Weldment with preset gold-tin connecting layer and preparation method and application of weldment

In the preparation of the Au80Sn20 gold-tin connection layer, the gold-tin layer is deposited layer by layer using a specifically set mask template and annealed. This solves the problems of material brittleness and composition uniformity, and achieves an efficient and low-cost gold-tin connection layer. preparation, improving product quality and production efficiency.

CN118848147AActive Publication Date: 2024-10-29SOLDERWELL MICROELECTRONIC PACKAGING MATERIALS CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411180874.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-10-29
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

When preparing the Au80Sn20 gold-tin connection layer in the existing technology, the brittleness of the material makes it difficult to prepare the thin layer, the processing cost is high, and the uniformity and proportion of the ingredients are difficult to control, which affects product quality and mass production.

Method used

A specially set mask is used as a template to deposit gold and tin layers layer by layer. The gold and tin layers are diffused through annealing treatment to form a gold-tin connection layer with high composition uniformity to ensure an accurate composition ratio.

Benefits of technology

It achieves high composition uniformity and high composition ratio matching of the gold-tin connecting layer, reduces production costs, and improves product use effects and production cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005012116140000011
    Figure HDA0005012116140000011
  • Figure HDA0005012116140000012
    Figure HDA0005012116140000012
  • Figure HDA0005012116140000021
    Figure HDA0005012116140000021
Patent Text Reader

Abstract

The invention discloses a welding part with a preset gold-tin connecting layer and a preparation method and application thereof, and belongs to the technical field of soft soldering, the preparation method of the welding part takes a specifically arranged mask as a template to carry out special deposition of a gold layer and a tin layer, the diffusion effect of the gold layer and the tin layer is good when an obtained composite deposition layer is subjected to annealing treatment, and the performance of the composite deposition layer is improved. The formed gold-tin connecting layer is high in component uniformity, and the matching degree of the component proportion of gold and tin and an expected result is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of soft soldering, and in particular to a soldering part with a pre-set gold-tin connection layer, a preparation method and an application thereof. Background Art

[0002] Gold-based Au80Sn20 material has the characteristics of high yield strength, excellent fatigue resistance, good wettability, strong corrosion resistance, good electrical conductivity / thermal properties, and its brazing temperature is moderate. Therefore, it is widely used as a soft soldering connection layer material in aerospace, automobile, communication and other fields.

[0003] At present, the methods for forming a pre-set Au80Sn20 material connection layer mainly include the following two methods: the first method is to directly roll the ready-made Au80Sn20 material into a foil, and then braze it on the weldment. This method is simple to operate, but due to the high brittleness of the Au80Sn20 material, the foil rolling can generally only be maintained at more than 10μm, and a thinner gold-tin connection layer cannot be prepared. The processing cost is high and the material utilization rate is low. At the same time, the foil obtained by rolling is extremely easy to oxidize during the subsequent hot rolling process, affecting the product quality. The second method is to alternately electroplate gold and tin layers on the entire surface to be welded until the required thickness is achieved. Compared with the first method, the size controllability and material utilization rate are high, but the composite coating obtained by this process has low mutual diffusion uniformity of gold and tin during brazing, making it difficult to obtain a gold-tin connection layer with uniform composition and accurate element ratio. In addition, there is also existing technology that uses electroplating to simultaneously electroplate gold and tin to obtain a gold-tin connection layer in one step, but the composition uniformity and component ratio accuracy of the product are still difficult to meet expectations, and there are too many interference factors in the process, making it difficult to carry out mass production in a factory. Summary of the Invention

[0004] Based on the defects of the existing technology, the purpose of the present invention is to provide a method for preparing a welding part with a pre-set gold-tin connection layer. This method uses a specifically set mask as a template to perform special deposition of gold and tin layers. The resulting composite deposited layer has good diffusion effects of the gold and tin layers when annealed, the formed gold-tin connection layer has high component uniformity, and the composition ratio of gold and tin is highly matched with the expected result.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for preparing a soldering part with a pre-set gold-tin connection layer comprises the following steps:

[0007] (1) depositing a first gold layer on the welding surface substrate; the thickness of the first gold layer is ≤ 0.2 μm;

