass;
[0012] Step S4: performing drawing-rolling tandem processing on the orthodontic square wire according to the deformation amount of the drawing fire and the deformation amount of the drawing pass;
[0013] Step S5: mirror polishing the orthodontic square wire.
[0014] Further, the drawing deformation is set to B, that is, when the actual drawing deformation of the orthodontic square wire reaches the drawing deformation B, an intermediate annealing is required to eliminate the tissue stress of the orthodontic square wire and reduce the hardness of the orthodontic square wire; determining the drawing deformation B of the orthodontic square wire includes the following steps;
[0015] Step S1.1: Select an orthodontic square wire of standard diameter, set N square molds with a deformation amount of 10% per pass, and the cross-sectional area S1 of the first square mold matches the orthodontic square wire of standard diameter;
[0016] Step S1.2: passing an orthodontic square wire of standard diameter through N square dies in sequence, and performing cold deformation square wire drawing, until the orthodontic square wire is broken in the nth square die, and calculating the sum of the deformation amount from the first square die to the n-1th square die as the limit fire deformation amount A, and obtaining the limit fire deformation amount of the orthodontic square wire to be broken as A; the value range of n is 0<n≤N;
[0017] Step S1.3: Set the safety factor to 80%, that is, the drawing deformation B of the orthodontic square wire is A×80%; when the actual drawing deformation of the orthodontic square wire reaches the drawing deformation B, perform an intermediate annealing to eliminate the work hardening generated during the drawing deformation of the orthodontic square wire.
[0018] Furthermore, the target cross-sectional area of the orthodontic square wire is set as S, and the initial wire diameter of the orthodontic square wire before drawing is obtained according to the deformation amount B of the drawing fire.
[0019] Furthermore, the drawing deformation amount is set as C, and determining the drawing deformation amount C of the orthodontic square wire includes the following steps:
[0020] Step S3.1: Take the orthodontic square wire in the as-supplied state and perform a tensile test to measure the tensile strength σ1 of the orthodontic square wire; take the orthodontic square wire in the solid solution state and perform a tensile test to measure the tensile strength σ2 of the orthodontic square wire; obtain the tensile strength σ of the orthodontic square wire; that is,
[0021] Step S3.2: Take M square dies, design the pass deformation C of the M square dies to increase in sequence with a constant t, and design the cross-sectional areas S of the M square dies to decrease in sequence with a constant z;
[0022] Step S3.3: Set the theoretical tensile force value F when the orthodontic square wire enters the square mold for drawing. The theoretical tensile force value F is the product of the cross-sectional area S of the square mold and the tensile strength σ during the orthodontic square wire drawing process, that is, F = σ × S; insert the orthodontic square wire with a starting round wire diameter of φ into M square molds, and measure the actual tensile force value F when entering the mth square mold. m , and at the same time, the theoretical tensile force value F when penetrating the m-th square mold is obtained according to the cross-sectional area S and the tensile strength σ of the m-th square mold; the value range of m is 0<m≤M;
[0023] Step S3.4: Determine the actual pulling force value F x Is it greater than the theoretical tensile force F? x ≤F, continue to insert and draw the m+1th square die; if F x >F, the drawing pass deformation C can be obtained as C m-1 .
[0024] Furthermore, the drawing-rolling tandem processing of the orthodontic square wire according to the drawing fire deformation amount and the drawing pass deformation amount includes the following steps:
[0025] Step S4.1: Take a round wire with a starting wire diameter of φ, and set the width and height of the square mold according to the target cross-sectional area S of the orthodontic square wire. Then, the number G of the square molds is obtained according to the drawing fire deformation B and the drawing pass deformation C, that is, the number of square molds is the ceiling rounding function;
[0026] Step S4.2: Drawing is performed in a square die with a deformation amount C in the g-th drawing pass, and the value range of g is 0<g≤G;
[0027] Step S4.3: Determine whether the edge radius R of the nickel-titanium orthodontic square wire is greater than 110 μm, determine whether the edge radius R of the TMA orthodontic square wire is greater than 90 μm, and determine whether the edge radius R of the stainless steel orthodontic square wire is greater than 90 μm. If so, proceed to step S4.4; if not, proceed to step S4.6;
[0028] Step S4.4: using a flat wire rolling mill to roll the orthodontic square wire; the outer surfaces of the two rollers moving relative to each other in the X direction are in contact with the two side surfaces in the width direction of the orthodontic square wire, and the outer surfaces of the two rollers moving relative to each other in the Y direction are in contact with the two side surfaces in the height direction of the orthodontic square wire; by screwing in or out the roller pressure knobs in the X direction and / or the Y direction, the pressure of the rollers in the X direction and / or the Y direction is controlled, so that the size of the orthodontic square wire in the width and height directions is further reduced, and the orthodontic square wire is squeezed in the directions of the four edge arcs, thereby recovering and reducing the gradually increasing radius of the four edge arcs generated by the square die drawing process;
[0029] Step S4.5: After rolling is completed, determine whether the edge radius of the nickel-titanium orthodontic square wire is 90μm≤R≤110μm, determine whether the edge radius of the TMA orthodontic square wire is 70μm≤R≤90μm, and determine whether the edge radius of the stainless steel orthodontic square wire is 70μm≤R≤90μm. If so, proceed to step S4.7; if not, proceed to step S4.4;
[0030] Step S4.6: Determine whether the edge radius R of the orthodontic square wire meets the target edge radius R 目 If the conditions are met, the orthodontic square wire preparation is completed; if not, proceed to step S4.7;
[0031] Step S4.7: Drawing is performed in a square die with a deformation amount of C in the g+1th drawing pass, where the value range of g is 0<g≤G; and step S4.3 is performed.
[0032] Furthermore, the pressing amount of the roller in the X direction and the Y direction is no more than 0.05 mm each time.
[0033] Furthermore, the orthodontic square wire includes TMA orthodontic square wire, stainless steel orthodontic square wire and nickel-titanium orthodontic square wire; the target edge radius R of the TMA orthodontic square wire is 目 The target edge radius R of the stainless steel orthodontic square wire is 60±10μm. 目 The target edge radius R of the nickel-titanium orthodontic square wire is 60±10μm. 目80±10μm.
