Method for preparing three-dimensional porous carbon nanoelectrode material based on chromium-containing scrap leather slag
By using boron-chromium-nitrogen co-doped carbon nanomaterials based on tannery solid waste and bayberry tannin modified in fuel cells, the degradation problem of platinum-based catalysts in high potential and strong acid environments was solved, and efficient and stable Oxygen reduction catalyst, better than commercial Pt/C catalyst.
Patent Information
- Application Number
- CN202410553455.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-05-07
AI Technical Summary
Platinum-based catalysts in existing fuel cells are expensive and prone to corrosion, leading to degradation in high potential and strong acid environments, affecting the activity and stability of the electrocatalyst, limiting the application of fuel cells.
A boron-chromium-nitrogen co-doped carbon nanometer three-dimensional fuel cell anode material was prepared based on the modification of chromium-containing waste skin residue and bayberry tannins from solid waste in the tanning industry. A high-performance oxygen reduction catalyst was formed through specific synthesis steps.
It achieves high potential and good ultimate current density, and significantly improves the stability of the catalyst, which is better than commercial Pt/C catalyst and reduces the preparation cost.
Smart Images

Figure CN118851158A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of proton membrane fuel cell catalysts, and specifically to a method for preparing a boron-chromium-nitrogen co-doped carbon nano three-dimensional fuel cell negative electrode material based on the use of chromium-containing waste leather residue from the leather industry as a carbon source precursor through modification with bayberry tannin extract. Background Art
[0002] At present, the reserves of fossil fuels are constantly depleting, and their large-scale use has seriously polluted the environment. Therefore, the development of clean, cheap and sustainable energy conversion and energy storage systems is the main direction of current research. Fuel cells use chemical reactions to directly convert the energy released by the reaction of fuel and oxygen into electrical energy. They are not limited by the Carnot cycle and can achieve efficient energy conversion. The ORR reaction at the cathode of the fuel cell is an important factor in determining the overall performance of the battery. Although platinum-based catalysts have shown excellent catalytic performance in the ORR reaction, their commercial application in the actual application of fuel cells is limited due to their high price and susceptibility to corrosion, deactivation and other factors. In addition, Pt / C catalysts are prone to degradation under harsh environments such as high potential and strong acidity, resulting in decreased activity and stability of the electrocatalyst, which in turn affects the overall performance and life of the fuel cell. To this end, researchers are actively looking for alternative platinum-based materials, such as non-precious metal catalysts, single-atom catalysts, alloy catalysts, etc., to solve the problems of platinum-based materials and obtain more stable and efficient fuel cell catalysts.
[0003] Single atom catalysts (SACs) have great potential in the field of ORR electrocatalysts. They have a fine MNC structure (M = iron, cobalt, nickel, etc.). The SAC structure can effectively reduce the coordination number of the metal center, avoid the binding effect formed by multiple metal atoms, and increase the contact rate between the reactants and metal ions, thereby improving the catalytic activity; at the same time, SAC can also achieve high atomic utilization and provide high catalytic activity and selectivity. The carrier of the transition metal-nitrogen-carbon-based material is a carbon-based material. After processing, an excellent mesoporous structure can be obtained, and it has the advantages of large specific surface area and strong methanol resistance. In addition, nitrogen doping can improve the overall conductivity of the material. Therefore, the transition metal-nitrogen-carbon-based material has great potential in the direction of fuel cell cathode catalysts. In order to further improve the catalytic activity of carbon-based electrocatalysts, it is often necessary to artificially introduce heteroatoms such as N, F, B, S, and P. Among them, N and B co-doping can simultaneously utilize the positive charge polarization effect of the N element and the negative charge polarization effect of the B element, and produce a synergistic effect when forming the NCB structure, significantly improving the catalytic activity of the active carbon site. However, the co-doping system is complex, and it is more difficult to synthesize carbon materials with a certain doping configuration in a targeted manner.
[0004] Tannin extract is a common biomass material containing aromatic rings in nature. Gelatin obtained from the hydrolysis of chromium-containing waste skin residue is used as a biomass precursor and the boron element chelated and modified by bayberry tannin extract is used as the main graphite phase carbon source to prepare a fuel cell negative electrode material with chromium and boron dual active sites. On the one hand, the effective coordination and chelation of boron element and bayberry tannin extract increases the abundant active sites for the catalytic reaction. On the other hand, the aromatic ring structure of bayberry tannin extract can further increase the content of graphite phase of the synthesized metal carbon-based material during the pyrolysis process, thereby hoping to obtain a higher performance ORR catalyst.