[0008] (2) Covering the first gold layer with a first mask, wherein the first mask is provided with a plurality of hollow circular holes distributed in a grid, wherein the area of ​​the hollow circular holes on the first mask accounts for 48-52%; the area of ​​a single hollow circular hole in the first mask is ≤0.05mm 2 ;

[0009] (3) depositing a first tin layer in the hollow circular hole area of ​​the first mask, wherein the thickness ratio of the first tin layer to the first gold layer is (3.8-4.2):1;

[0010] (4) removing the first mask, then covering the first tin layer with a second mask and depositing a second gold layer in an area not covered by the second mask, wherein the thickness of the second gold layer is the same as the thickness of the first tin layer;

[0011] (5) removing the second mask, and then depositing a third gold layer on the plane of the first tin layer and the second gold layer; the thickness of the third gold layer is the same as the thickness of the first gold layer;

[0012] (6) covering the third gold layer with a first mask, and depositing a fourth gold layer in the hollow circular hole area of ​​the first mask, wherein the thickness of the fourth gold layer is the same as the thickness of the first tin layer;

[0013] (7) removing the first mask, then covering the fourth gold layer with a second mask and depositing a second tin layer in an area not covered by the second mask, wherein the thickness of the second tin layer is the same as the thickness of the fourth gold layer;

[0014] (8) removing the second mask, and then repeating steps (1) to (7) until the obtained composite deposition layer reaches a predetermined thickness, and after annealing, obtaining the soldering part with the preset gold-tin connection layer; the temperature during the annealing treatment is 200 to 220°C.

[0015] Existing pre-set gold-tin connection layers are generally obtained by directly rolling the existing gold-tin material Au80Sn20 into foils and then brazing them, or by using an alternating deposition method to form a composite gold-tin layer, which is then annealed to allow the layers to diffuse into each other to obtain a gold-tin connection layer. However, the former is limited by the brittleness of the Au80Sn20 material and cannot produce thinner products. At the same time, the process has low material utilization, and the rolled foil needs to be further hot-rolled, which makes it easy to oxidize, affecting product quality. Although the latter can produce products of various thicknesses and sizes, the composition of such products is uneven and the element ratio is difficult to accurately control. To this end, in the technical solution of the present invention, the inventors have developed a welding part with a pre-set gold-tin connection layer. When preparing this product, a first gold layer is first set as the bottom layer, and then a first mask with hollow circular holes distributed in a grid is used as a deposition template to cover the first gold layer, and a first tin layer of a specific thickness is deposited in the exposed area corresponding to the hollow circular hole. After the deposition of the tin layer is completed, the second mask is used to completely cover each cylindrical tin layer, and then the second gold layer is deposited on the first gold layer not covered by the mask, and the thickness of the second gold layer is limited to the same as that of the first tin layer, so that the second gold layer can evenly wrap the tin layer and form a flat composite layer; then, similar to the above steps, after a gold layer is deposited on the composite layer, the first and second masks are used to construct another composite layer with the same structure but the positions of the gold layer and the tin layer are interchanged, and finally a complete composite deposition layer is formed. The composite deposited layer can be repeatedly set according to actual needs to adjust the thickness of the resulting welded part, overcoming the limitation of traditional processes for manufacturing products, which cannot widely adjust the thickness of the product due to process or material limitations. During the annealing treatment of the composite deposited layer obtained by the present invention, the first gold layer and the tin layer in the multiple composite layers can diffuse between the upper and lower layers. At the same time, the tin layer and the second gold layer can also diffuse between each other within the same composite layer plane. Therefore, the overall welded part has a high composition uniformity after the gold-tin connecting layer is formed. Based on the specific restrictions on the interlayer thickness and the area ratio of the mask hollow hole, the formed gold-tin connecting layer can achieve a relatively precise Au80Sn20 composition ratio, and the product has excellent performance.

[0016] In addition, the inventors have discovered through experiments that, in terms of diffusion efficiency and diffusion uniformity, during the deposition process of the tin layer described in the present invention, if the hollow structure in the first mask used is not a limited circular hole shape, it may cause the formed tin layer or gold layer to be unable to achieve uniform diffusion during annealing, and the composition uniformity of the gold-tin connection layer may not be as expected.

[0017] Preferably, the area of ​​a single hollow circular hole in the first mask is 0.01 to 0.05 mm 2 .