[0034] Furthermore, the mirror polishing of the orthodontic square wire comprises the following steps:
[0035] Step S5.1: placing the orthodontic square wire into a placement slot that matches the outer contour of the orthodontic square wire, then applying water-soluble glue to both ends and the middle of the orthodontic square wire, and bonding the orthodontic square wire to the bottom end of the placement slot;
[0036] Step S5.2: Using compressed air as a power source, selecting polishing particles with elasticity, and using a programmed nozzle to bombard the orthodontic square wire placed inside the placement slot with polishing particles, while using a decompression valve to adjust the speed of the nozzle spraying polishing particles so that the nozzle can reciprocate along the contour of the placement slot; the polishing particles that collide with the orthodontic square wire are discharged from the leakage hole at the bottom of the placement slot;
[0037] Step S5.3: After the spraying is completed, the placement slot with the orthodontic square wire bonded thereto is immersed in water to dissolve the water-soluble glue, so that the orthodontic square wire is separated from the placement slot, and the moisture on the surface of the orthodontic square wire and the placement slot is blown dry;
[0038] Step S5.4: Turn the orthodontic square wire over, and perform steps S5.1, S5.2, and S5.3 again to obtain the orthodontic square wire with surface oxide scale and scratches removed.
[0039] Furthermore, the surface roughness R of the orthodontic square wire after mirror polishing is a Not more than 0.8μm.
[0040] Furthermore, the hardness value of the polishing particles is between 0.2 and 0.5 times the hardness value of the orthodontic square wire.
[0041] The structural design of the present invention is reasonable and reliable. Through theoretical modeling, the parameters of orthodontic square wire in the manufacturing process can be known, wherein the deformation amount of the drawing fire is the critical drawing cold deformation amount of the orthodontic square wire in the drawing process, and the deformation amount of the drawing pass is the critical drawing force that the orthodontic square wire can withstand in each drawing process. The deformation amount B of the drawing fire and the deformation amount C of the drawing pass can be obtained to formulate the optimal number of drawing dies and the drawing force according to the target size of the orthodontic square wire to the greatest extent. The core process of the front process is a method of orthodontic square wire drawing and rolling in series, and an orthodontic square wire with a stable edge curvature radius is prepared. The core process of the back process is a mirror polishing method, which not only removes the oxide scale on the surface of the orthodontic square wire during the heat setting process, but more importantly, the polishing particles will not damage the edge curvature radius of the orthodontic square wire, so that the edge bevel of the orthodontic square wire of the same material and different cross-sectional areas remains consistent, thereby improving the torque expression accuracy of the orthodontic square wire in the orthodontic bracket groove, establishing a stable and controllable orthodontic mechanical system, and more accurately controlling the movement of teeth. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a schematic diagram of the process flow of the present invention.
[0043] Figure 2 The stress-strain curves of the nickel-titanium orthodontic square wire of 0.014×0.025 inch in the as-supplied state and the solid solution state in the present invention;
[0044] Figure 3 The stress-strain curves of the TMA orthodontic square wires of 0.017×0.025 inch in the as-supplied state and the solid solution state in the present invention;
[0045] Figure 4 The stress-strain curves of the stainless steel orthodontic square wire of 0.019×0.025 inch in the as-supplied state and the solid solution state in the present invention;
[0046] Figure 5 This is a schematic diagram of the edge radius of the 0.014×0.025 inch nickel-titanium orthodontic square wire in Example 1 of the present invention;
[0047] Figure 6 This is a schematic diagram of the edge radius of the 0.017×0.025 inch TMA orthodontic square wire in Example 2 of the present invention;
[0048] Figure 7 This is a schematic diagram of the edge radius of the 0.019×0.025 inch stainless steel orthodontic square wire in Example 3 of the present invention;
[0049] Figure 8 It is a schematic diagram of the structure of the placement groove and the nozzle in the present invention.
[0050] In the figure: 1- placement groove, 2- nozzle, 3- leakage hole. DETAILED DESCRIPTION
[0051] The core process of orthodontic square wire preparation is the total drawing deformation and the deformation per pass. The drawing parameters of orthodontic square wires of different materials are different, and the drawing parameters of orthodontic square wires of the same material but different proportions are also different. The present invention proposes a preparation method for improving the torque expression accuracy of orthodontic square wires. Different from the prior art in which drawing parameters are judged based on the experience of staff, the present invention proposes a replicable, safe and efficient preparation method through theoretical modeling and combined with the processing performance characteristics of orthodontic square wires of different materials during specific drawing.
[0052] Example 1
[0053] Taking the preparation of nickel-titanium orthodontic square wire with a target size of 0.014×0.025 inch as an example, a preparation method for improving the torque expression accuracy of orthodontic square wire is provided. Figure 1 , Attachment Figure 2, Attachment Figure 5 As shown, the method comprises the following steps:
[0054] Step S1: determining the drawing deformation of the orthodontic wire; setting the drawing deformation to B, that is, when the actual drawing deformation of the orthodontic wire reaches the drawing deformation B, an intermediate annealing is required to eliminate the tissue stress of the orthodontic wire and reduce the hardness of the orthodontic wire; determining the drawing deformation B of the orthodontic wire includes the following steps:
[0055] Step S1.1: Select a nickel-titanium orthodontic square wire with a diameter of 1.0 mm, set N square molds with a deformation amount of 10% per pass, and the cross-sectional area of the square mold matches the nickel-titanium orthodontic square wire of 1.0 mm; that is, the cross-sectional areas of the N square molds are: S1 = 0.9 mm 2 、S2=0.81mm 2 、S3=0.73mm 2 、S4=0.66mm 2 、S5=0.59mm 2 ……;
[0056] Step S1.2: Pass a 1.0 mm nickel-titanium orthodontic square wire through N square dies in sequence, and perform cold deformation square wire drawing until the nickel-titanium orthodontic square wire is broken in the sixth square die. The sum of the deformation amount from the first square die to the fifth square die is calculated as the limit fire deformation amount, which is 50%, and the breaking limit fire deformation amount A of the nickel-titanium orthodontic square wire is 50%;
[0057] Step S1.3: Set the safety factor to 80%, that is, the drawing deformation B of the nickel-titanium orthodontic square wire is A×80%=40%; when the actual drawing deformation of the nickel-titanium orthodontic square wire reaches the drawing deformation B, perform an intermediate annealing to eliminate the work hardening generated during the drawing deformation of the nickel-titanium orthodontic square wire.
[0058] Step S2: Set the target cross-sectional area of the nickel-titanium orthodontic square wire to S = 0.23 mm 2 , that is, the target size of nickel-titanium orthodontic square wire is 0.014×0.025 inch, and the deformation amount B of the drawing fire is 40%. According to the deformation amount B of the drawing fire=40%, the initial wire diameter of the nickel-titanium orthodontic square wire before drawing is obtained.