[0005] Chromium-containing waste leather residue is the main component of leather solid waste, and its surface contains rich functional groups. Its hydrolysis product, chromium-containing gelatin, is a natural polymer material with good conductivity, rich in various polar functional groups such as amino and hydroxyl groups, and rich heteroatoms. It has a natural hierarchical fibrous structure and can be used as an organic ligand of metal catalysts to construct a one-dimensional carbon-based electrocatalyst with a certain hierarchical porous structure and realize the natural doping of N. Therefore, in this study, gelatin obtained by hydrolysis of chromium-containing waste leather residue and boron chelated by bayberry tannin were compounded in a certain proportion, and a high-performance and low-cost metal polyphenol-modified boron-chromium-nitrogen co-doped carbon-based oxygen reduction fuel cell cathode material was prepared by pyrolysis. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a boron-chromium-nitrogen co-doped three-dimensional carbon nanofuel cell negative electrode material based on chromium-containing waste leather residue from the leather industry as a carbon source precursor through modification of bayberry tannin extract, so as to solve the problems raised in the above background technology.
[0007] To achieve the above object, the present invention provides the following technical solution, and the specific steps are as follows:
[0008] Step 1: Weigh a certain amount of chromium-containing waste leather residue, prepare a certain amount of sodium hydroxide and sodium chloride solution and mix them together, dissolve the chromium-containing waste leather residue in the mixed solution, and then stir it on a magnetic stirrer to form a chromium-containing gelatin solution, then filter and precipitate the impurities, and then neutralize it with acid to a pH between 6-8. Finally, freeze it in a refrigerator, and then put it in a freeze dryer to dry for 24 hours to obtain a chromium-containing gelatin solid;
[0009] Step 2: Weigh a certain amount of bayberry tannin extract, dissolve it in deionized water, and perform magnetic stirring after ultrasonic treatment to obtain a bayberry tannin extract solution.
[0010] Step 3: Weigh a certain amount of boric acid and dissolve it in deionized water, stir to form a uniform boric acid solution, and pour the chromium-containing gelatin prepared in step 1 into the boric acid solution;
[0011] Step 4: Pour the bayberry tannin extract solution in step 2 into the mixed solution in step 3, and then place it on a magnetic stirrer for full stirring to evaporate the water;
[0012] Step 5: Wash the product of step 4 with deionized water and anhydrous ethanol 2 to 3 times, filter and dry the product in an oven to obtain C@CrB-BT-N;
[0013] Step 6: Place the dried precursor product in a tubular furnace in a nitrogen atmosphere for high-temperature pyrolysis, and cool naturally to room temperature.
[0014] Step 7: Reflux the calcined sample in boiling water, then wash and dry the sample to obtain a fuel cell cathode material.
[0015] As a preferred embodiment, in step one, the amount of chromium-containing waste leather residue and the mixed solution is 1g / 50ml; the mixed solution is prepared by mixing 0.1mol / l sodium hydroxide and 2mol / l sodium chloride solution in a certain volume ratio, the temperature of the magnetic stirrer is 60 degrees Celsius, the speed is 700rpm, the time is 7h, the refrigerator freezing time is 12h, and the freeze dryer temperature is -78°C for 24h.
[0016] As a preferred embodiment, in step 2, the concentration of the prepared bayberry tannin extract solution is 0.05 g / mol.
[0017] As a preferred solution, in step three, the concentration of the boric acid solution is 1.5 mol / l, and the required amount is 200 ml.
[0018] As a preferred embodiment, in step 4, the temperature of the magnetic stirrer is 80° C. and the stirring time is 24 h.
[0019] As a preferred solution, in step five, the oven drying temperature is 60° C. and the time is 18 hours.
[0020] As a preferred solution, in step six, the specific operation of high-temperature pyrolysis is: in a pure nitrogen atmosphere, the temperature is increased to 400°C at a heating rate of 5°C / min and stabilized for 30 minutes, then the temperature is increased to 800°C at a heating rate of 5°C / min and maintained for 2 hours, and finally cooled to room temperature with the furnace.
[0021] As a preferred embodiment, in step seven, the reflux time in boiling water is 2 hours.