[0018] More preferably, the area of ​​a single hollow circular hole in the first mask is 0.01 mm 2 , 0.015mm 2, 0.02mm 2 , 0.03mm 2 , 0.04mm 2 , 0.05mm 2 The range of values ​​for one or both of .

[0019] The size of the hollow circular hole determines the size of the deposited cylindrical tin layer. If the area is too large, the size of the prepared tin layer will be too large, which will cause the gold layer and the tin layer to diffuse too far from each other in the same plane, resulting in poor diffusion effect within the plane. However, if the area of ​​the hollow circular hole is too small, the mask processing difficulty will increase and the production cost will increase. Therefore, when the area of ​​the hollow circular hole is preferably within the above range, the overall product preparation difficulty and cost are low, and the prepared product quality is better.

[0020] Preferably, the thickness of the first gold layer and the third gold layer is 0.15-0.2 μm.

[0021] More preferably, the thickness of the first gold layer and the third gold layer is in the range of one or any two of 0.15 μm, 0.16 μm, 0.17 μm, 0.18 μm, 0.19 μm, and 0.2 μm.

[0022] The thickness of the first gold layer and the third gold layer is related to the thickness of the tin layer and the formed composite layer. If the thickness of the first gold layer and the third gold layer increases, the thickness of the composite layer also increases, the diffusion distance between the upper and lower layers of the gold layer and the tin layer increases, and the diffusion uniformity between the layers is reduced. However, if the thickness of the first gold layer and the third gold layer is too thin, it may result in the composite layer being too thin, and multiple deposition steps need to be repeated to reach the expected thickness, which increases the number of processing steps and the production cost. When the thickness of the first gold layer and the third gold layer is preferably within the above range, the production difficulty, production cost and product quality of the product can be taken into account, and the product production cost-effectiveness is higher.

[0023] Preferably, the first mask and the second mask are PET masks.

[0024] PET has good air tightness and mechanical properties, adheres tightly to the metal layer, will not be penetrated during the metal deposition process, and has higher toughness and tensile strength than other polymer materials and good dimensional stability. Therefore, it is more suitable for the production process of the welded parts described in the present invention.

[0025] Preferably, in step (1), the welding surface substrate is further cleaned before depositing the first gold layer, and the cleaning agent used for the cleaning includes at least one of acetone and isopropyl alcohol.

[0026] Preferably, the gold layer and / or tin layer is deposited by electroplating.

[0027] Preferably, the vacuum degree during the annealing treatment is ≤200Pa.

[0028] Preferably, the annealing treatment lasts for 3 to 4 hours.

[0029] The welding part with pre-set gold-tin connection layer described in the present invention is based on a special interlayer structure design. After annealing treatment, the composite deposited layer can accurately reach the gold-tin composition ratio of Au80Sn20 material. At the same time, the composition uniformity of the formed gold-tin connection layer is excellent, so it has excellent use effect.

[0030] During the annealing process, the use of the above-mentioned preferred annealing conditions can not only effectively control the oxidation degree of the metal layer to a lower level during the annealing process, but also ensure the gold-tin diffusion effect of each layer under low energy consumption, and the component uniformity of the product is better.

[0031] Another object of the present invention is to provide a welding part prepared by the method for preparing a welding part with a pre-set gold-tin connection layer, wherein the welding part includes a welding surface base and a gold-tin connection layer.

[0032] Preferably, the mass ratio of gold element to tin element in the gold-tin connection layer formed after the composite deposition layer is annealed is (78:22) to (82:18).

[0033] Another object of the present invention is to provide an application of the welding piece with a pre-set gold-tin connection layer in soft soldering.

[0034] The beneficial effect of the present invention is that the present invention provides a method for preparing a welding part with a pre-set gold-tin connection layer. The method uses a specifically set mask as a template to perform special deposition of the gold layer and the tin layer. The resulting composite deposited layer has good diffusion effects of the gold layer and the tin layer when subjected to annealing treatment. The formed gold-tin connection layer has high component uniformity, and the composition ratio of gold and tin is highly matched with the expected result. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a schematic diagram of the first mask covering the first gold layer during the preparation of the soldering piece with a pre-set gold-tin connection layer according to the present invention.