[0059] Step S3: setting the drawing deformation amount C, determining the drawing deformation amount C of the nickel-titanium orthodontic square wire includes the following steps:
[0060] Step S3.1: Take three groups of 0.014×0.025 inch nickel-titanium orthodontic square wires in the as-supplied state for a tensile test, and measure the tensile strengths of the three groups of nickel-titanium orthodontic square wires to be 1849.1MPa, 1855.5MPa, and 1846.7MPa, respectively. Take the average value as the tensile strength σ1=1849.4Mpa of the nickel-titanium orthodontic square wire in the as-supplied state; take three groups of nickel-titanium orthodontic square wires in the solid solution state for a tensile test, and measure the tensile strengths of the three groups of nickel-titanium orthodontic square wires to be 534.0MPa, 544.5MPa, and 528.8MPa, respectively. Take the average value as the tensile strength σ2=535.8MPa of the nickel-titanium orthodontic square wire in the solid solution state; obtain the tensile strength σ of the nickel-titanium orthodontic square wire; that is, The tensile test for measuring the tensile strength of orthodontic square wire is a prior art and will not be described in detail here.
[0061] Step S3.2: Take 8 square dies, design the deformation C of the 8 square dies to increase in sequence with a constant of 2%, that is, C1 is 2%, C2 is 4%, C3 is 6%, C4 is 8%, C5 is 10%, C6 is 12%, C7 is 14%, C8 is 16%, and design the cross-sectional area S of the 8 square dies to be a constant of 0.02mm 2 Decrease in sequence, that is, S1 is 0.98mm 2 , S2 is 0.96mm 2 , S3 is 0.94mm 2 , S4 is 0.92mm 2 , S5 is 0.90mm 2 , S6 is 0.88mm 2 , S7 is 0.86mm 2 , S8 is 0.84mm 2 ;
[0062] Step S3.3: setting the theoretical pulling force value of the nickel-titanium orthodontic square wire when entering the square die for drawing to F, the theoretical pulling force value F is the product of the cross-sectional area S of the square die and the tensile strength σ of the nickel-titanium orthodontic square wire during drawing, that is, F=σ×S;
[0063] The nickel-titanium orthodontic square wire with a starting round wire diameter of φ=1.0 mm was first inserted into the first square mold, and the actual tensile force value F1=557N was measured when the wire was inserted into the first square mold. At the same time, according to the cross-sectional area S and tensile strength σ of the first square mold, the theoretical tensile force value F=0.98×1192.6=1168.8N was obtained when the wire was inserted into the first square mold; that is, F1<F;
[0064] Repeat the above steps to measure the actual pulling force value F2 = 636N when penetrating the second square mold, and obtain the theoretical pulling force value F = 0.96 × 1192.6 = 1144.9N when penetrating the second square mold; that is, F2 < F;
[0065] The actual tensile force value when penetrating the third square die is measured to be F3=759N, and the theoretical tensile force value when penetrating the third square die is F=0.94×1192.6=1121.0N; that is, F3<F;
[0066] The actual tensile force value F4 = 861N when penetrating the fourth square die is measured, and the theoretical tensile force value F = 0.92 × 1192.6 = 1097.2N when penetrating the fourth square die is measured; that is, F4 < F;
[0067] The actual tensile force value F5 = 972N when penetrating the fifth square die is measured, and the theoretical tensile force value F = 0.90 × 1192.6 = 1073.3N when penetrating the fifth square die is measured; that is, F5 < F;
[0068] The actual tensile force value F6 = 1067N when penetrating the sixth square die is measured, and the theoretical tensile force value F = 0.88 × 1192.6 = 1049.5N when penetrating the sixth square die is measured; at this time, F6>F;
[0069] It can be known that when the nickel-titanium orthodontic square wire with a diameter of 1.0 mm passes through a square die with a deformation of 12% in the sixth pass, its actual tensile force value F6 is greater than the theoretical tensile force F. Therefore, the drawing deformation of the nickel-titanium orthodontic square wire with a size of 0.014×0.025 inches is C=C5=10%.
[0070] Step S4: According to the drawing fire deformation amount B of 40% and the drawing pass deformation amount C of 10% obtained in the above steps S1 to S3, the nickel-titanium orthodontic square wire is subjected to drawing-rolling tandem processing, which includes the following steps:
[0071] Step S4.1: Take a nickel-titanium round wire with a starting wire diameter of φ=0.70 mm, and set the target cross-sectional area S of the nickel-titanium orthodontic square wire to 0.23 mm 2 , that is, the target size of the square die is 0.014×0.025 inch, and then the number of square dies G is obtained according to the drawing fire deformation B of 40% and the drawing pass deformation C of 10%, that is, the number of square dies is the ceiling rounding function;
[0072] Step S4.2: Drawing is performed in a square die with a deformation amount C in the g-th drawing pass, and the value range of g is 0<g≤G;
[0073] Step S4.3: Determine whether the edge radius R of the nickel-titanium orthodontic square wire is greater than 110 μm. If so, proceed to step S4.4; if not, proceed to step S4.6;
[0074] Step S4.4: using a flat wire rolling mill to roll the nickel-titanium orthodontic square wire; the outer surfaces of the two rollers moving relative to each other in the X direction are in contact with the two side surfaces in the width direction of the nickel-titanium orthodontic square wire, and the outer surfaces of the two rollers moving relative to each other in the Y direction are in contact with the two side surfaces in the height direction of the nickel-titanium orthodontic square wire; by screwing in or out the roller pressure knobs in the X direction and / or the Y direction, the pressure of the rollers in the X direction and / or the Y direction is controlled, so that the size of the nickel-titanium orthodontic square wire in the width and height directions is further reduced, and the nickel-titanium orthodontic square wire is extruded in the directions of the four edge arcs, thereby recovering and reducing the gradually increasing radius of the four edge arcs generated by the square die drawing process;
[0075] Step S4.5: After rolling is completed, determine whether the edge radius of the nickel-titanium orthodontic square wire is 90 μm ≤ R ≤ 110 μm. If yes, proceed to step S4.7; if not, proceed to step S4.4;
[0076] Step S4.6: Determine whether the edge radius R of the nickel-titanium orthodontic square wire meets the target edge radius R 目 , the target edge radius R of the nickel-titanium orthodontic square wire 目 is 80±10μm; if it meets the requirements, the target size is 0.014×0.025inch and the target cross-sectional area S is 0.23mm 2 The nickel-titanium orthodontic square wire is prepared; if it does not meet the requirements, proceed to step S4.7;
[0077] Step S4.7: Drawing is performed in a square die with a deformation amount C of 10% in the g+1th drawing pass, where the value range of g is 0<g≤G; and step S4.3 is performed.
[0078] The pressing amount of the roller in the X direction and the Y direction each time is not more than 0.05mm.