[0036] Figure 2 This is a schematic diagram of the second mask covering the first tin layer during the preparation of the soldering piece with a pre-set gold-tin connection layer according to the present invention.

[0037] Figure 3 This is a schematic structural diagram of the welding component with a pre-set gold-tin connection layer before annealing treatment according to the present invention.

[0038] Figure 4 This is a schematic diagram of the structure of the welding part with a pre-set gold-tin connection layer after annealing treatment according to the present invention. DETAILED DESCRIPTION

[0039] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples. Its purpose is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise all fall within the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention are all conventional common reagents and instruments unless otherwise specified.

[0040] Example 1

[0041] The present invention provides a welding part with a pre-set gold-tin connection layer, a preparation method thereof, and an embodiment of its application. The preparation method of the welding part includes the following steps:

[0042] (1) A first gold layer is deposited by electroplating on a soldering surface substrate made of an iron-cobalt-nickel alloy after cleaning with acetone and isopropyl alcohol; the diameter of the soldering surface substrate is 8 mm; the thickness of the first gold layer is 0.15 μm; and the electroplating gold process parameters are: a plating bath temperature of 55° C., a current density of 0.4 A / dm 2 , electroplating time 3.5min;

[0043] (2) Covering the first gold layer with a first mask, wherein the first mask is a PET film, such as Figure 1 As shown, the film is provided with a plurality of hollow circular holes in a grid distribution, and the area of ​​a single hollow circular hole is 0.01mm 2 , the area of ​​the hollow circular hole on the first mask accounts for 50%;

[0044] (3) Electroplating is used to deposit a plurality of cylindrical first tin layers in the hollow circular hole area of ​​the first mask, wherein the thickness of the first tin layer is 0.6 μm; the electroplating tin process parameters are: bath temperature 50° C., current density 1.5 A / dm 2 , electroplating time 12min;

[0045] (4) removing the first mask, then covering the first tin layer with a second mask and depositing a second gold layer in the area not covered by the second mask, as shown in FIG. Figure 2 As shown, the thickness of the second gold layer is the same as the thickness of the first tin layer; the second mask is a PET film;

[0046] (5) removing the second mask, and then depositing a third gold layer on the plane of the first tin layer and the second gold layer; the thickness of the third gold layer is the same as the thickness of the first gold layer;

[0047] (6) covering the third gold layer with a first mask, and depositing a fourth gold layer in the hollow circular hole area of ​​the first mask, wherein the thickness of the fourth gold layer is the same as the thickness of the first tin layer;

[0048] (7) removing the first mask, then covering the fourth gold layer with a second mask and depositing a second tin layer in an area not covered by the second mask, wherein the thickness of the second tin layer is the same as the thickness of the fourth gold layer;

[0049] (8) Remove the second mask, and then repeat steps (1) to (7) until the resulting composite deposition layer reaches a predetermined thickness of about 10 μm. Figure 3 After annealing, the soldering part with the preset gold-tin connection layer is obtained, as shown in FIG. Figure 4 As shown;

[0050] The vacuum degree during the annealing treatment is 200 Pa, the temperature is 220° C., and the time is 3.5 h.

[0051] Example 2

[0052] The embodiment of the soldering part with a pre-set gold-tin connection layer, its preparation method, and application described in the present invention differs from Example 1 only in that the thickness of the first gold layer is 0.2 μm, and the thickness of the first tin layer is 0.8 μm.

[0053] Example 3

[0054] The embodiment of the soldering part with a pre-set gold-tin connection layer, its preparation method, and application described in the present invention differs from Example 1 only in that the thickness of the first gold layer is 0.18 μm, and the thickness of the first tin layer is 0.72 μm.

[0055] Example 4

[0056] The embodiment of the present invention, a welding part with a pre-set gold-tin connection layer, a preparation method thereof, and an application thereof, differs from embodiment 1 only in that the area of ​​the single hollow circular hole on the first mask is 0.05mm 2 .

[0057] Example 5

[0058] The embodiment of the present invention, a welding part with a pre-set gold-tin connection layer, a preparation method thereof, and an application thereof, differs from embodiment 1 only in that the area of ​​the single hollow circular hole on the first mask is 0.03 mm 2 .