[0079] Through step S1, step S2 and step S3, the parameters of nickel-titanium orthodontic square wire in the manufacturing process can be known, wherein the obtained drawing fire deformation B is the critical drawing cold deformation of the nickel-titanium orthodontic square wire in the drawing process, and the drawing pass deformation C is the critical drawing force that the nickel-titanium orthodontic square wire can withstand in each drawing process. The drawing fire deformation B and the drawing pass deformation C can be used to determine the optimal number of drawing dies and drawing force according to the target size of the nickel-titanium orthodontic square wire to the greatest extent.
[0080] Step S4 is to prepare nickel-titanium orthodontic square wire according to the parameters determined in steps S1, S2 and S3 to obtain nickel-titanium orthodontic square wire that conforms to the torque expression. Compared with the torque expression of the existing nickel-titanium orthodontic square wire prepared based on the experience of the staff, the present invention greatly improves the accuracy of the torque expression of the nickel-titanium orthodontic square wire.
[0081] The smaller the edge radius of orthodontic square wire, the better. The smaller the edge radius, the sharper the edge of the orthodontic square wire. Too sharp edges can easily scratch the oral mucosa of the user and the doctor's hands. As the edge radius of the orthodontic square wire increases, the probability of it spinning in the groove of the orthodontic bracket increases, that is, the torque loss of the square wire increases. The torque applied by the doctor on the tooth is consumed by the square wire with a large edge radius, which ultimately leads to ineffective treatment effects.
[0082] As attached Figure 5 As shown, the edge radii of 0.014×0.025 inch nickel-titanium orthodontic square wire are 85μm, 77μm, 82μm, and 77μm respectively.
[0083] Step S5: mirror polishing the nickel-titanium orthodontic square wire; after the nickel-titanium orthodontic square wire of the target size is prepared through steps S1 to S4, since its microstructure is in a cold-drawn or cold-rolled state, it is necessary to perform a subsequent heat treatment process to heat-set the cold-drawn or cold-rolled nickel-titanium orthodontic square wire to an arch shape that matches the ideal dental arch shape; the surface of the nickel-titanium orthodontic square wire will oxidize after heat treatment, so mirror polishing is required to remove the oxide scale on the surface of the nickel-titanium orthodontic square wire.
[0084] Traditional methods for removing oxide scale from the surface of orthodontic square wires include mechanical polishing, electrochemical polishing, chemical corrosion, etc. These process equipments are complex, pollute the environment, and are costly. More importantly, while polishing and removing the oxide scale from the surface of the orthodontic square wire, the edge radius of the orthodontic square wire will be rounded, which increases the edge radius of the orthodontic square wire and reduces the torque expression accuracy of the orthodontic square wire. Therefore, the present invention proposes a mirror polishing method, which can remove the oxide scale from the surface of the orthodontic square wire while avoiding increasing the edge radius of the orthodontic square wire, as shown in the attached Figure 8 As shown; the specific steps are as follows:
[0085] Step S5.1: placing the orthodontic square wire into a placement slot 1 that matches the outer contour of the orthodontic square wire, then applying water-soluble glue to both ends and the middle of the orthodontic square wire, and bonding the orthodontic square wire to the bottom end of the placement slot 1;
[0086] Step S5.2: Using compressed air as a power source, selecting polishing particles with elasticity, using a programmed nozzle 2 to bombard the orthodontic square wire placed inside the placement slot 1 with polishing particles, and using a decompression valve to adjust the speed of the nozzle 2 spraying the polishing particles, so that the nozzle 2 can reciprocate along the contour of the placement slot 1; the polishing particles that collide with the orthodontic square wire are discharged from the leakage hole 3 at the bottom end of the placement slot 1;
[0087] During bombardment, the polishing particles sprayed onto the side wall of the placement groove 1 are reflected to the side of the orthodontic square wire due to their elastic characteristics. In this way, each bombardment can spray onto three sides of the orthodontic square wire, and its hardness is between 0.2 and 0.5 times the hardness of the orthodontic square wire, which will not cause damage to the edge radius of the prepared orthodontic square wire. The polishing particles and the oxide scale of the orthodontic square wire are fully mechanically rubbed to remove the oxide scale and scratches on the surface of the orthodontic square wire.
[0088] Step S5.3: After the spraying is completed, the placement slot 1 bonded with the orthodontic square wire is immersed in water to dissolve the water-soluble glue, so that the orthodontic square wire is separated from the placement slot 1, and the moisture on the surface of the orthodontic square wire and the placement slot 1 is blown dry;
[0089] Step S5.4: Turn the orthodontic square wire over, and perform steps S5.1, S5.2, and S5.3 again to obtain the orthodontic square wire with surface oxide scale and scratches removed.
[0090] Surface roughness R of orthodontic square wire after mirror polishing a No larger than 0.8μm, with bright surface, clean and oil-free, no obvious scratches, no corners, and no burrs.
[0091] The hardness value of the polishing particles is between 0.2 and 0.5 times the hardness value of the orthodontic square wire.
[0092] The computer program controls the movement trajectory of the nozzle 2 so that it reciprocates along the placement slot 1 that matches the outer contour of the orthodontic square wire, thereby ensuring the uniformity and consistency of the mirror polishing process.
[0093] Example 2
[0094] Taking the preparation of TMA orthodontic square wire with a target size of 0.017×0.025 inch as an example, a preparation method for improving the torque expression accuracy of orthodontic square wire is provided. Figure 1 , Attachment Figure 3 , Attachment Figure 6 As shown, the method comprises the following steps:
[0095] Step S1: determining the drawing deformation of the orthodontic wire; setting the drawing deformation to B, that is, when the actual drawing deformation of the orthodontic wire reaches the drawing deformation B, an intermediate annealing is required to eliminate the tissue stress of the orthodontic wire and reduce the hardness of the orthodontic wire; determining the drawing deformation B of the orthodontic wire includes the following steps;
[0096] Step S1.1: Select a TMA orthodontic square wire with a diameter of 1.0 mm, set N square molds with a deformation amount of 10% per pass, and the cross-sectional area of the square mold matches the 1.0 mm TMA orthodontic square wire; that is, the cross-sectional areas of the N square molds are: S1 = 0.9 mm 2 、S2=0.81mm 2 、S3=0.73mm 2 、S4=0.66mm 2 、S5=0.59mm 2 ……;
[0097] Step S1.2: Pass a 1.0 mm TMA orthodontic square wire through N square dies in sequence, and perform cold deformation square wire drawing until the TMA orthodontic square wire is broken in the fourth square die. The sum of the deformation amount from the first square die to the third square die is calculated as the limit fire deformation amount, which is 30%, and the breaking limit fire deformation amount A of the TMA orthodontic square wire is 30%;
[0098] Step S1.3: Set the safety factor to 80%, that is, the drawing deformation B of the TMA orthodontic square wire is A×80%=24%; when the actual drawing deformation of the TMA orthodontic square wire reaches the drawing deformation B, perform an intermediate annealing to eliminate the work hardening generated during the drawing deformation of the TMA orthodontic square wire.
[0099] Step S2: Set the target cross-sectional area of the TMA orthodontic square wire to S = 0.27 mm 2 , that is, the target size of TMA orthodontic square wire is 0.017×0.025 inch, and the deformation amount B of the drawing fire is 24%. According to the deformation amount B of the drawing fire=24%, the initial wire diameter of the TMA orthodontic square wire before drawing is obtained.
[0100]
[0101] Step S3: setting the drawing deformation amount C, and determining the drawing deformation amount C of the TMA orthodontic square wire includes the following steps:
[0102] Step S3.1: Take three groups of 0.017×0.025 inch TMA orthodontic square wires in the as-supplied state for a tensile test, and measure the tensile strengths of the three groups of TMA orthodontic square wires to be 1312.9 MPa, 1285.6 MPa, and 1302.8 MPa, respectively. Take the average value as the tensile strength σ1=1300.4 MPa of the TMA orthodontic square wires in the as-supplied state; take three groups of TMA orthodontic square wires in the solid solution state for a tensile test, and measure the tensile strengths of the three groups of TMA orthodontic square wires to be 946.0 MPa, 955.5 MPa, and 944.5 MPa, respectively. Take the average value as the tensile strength σ2=948.7 MPa of the TMA orthodontic square wires in the solid solution state; obtain the tensile strength σ of the TMA orthodontic square wire; that is, The tensile test for measuring the tensile strength of orthodontic square wire is a prior art and will not be described in detail here.
[0103] Step S3.2: Take 8 square dies, design the deformation C of the 8 square dies to increase in sequence with a constant of 2%, that is, C1 is 2%, C2 is 4%, C3 is 6%, C4 is 8%, C5 is 10%, C6 is 12%, C7 is 14%, C8 is 16%, and design the cross-sectional area S of the 8 square dies to be a constant of 0.02mm 2 Decrease in sequence, that is, S1 is 0.98mm 2 , S2 is 0.96mm 2 , S3 is 0.94mm 2 , S4 is 0.92mm 2 , S5 is 0.90mm 2 , S6 is 0.88mm 2 , S7 is 0.86mm 2 , S8 is 0.84mm 2 ;
[0104] Step S3.3: setting the theoretical pulling force value of the TMA orthodontic square wire when entering the square mold for drawing as F, the theoretical pulling force value F is the product of the cross-sectional area S of the square mold and the tensile strength σ during the drawing process of the TMA orthodontic square wire, that is, F=σ×S;
[0105] The TMA orthodontic square wire with a starting round wire diameter of φ=1.0 mm was first inserted into the first square mold, and the actual tensile force value F1=950N was measured when the wire was inserted into the first square mold. At the same time, according to the cross-sectional area S and tensile strength σ of the first square mold, the theoretical tensile force value F=0.98×1124.6=1102.1N was obtained when the wire was inserted into the first square mold; that is, F1<F;
[0106] Repeat the above steps to measure the actual tensile force value F2 = 1002N when penetrating the second square mold, and obtain the theoretical tensile force value F = 0.96 × 1124.6 = 1079.6N when penetrating the second square mold; that is, F2 < F;
[0107] The actual tensile force value F3 = 1051N when penetrating the third square die is measured, and the theoretical tensile force value F = 0.94 × 1124.6 = 1057.1N when penetrating the third square die is measured; that is, F3 < F;
[0108] The actual tensile force value F4 = 1136 N when penetrating the fourth square die is measured, and the theoretical tensile force value F = 0.92 × 1124.6 = 1034.6 N when penetrating the fourth square die is measured; at this time, F4>F;
[0109] It can be known that when the TMA orthodontic square wire with a diameter of 1.0 mm passes through a square die with a deformation of 8% in the fourth pass, its actual tensile force value F4 is greater than the theoretical tensile force F. Therefore, the drawing deformation of the TMA orthodontic square wire with a size of 0.017×0.025 inch is C=C3=6%.
[0110] Step S4: According to the drawing fire deformation amount B of 24% and the drawing pass deformation amount C of 6% obtained in the above steps S1 to S3, the TMA orthodontic square wire is subjected to drawing-rolling tandem processing, which includes the following steps:
[0111] Step S4.1: Take a TMA round wire with a starting wire diameter of φ = 0.67 mm, and set the target cross-sectional area S of the TMA orthodontic square wire to 0.27 mm 2 , that is, the target size of the square die is 0.017×0.025 inch, and then the number of square dies G is obtained according to the drawing fire deformation B of 24% and the drawing pass deformation C of 6%, that is, the number of square dies is the ceiling rounding function;
[0112] Step S4.2: Drawing is performed in a square die with a deformation amount C in the g-th drawing pass, and the value range of g is 0<g≤G;
[0113] Step S4.3: Determine whether the edge radius R of the TMA orthodontic square wire is greater than 90 μm. If yes, proceed to step S4.4; if not, proceed to step S4.6;
[0114] Step S4.4: using a flat wire rolling mill to roll the TMA orthodontic square wire; the outer surfaces of the two rollers moving relative to each other in the X direction are in contact with the two side surfaces in the width direction of the TMA orthodontic square wire, and the outer surfaces of the two rollers moving relative to each other in the Y direction are in contact with the two side surfaces in the height direction of the TMA orthodontic square wire; by screwing in or out the roller pressure knobs in the X direction and / or the Y direction, the pressure of the rollers in the X direction and / or the Y direction is controlled, so that the size of the TMA orthodontic square wire in the width and height directions is further reduced, and the TMA orthodontic square wire is extruded in the directions of the four edge arcs, thereby recovering and reducing the gradually increasing radius of the four edge arcs generated by the square die drawing process;
[0115] Step S4.5: After rolling is completed, determine whether the edge radius of the TMA orthodontic square wire is 70 μm ≤ R ≤ 90 μm. If yes, proceed to step S4.7; if not, proceed to step S4.4;
[0116] Step S4.6: Determine whether the edge radius R of the TMA orthodontic square wire meets the target edge radius R 目 , the target edge radius R of the TMA orthodontic square wire 目 If the target size is 60±10μm, the target cross-sectional area S is 0.27mm. 2 The TMA orthodontic square wire preparation is completed; if it does not meet the requirements, proceed to step S4.7;
[0117] Step S4.7: Drawing is performed in a square die with a deformation amount C of 6% in the g+1th drawing pass, where the value range of g is 0<g≤G; and step S4.3 is performed.
[0118] The pressing amount of the roller in the X direction and the Y direction each time is not more than 0.05mm.