[0059] Example 6

[0060] The embodiment of the soldering part with a pre-set gold-tin connection layer, the preparation method thereof, and the application thereof described in the present invention is different from Example 1 only in that the temperature during the annealing treatment is 210°C.

[0061] Example 7

[0062] The embodiment of the soldering part with a pre-set gold-tin connection layer, the preparation method thereof, and the application thereof described in the present invention is different from Example 1 only in that the temperature during the annealing treatment is 200°C.

[0063] Comparative Example 1

[0064] A welding part with a pre-set gold-tin connection layer, a preparation method thereof, and an application thereof, which differ from Example 1 only in that the thickness of the first gold layer is 0.3 μm, and the thickness of the first tin layer is 1.2 μm.

[0065] Comparative Example 2

[0066] A welding part with a pre-set gold-tin connection layer, a preparation method thereof, and an application thereof, the difference from Example 1 is that the area of ​​a single hollow circular hole on the first mask is 0.1mm 2 .

[0067] Comparative Example 3

[0068] A welding part with a pre-set gold-tin connection layer, a preparation method thereof, and an application thereof, which differ from Example 1 only in that the hollow circular holes on the first mask are replaced with hollow square holes of 0.1 mm×0.1 mm.

[0069] Comparative Example 4

[0070] A soldering part with a pre-set gold-tin connection layer, a preparation method thereof, and an application thereof, the difference from Example 1 being that the temperature during the annealing treatment is 150°C.

[0071] Comparative Example 5

[0072] A soldering part with a pre-set gold-tin connection layer, a preparation method thereof, and an application thereof, the difference from Example 1 being that the preparation method comprises the following steps:

[0073] (1) depositing a gold layer by electroplating on a soldering surface substrate made of an iron-cobalt-nickel alloy after cleaning with acetone and isopropyl alcohol; the thickness of the gold layer is 0.15 μm;

[0074] (2) A tin layer is deposited on the gold layer by electroplating. The thickness of the tin layer is the same as that of the gold layer. The electroplating time is 3 minutes.

[0075] (3) repeating steps (1) to (2) until the obtained composite deposition layer reaches a predetermined thickness of about 10 μm, and after annealing, the soldering part with the pre-set gold-tin connection layer is obtained;

[0076] The vacuum degree during the annealing treatment is 200 Pa, the temperature is 220° C., and the time is 3.5 h.

[0077] Effect example

[0078] In order to verify the composition and composition uniformity of the welded parts described in the present invention, the following steps are used to test the products of each embodiment and comparative example:

[0079] The gold-tin connection layer of each embodiment and comparative example product is divided into four equal parts in a "field" shape, and the EDS energy spectrometer is used to detect the composition of the center position of the gold-tin connection layer and the center position in each of the four equal parts (that is, the composition of 5 points is detected in total). Since the connection layer only contains two elements, gold and tin, it is only necessary to detect the mass content of tin element. Then, the average value and standard deviation of the mass content of tin element at 5 points are taken. The closer the average value of the mass content of tin element is to 20%, and the smaller the standard deviation, the closer the composition of the gold-tin connection layer is to the target value, and the smaller the composition fluctuation, that is, the better the quality of the gold-tin connection layer.

[0080] The test results are shown in Table 1.

[0081] Table 1 Test results

[0082] project Average tin content (mass fraction, %) Standard deviation Example 1 20.18 0.271 Example 2 20.28 0.529 Example 3 20.26 0.493 Example 4 20.39 0.618 Example 5 20.32 0.575 Example 6 20.48 0.632 Example 7 20.53 0.658 Comparative Example 1 20.73 1.029 Comparative Example 2 20.66 0.710 Comparative Example 3 20.52 0.677 Comparative Example 4 20.86 1.039 Comparative Example 5 20.98 1.869

[0083] It can be seen from the test results that in the welded parts with the pre-set gold-tin connection layer described in the present invention, the gold and tin components of the gold-tin connection layer are close to the ratio of 80:20, which fully meets the expected design of the Au80Sn20 material. At the same time, the product has high composition uniformity, and the test standard deviation is basically maintained within 0.66, and the lowest is only 0.271.