[0119] Through step S1, step S2 and step S3, the parameters of TMA orthodontic square wire in the production process can be known, wherein the obtained drawing fire deformation B is the critical drawing cold deformation of the TMA orthodontic square wire in the drawing process, and the drawing pass deformation C is the critical drawing force that the TMA orthodontic square wire can withstand in each drawing process. The drawing fire deformation B and the drawing pass deformation C can be used to determine the optimal number of drawing dies and drawing force according to the target size of the TMA orthodontic square wire to the greatest extent.
[0120] Step S4 is to prepare TMA orthodontic square wire according to the parameters measured in steps S1, S2 and S3 to obtain TMA orthodontic square wire that conforms to the torque expression. Compared with the torque expression of the existing TMA orthodontic square wire prepared based on the experience of the staff, the present invention greatly improves the accuracy of the torque expression of the TMA orthodontic square wire.
[0121] As attached Figure 6 As shown, the edge radius of 0.017×0.025 inch TMA orthodontic square wire is 43μm, 45μm, 53μm, and 49μm respectively.
[0122] The surface of the TMA orthodontic square wire will also be oxidized after heat treatment and needs mirror polishing to remove the surface oxide scale. The mirror polishing of the TMA orthodontic square wire is the same as step S5 in Example 1, and will not be repeated.
[0123] Example 3
[0124] Taking the preparation of stainless steel orthodontic square wire with a target size of 0.019×0.025 inch as an example, a preparation method for improving the torque expression accuracy of orthodontic square wire is provided. Figure 1 , Attachment Figure 4 , Attachment Figure 7 As shown, the method comprises the following steps:
[0125] Step S1: determining the drawing deformation of the orthodontic wire; setting the drawing deformation to B, that is, when the actual drawing deformation of the orthodontic wire reaches the drawing deformation B, an intermediate annealing is required to eliminate the tissue stress of the orthodontic wire and reduce the hardness of the orthodontic wire; determining the drawing deformation B of the orthodontic wire includes the following steps;
[0126] Step S1.1: Select a stainless steel orthodontic square wire with a diameter of 1.0 mm, set N square molds with a deformation amount of 10% per pass, and the cross-sectional area of the square mold matches the 1.0 mm stainless steel orthodontic square wire; that is, the cross-sectional areas of the N square molds are: S1 = 0.9 mm 2 、S2=0.81mm 2 、S3=0.73mm 2 、S4=0.66mm 2 、S5=0.59mm 2 ……;
[0127] Step S1.2: Pass a 1.0 mm stainless steel orthodontic square wire through N square dies in sequence, and perform cold deformation square wire drawing until the stainless steel orthodontic square wire is broken in the sixth square die. The sum of the deformation amount from the first square die to the fifth square die is calculated as the limit fire deformation amount, which is 50%, and the breaking limit fire deformation amount A of the stainless steel orthodontic square wire is 50%;
[0128] Step S1.3: Set the safety factor to 80%, that is, the drawing deformation B of the stainless steel orthodontic square wire is A×80%=40%; when the actual drawing deformation of the stainless steel orthodontic square wire reaches the drawing deformation B, perform an intermediate annealing to eliminate the work hardening generated during the drawing deformation of the stainless steel orthodontic square wire.
[0129] Step S2: Set the target cross-sectional area of the stainless steel orthodontic square wire to S = 0.31 mm 2 , that is, the target size of the stainless steel orthodontic square wire is 0.019×0.025 inch, and the deformation amount B of the drawing fire is 40%. According to the deformation amount B of the drawing fire=40%, the initial wire diameter of the stainless steel orthodontic square wire before drawing is obtained.
[0130] Step S3: setting the drawing deformation amount C, determining the drawing deformation amount C of the stainless steel orthodontic square wire includes the following steps:
[0131] Step S3.1: Take three groups of 0.019×0.025 inch stainless steel orthodontic square wires in the supply state for tensile test, and measure the tensile strengths of the three groups of stainless steel orthodontic square wires to be 1976.8MPa, 1946.6MPa, and 1963.4MPa, respectively. Take the average value as the tensile strength σ1=1962.9Mpa of the stainless steel orthodontic square wire in the supply state; take three groups of stainless steel orthodontic square wires in the solid solution state for tensile test, and measure the tensile strengths of the three groups of stainless steel orthodontic square wires to be 867.9MPa, 869.1MPa, and 865.8MPa, respectively. Take the average value as the tensile strength σ2=867.6MPa of the stainless steel orthodontic square wire in the solid solution state; obtain the tensile strength σ of the stainless steel orthodontic square wire; that is, The tensile test for measuring the tensile strength of orthodontic square wire is a prior art and will not be described in detail here.
[0132] Step S3.2: Take 8 square dies, design the deformation C of the 8 square dies to increase in sequence with a constant of 2%, that is, C1 is 2%, C2 is 4%, C3 is 6%, C4 is 8%, C5 is 10%, C6 is 12%, C7 is 14%, C8 is 16%, and design the cross-sectional area S of the 8 square dies to be a constant of 0.02mm 2 Decrease in sequence, that is, S1 is 0.98mm 2 , S2 is 0.96mm 2 , S3 is 0.94mm 2 , S4 is 0.92mm 2 , S5 is 0.90mm 2 , S6 is 0.88mm 2 , S7 is 0.86mm 2, S8 is 0.84mm 2 ;
[0133] Step S3.3: setting the theoretical pulling force value of the stainless steel orthodontic square wire when entering the square die for drawing as F, the theoretical pulling force value F is the product of the cross-sectional area S of the square die and the tensile strength σ of the stainless steel orthodontic square wire during drawing, that is, F=σ×S;
[0134] A stainless steel orthodontic square wire with a starting round wire diameter of φ=1.0 mm is first inserted into the first square mold, and the actual tensile force value F1=876N is measured when the wire is inserted into the first square mold. At the same time, according to the cross-sectional area S and tensile strength σ of the first square mold, the theoretical tensile force value F=0.98×1415.3=1387.0N is obtained when the wire is inserted into the first square mold; that is, F1<F;
[0135] Repeat the above steps to measure the actual pulling force value F2 = 992N when penetrating the second square mold, and obtain the theoretical pulling force value F = 0.96 × 1415.3 = 1358.7N when penetrating the second square mold; that is, F2 < F;
[0136] The actual tensile force value when penetrating the third square die is measured to be F3=1048N, and the theoretical tensile force value when penetrating the third square die is F=0.94×1415.3=1330.4N; that is, F3<F;
[0137] The actual tensile force value F4 = 1144 N when penetrating the fourth square die is measured, and the theoretical tensile force value F = 0.92 × 1415.3 = 1302.1 N when penetrating the fourth square die is measured; at this time, F4 < F;
[0138] The actual tensile force value F5 = 1257 N when penetrating the fifth square die is measured, and the theoretical tensile force value F = 0.90 × 1415.3 = 1273.8 N when penetrating the fifth square die is measured; at this time, F5 < F;
[0139] The actual tensile force value F6 when penetrating the sixth square die is measured to be 1341N, and the theoretical tensile force value F when penetrating the sixth square die is measured to be 0.88×1415.3=1245.46N; at this time, F6>F;
[0140] It can be known that when the stainless steel orthodontic square wire with a diameter of 1.0 mm passes through a square die with a deformation of 12% in the sixth pass, its actual tensile force value F6 is greater than the theoretical tensile force F. Therefore, the drawing deformation of the stainless steel orthodontic square wire with a size of 0.019×0.025 inch is C=C5=10%.
[0141] Step S4: According to the drawing fire deformation amount B of 40% and the drawing pass deformation amount C of 10% obtained in the above steps S1 to S3, the stainless steel orthodontic square wire is subjected to drawing-rolling tandem processing, which includes the following steps:
[0142] Step S4.1: Take a stainless steel round wire with a starting wire diameter of φ = 0.81 mm, and set the target cross-sectional area S of the stainless steel orthodontic square wire to 0.31 mm 2 , that is, the target size of the square die is 0.019×0.025 inch, and then the number of square dies G is obtained according to the drawing fire deformation B of 40% and the drawing pass deformation C of 10%, that is, the number of square dies is the ceiling rounding function;
[0143] Step S4.2: Drawing is performed in a square die with a deformation amount C in the g-th drawing pass, and the value range of g is 0<g≤G;
[0144] Step S4.3: Determine whether the edge radius R of the stainless steel orthodontic square wire is greater than 90 μm. If so, proceed to step S4.4; if not, proceed to step S4.6;
[0145] Step S4.4: using a flat wire rolling mill to roll the stainless steel orthodontic square wire; the outer surfaces of the two rollers moving relative to each other in the X direction are in contact with the two side surfaces in the width direction of the stainless steel orthodontic square wire, and the outer surfaces of the two rollers moving relative to each other in the Y direction are in contact with the two side surfaces in the height direction of the stainless steel orthodontic square wire; by screwing in or out the roller pressure knobs in the X direction and / or the Y direction, the pressure of the rollers in the X direction and / or the Y direction is controlled, so that the size of the orthodontic square wire in the width and height directions is further reduced, and the orthodontic square wire is squeezed in the directions of the four edge arcs, thereby recovering and reducing the gradually increasing radius of the four edge arcs generated by the square die drawing process;
[0146] Step S4.5: After rolling is completed, determine whether the edge radius of the stainless steel orthodontic square wire is 70 μm ≤ R ≤ 90 μm. If yes, proceed to step S4.7; if not, proceed to step S4.4;
[0147] Step S4.6: Determine whether the edge radius R of the stainless steel orthodontic square wire meets the target edge radius R 目 , the target edge radius R of the stainless steel orthodontic square wire 目 If the target size is 60±10μm, the target cross-sectional area S is 0.31mm. 2 The stainless steel orthodontic square wire is prepared; if it does not meet the requirements, proceed to step S4.7;
[0148] Step S4.7: Drawing is performed in a square die with a deformation amount C of 6% in the g+1th drawing pass, where the value range of g is 0<g≤G; and step S4.3 is performed.
[0149] The pressing amount of the roller in the X direction and the Y direction each time is not more than 0.05mm.
[0150] Through step S1, step S2 and step S3, the parameters of the stainless steel orthodontic square wire in the manufacturing process can be known, wherein the obtained drawing fire deformation B is the critical drawing cold deformation of the stainless steel orthodontic square wire in the drawing process, and the drawing pass deformation C is the critical drawing force that the stainless steel orthodontic square wire can withstand in each drawing process. The drawing fire deformation B and the drawing pass deformation C can be used to determine the optimal number of drawing dies and drawing force according to the target size of the stainless steel orthodontic square wire to the greatest extent.
[0151] Step S4 is to prepare the stainless steel orthodontic square wire according to the parameters measured in steps S1, S2 and S3, to obtain the stainless steel orthodontic square wire that conforms to the torque expression. Compared with the torque expression of the existing stainless steel orthodontic square wire prepared based on the experience of the staff, the present invention greatly improves the accuracy of the torque expression of the stainless steel orthodontic square wire.
[0152] As attached Figure 7 As shown, the edge radii of 0.019×0.025 inch stainless steel orthodontic square wire are 55μm, 51μm, 52μm, and 58μm respectively.
[0153] The surface of the stainless steel orthodontic square wire will also be oxidized after heat treatment and needs mirror polishing to remove the surface oxide scale. The mirror polishing of the stainless steel orthodontic square wire is the same as step S5 in embodiment 1, and will not be repeated.
[0154] In the description of the present invention, it is necessary to understand that the indicated orientation or positional relationship is based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0155] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A preparation method for improving the torque expression accuracy of orthodontic square wire, characterized in that: The method comprises the following steps: Step S1: determining the deformation amount of the orthodontic square wire after drawing; Step S2: determining the starting round wire diameter of the orthodontic square wire before drawing according to the target cross-sectional area of the orthodontic square wire; Step S3: determining the deformation amount of the orthodontic square wire during each drawing pass; Step S4: performing drawing-rolling tandem processing on the orthodontic square wire according to the deformation amount of the drawing fire and the deformation amount of the drawing pass; Step S5: mirror polishing the orthodontic square wire.
2. A preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 1, characterized in that: The drawing deformation is set to B, that is, when the actual drawing deformation of the orthodontic wire reaches the drawing deformation B, an intermediate annealing is required to eliminate the tissue stress of the orthodontic wire and reduce the hardness of the orthodontic wire. Determining the drawing deformation B of the orthodontic wire includes the following steps: Step S1.1: Select an orthodontic square wire of standard diameter, set N square molds with a deformation amount of 10% per pass, and the cross-sectional area S1 of the first square mold matches the orthodontic square wire of standard diameter; Step S1.2: passing an orthodontic square wire of standard diameter through N square dies in sequence, and performing cold deformation square wire drawing, until the orthodontic square wire is broken in the nth square die, and calculating the sum of the deformation amount from the first square die to the n-1th square die as the limit fire deformation amount A, and obtaining the limit fire deformation amount of the orthodontic square wire to be broken as A; the value range of n is 0<n≤N; Step S1.3: Set the safety factor to 80%, that is, the drawing deformation B of the orthodontic square wire is A×80%; when the actual drawing deformation of the orthodontic square wire reaches the drawing deformation B, perform an intermediate annealing to eliminate the work hardening generated during the drawing deformation of the orthodontic square wire.