[0084] In contrast, in the process of preparing the products of Comparative Examples 1-3, the appropriate interlayer thickness and the size and shape of the hollow structure of the mask grid distribution were not selected, resulting in uneven interlayer diffusion during the annealing process of the deposited composite deposition layer, and the product had poor composition uniformity; the annealing temperature of the product of Comparative Example 4 was insufficient, and the diffusion degree of the gold layer and the tin layer was insufficient, and the same effect could not be achieved. Comparative Example 5 belongs to the existing formation process of the gold-tin connection layer. It forms a composite deposition layer by alternately depositing gold layers and tin layers with no special structure on the plane. The final product not only has poor composition uniformity, but also the composition ratio is difficult to achieve the expected result.

[0085] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those of ordinary skill in the art should understand that the technical solutions of the present invention can be modified or equivalently replaced without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A method for preparing a welding part with a pre-set gold-tin connection layer, characterized in that: The following steps are involved: (1) depositing a first gold layer on the welding surface substrate; the thickness of the first gold layer is ≤ 0.2 μm; (2) A first mask is covered on the first gold layer, wherein the first mask is provided with a plurality of hollow circular holes distributed in a grid, and the area of ​​the hollow circular holes on the first mask accounts for 48-52%; the area of ​​a single hollow circular hole in the first mask is ≤0.05mm 2 ; (3) depositing a first tin layer in the hollow circular hole area of ​​the first mask, wherein the thickness ratio of the first tin layer to the first gold layer is (3.8-4.2):1; (4) removing the first mask, then covering the first tin layer with a second mask and depositing a second gold layer in an area not covered by the second mask, wherein the thickness of the second gold layer is the same as the thickness of the first tin layer; (5) removing the second mask, and then depositing a third gold layer on the plane of the first tin layer and the second gold layer; the thickness of the third gold layer is the same as the thickness of the first gold layer; (6) covering the third gold layer with a first mask, and depositing a fourth gold layer in the hollow circular hole area of ​​the first mask, wherein the thickness of the fourth gold layer is the same as the thickness of the first tin layer; (7) removing the first mask, and then covering the fourth gold layer with a second mask and depositing a second tin layer in an area not covered by the second mask, wherein the thickness of the second tin layer is the same as the thickness of the fourth gold layer; (8) removing the second mask, and then repeating steps (1) to (7) until the obtained composite deposition layer reaches a predetermined thickness, and after annealing, obtaining the welding part with the preset gold-tin connection layer; the temperature during the annealing is 200 to 220°C.

2. The method for preparing a welding part with a pre-set gold-tin connection layer as claimed in claim 1, characterized in that: The area of ​​a single hollow circular hole in the first mask is 0.01-0.05 mm 2 .

3. The method for preparing a welding part with a pre-set gold-tin connection layer as claimed in claim 1, characterized in that: The thickness of the first gold layer and the third gold layer is 0.15-0.2 μm.

4. The method for preparing a welding part with a pre-set gold-tin connection layer as claimed in claim 1, characterized in that: The first mask and the second mask are PET masks.

5. The method for preparing a welding part with a pre-set gold-tin connection layer as claimed in claim 1, characterized in that: In the step (1), the welding surface substrate is also cleaned before the first gold layer is deposited, and the cleaning agent used in the cleaning process includes at least one of acetone and isopropyl alcohol.

6. The method for preparing a welding part with a pre-set gold-tin connection layer as claimed in claim 1, characterized in that: The vacuum degree during the annealing treatment is ≤200Pa.

7. A welded part prepared by the method for preparing a welded part with a pre-set gold-tin connection layer according to any one of claims 1 to 6.

8. The weldment according to claim 7, characterized in that: The welding piece includes a welding surface base and a gold-tin connection layer.

9. The weldment according to claim 8, characterized in that: The mass ratio of gold element to tin element in the gold-tin connection layer is (78:22) to (82:18).

10. Use of the weldment according to any one of claims 7 to 9 in soft soldering.

Citation Information

Patent Citations

  • Lid or case for sealing package and method for manufacturing the lid or the case

    CN101558488A

  • Method for coating copper electrode of silicon heterojunction solar cell

    CN110797439A

  • Gold-tin alloy film preparation method

    CN111876728A

  • Gold-tin alloy heat sink film and preparation method thereof, heat sink substrate and LED device

    CN112779501A

  • Metal plate, deposition mask, and manufacturing method therefor

    CN113622004A