3. A preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 2, characterized in that: Set the target cross-sectional area of the orthodontic square wire as S, and obtain the initial wire diameter of the orthodontic square wire before drawing according to the deformation amount B of the drawing fire.
4. A preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 3, characterized in that: The drawing deformation amount is set as C, and determining the drawing deformation amount C of the orthodontic square wire includes the following steps: Step S3.1: Take the orthodontic square wire in the as-supplied state and perform a tensile test to measure the tensile strength σ1 of the orthodontic square wire; take the orthodontic square wire in the solid solution state and perform a tensile test to measure the tensile strength σ2 of the orthodontic square wire; obtain the tensile strength σ of the orthodontic square wire; that is, Step S3.2: Take M square dies, design the pass deformation C of the M square dies to increase in sequence with a constant t, and design the cross-sectional areas S of the M square dies to decrease in sequence with a constant z; Step S3.3: Set the theoretical tensile force value F when the orthodontic square wire enters the square mold for drawing. The theoretical tensile force value F is the product of the cross-sectional area S of the square mold and the tensile strength σ during the orthodontic square wire drawing process, that is, F = σ × S; insert the orthodontic square wire with a starting round wire diameter of φ into M square molds, and measure the actual tensile force value F when entering the mth square mold. m , and at the same time, the theoretical tensile force value F when penetrating the m-th square mold is obtained according to the cross-sectional area S and the tensile strength σ of the m-th square mold; the value range of m is 0<m≤M; Step S3.4: Determine the actual pulling force value F x Is it greater than the theoretical tensile force F? x ≤F, continue to insert and draw the m+1th square die; if F x >F, the drawing pass deformation C can be obtained as C m-1 .
5. A preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 4, characterized in that: The drawing-rolling tandem processing of orthodontic square wire according to the drawing fire deformation amount and the drawing pass deformation amount comprises the following steps: Step S4.1: Take a round wire with a starting wire diameter of φ, and set the width and height of the square mold according to the target cross-sectional area S of the orthodontic square wire. Then, the number G of the square molds is obtained according to the drawing fire deformation B and the drawing pass deformation C, that is, the number of square molds is the ceiling rounding function; Step S4.2: Drawing is performed in a square die with a deformation amount C in the g-th drawing pass, and the value range of g is 0<g≤G; Step S4.3: Determine whether the edge radius R of the nickel-titanium orthodontic square wire is greater than 110 μm, determine whether the edge radius R of the TMA orthodontic square wire is greater than 90 μm, and determine whether the edge radius R of the stainless steel orthodontic square wire is greater than 90 μm. If so, proceed to step S4.4; if not, proceed to step S4.6; Step S4.4: using a flat wire rolling mill to roll the orthodontic square wire; the outer surfaces of the two rollers moving relative to each other in the X direction are in contact with the two side surfaces in the width direction of the orthodontic square wire, and the outer surfaces of the two rollers moving relative to each other in the Y direction are in contact with the two side surfaces in the height direction of the orthodontic square wire; by screwing in or out the roller pressure knobs in the X direction and / or the Y direction, the pressure of the rollers in the X direction and / or the Y direction is controlled, so that the size of the orthodontic square wire in the width and height directions is further reduced, and the orthodontic square wire is squeezed in the directions of the four edge arcs, thereby recovering and reducing the gradually increasing radius of the four edge arcs generated by the square die drawing process; Step S4.5: After rolling is completed, determine whether the edge radius of the nickel-titanium orthodontic square wire is 90μm≤R≤110μm, determine whether the edge radius of the TMA orthodontic square wire is 70μm≤R≤90μm, and determine whether the edge radius of the stainless steel orthodontic square wire is 70μm≤R≤90μm. If so, proceed to step S4.7; if not, proceed to step S4.4; Step S4.6: Determine whether the edge radius R of the orthodontic square wire meets the target edge radius R 目 If the conditions are met, the orthodontic square wire preparation is completed; if not, proceed to step S4.7; Step S4.7: Drawing is performed in a square die with a deformation amount of C in the g+1th drawing pass, where the value range of g is 0<g≤G; and step S4.3 is performed.
6. A preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 5, characterized in that: The pressing amount of the roller in the X direction and the Y direction each time is not more than 0.05mm.
7. A preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 5, characterized in that: The orthodontic square wires include TMA orthodontic square wires, stainless steel orthodontic square wires and nickel-titanium orthodontic square wires; the target edge radius R of the TMA orthodontic square wires 目 The target edge radius R of the stainless steel orthodontic square wire is 60±10μm. 目 The target edge radius R of the nickel-titanium orthodontic square wire is 60±10μm. 目 80±10μm.
8. A method for improving the torque expression accuracy of orthodontic square wire according to claim 5, characterized in that: The mirror polishing of the orthodontic square wire comprises the following steps: Step S5.1: placing the orthodontic square wire into a placement slot (1) matching the outer contour of the orthodontic square wire, then applying water-soluble glue to both ends and the middle of the orthodontic square wire, and bonding the orthodontic square wire to the bottom end of the placement slot (1); Step S5.2: using compressed air as a power source, selecting polishing particles with elasticity, and using a programmed nozzle (2) to bombard the orthodontic square wire placed inside the placement groove (1) with polishing particles, while using a decompression valve to adjust the speed of the nozzle (2) spraying the polishing particles so that the nozzle (2) can reciprocate along the contour of the placement groove (1); the polishing particles that collide with the orthodontic square wire are discharged from the leakage hole (3) at the bottom end of the placement groove (1); Step S5.3: After the spraying is completed, the placement slot (1) bonded with the orthodontic square wire is immersed in water to dissolve the water-soluble glue, so that the orthodontic square wire is separated from the placement slot (1), and the moisture on the surface of the orthodontic square wire and the placement slot (1) is blown dry; Step S5.4: Flip the orthodontic square wire and perform steps S5.1, S5.2, and S5.3 again; The orthodontic square wire with surface oxide scale and scratches removed is obtained.
9. A method for improving the torque expression accuracy of orthodontic square wire according to claim 8, characterized in that: Surface roughness R of orthodontic square wire after mirror polishing a Not more than 0.8μm.
10. A preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 8, characterized in that: The hardness value of the polishing particles is between 0.2 and 0.5 times the hardness value of orthodontic square wire.
Citation Information
Patent Citations
Parallel wire roller pulling combined forming technology and production equipment thereof
CN103128127A
Preparation method of beta-type titanium alloy dental arch wire
CN116329306A
Film removal method of rectangular wire
JP2023041414A
Hybrid orthodontic archwire
US20070172788A1