[0022] Compared with commercial Pt / C catalysts, the boron-nitrogen co-doped carbon-based oxygen reduction fuel cell electrocatalyst modified by metal polyphenols of the present invention has the following advantages:
[0023] 1. The present invention adopts a simple and convenient synthesis method, which is economical, efficient, green and environmentally friendly. The synthesis steps are simple to operate, the reaction conditions are mild and easy to control, and the preparation cost is low. The prepared oxygen reduction catalyst not only exhibits high potential and good limiting current, but also has excellent stability;
[0024] 2. The prepared metal polyphenol-modified boron-nitrogen co-doped carbon-based oxygen reduction fuel cell electrocatalyst has an initial potential of 1.088 V, a half-wave potential of 0.666 V, and a limiting current density of 6.05 mA cm-2, which is slightly higher than the commercial platinum-carbon catalyst, and the electrocatalytic stability is better than the commercial Pt / C catalyst. The catalyst is better than the commercial platinum-carbon catalyst overall. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is the SEM image of C@CrB-BT-N nanocomposite;
[0026] Figure 2 XRD patterns of C@CrB-BT-N nanocomposites at different calcination temperatures (scanning range: 5°-80°, step size: 0.02°, scanning rate: 1.5° / min);
[0027] Figure 3 It is the XPS analysis diagram of C@CrB-BT-N nanocomposite;
[0028] Figure 4 This is the cyclic voltammetric characteristic curve of the C@CrB-BT-N catalyst (test voltage scanning range: -0.9-0.1V, scanning speed: 50mV / s);
[0029] Figure 5 This is the linear cyclic voltammogram of C@CrB-BT-N with different composite ratios of boron and metallic chromium in 0.1M KOH saturated with O2 (scanning range is -0.9-0.1V, scanning rate is 10mv / s);
[0030] Figure 6 It is the linear cyclic voltammogram at different temperatures in 0.1M KOH saturated with O2 when the molar ratio of boron element and metallic chromium is 1:1 (scanning range is -0.9-0.1V, scanning rate is 10mv / s);
[0031] Figure 7 This is the linear cyclic voltammogram of C@CrB-BT-N catalyst under different rotation speeds (400, 625, 900, 1225, 1600, 2025, 2500rmp) (scanning speed: 10mV / s);
[0032] Figure 8 This is a test graph of methanol tolerance of C@CrB-BT-N catalyst and commercial Pt / C (20wt% Pt) catalyst measured by constant voltage chronoamperometry;
[0033] Fig. 9This is a stability test chart of C@CrB-BT-N catalyst and commercial Pt / C (20wt% Pt) catalyst measured by constant voltage chronoamperometry. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0035] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0036] Example:
[0037] The embodiment of the present invention provides a method for preparing a boron-nitrogen co-doped carbon-based oxygen reduction fuel cell electrocatalyst based on metal polyphenol modification, comprising the following steps:
[0038] Step 1: Weigh a certain amount of white skin powder, prepare a certain amount of sodium hydroxide and sodium chloride solution and mix them together, dissolve the white skin powder in the mixed solution, and then stir it on a magnetic stirrer to form a gelatin solution, and then filter and precipitate the impurities, and then neutralize it with acid to a pH between 6-8. Finally, freeze it in a refrigerator, and then put it in a freeze dryer to dry for 24 hours to obtain gelatin solid. Among them, the amount of white skin powder and the mixed solution is 1g / 50ml; the mixed solution is made by mixing 0.1mol / l sodium hydroxide and 2mol / l sodium chloride solution in a volume ratio of 3:2, the temperature of the magnetic stirrer is 60 degrees Celsius, the speed is 700rpm, the time is 7h, the refrigerator freezing time is 12h, the freezer temperature is -78℃, and the time is 24h;
[0039] Step 2: Weigh a certain amount of bayberry tannin and Cr(NO3)3·9(H2O), dissolve them in deionized water, and then perform magnetic stirring after ultrasonic treatment to obtain a metal polyphenol network precursor solution constructed by tannin. The concentration of the prepared tannic acid solution is 0.05g / mol, and the concentration of Cr(NO3)3·9(H2O) is 2mol / l. ;
[0040] Step 3: Weigh a certain amount of boric acid and dissolve it in deionized water, stir to form a uniform boric acid solution, and pour the gelatin prepared in step 1 into the boric acid solution. The concentration of the boric acid solution is 1.5 mol / l, and the required amount is 200 ml;
[0041] Step 4: Pour the metal polyphenol precursor solution in step 2 into the mixed solution in step 3, and then place it on a magnetic stirrer for thorough stirring to evaporate all the water. The temperature of the magnetic stirrer is 80°C, and the stirring time is 24 hours;
[0042] Step 5: Wash the product of step 4 with deionized water and anhydrous ethanol for 2 to 3 times, filter and dry the product in an oven to obtain C@CrB-BT-N. The oven drying temperature is 60°C and the drying time is 18 hours;
[0043] Step 6: Place the dried precursor product in a tubular furnace in a nitrogen atmosphere for high-temperature pyrolysis, and cool naturally to room temperature to obtain a fuel cell cathode material. The specific operation of high-temperature pyrolysis is: in a pure nitrogen atmosphere, heat up to 400°C at a heating rate of 5°C / min and stabilize for 30 minutes, then heat up to 800°C at a heating rate of 5°C / min and maintain for 2 hours, and finally cool to room temperature with the furnace.
[0044] Step 7: Reflux the calcined sample in boiling water for 2 hours, then wash and dry the sample to obtain the fuel cell cathode material.
[0045] The active material described in the present invention is abbreviated as C@CrB-BT-N.
[0046] The present invention uses a carbon rod as a counter electrode, a saturated silver chloride electrode (Ag / AgCl) as a reference electrode, and a glassy carbon electrode as a working electrode.
[0047] The concentration of Nafion added in the catalyst preparation process of the present invention is 5%, and the dosage is 15ul.
[0048] The catalyst preparation of the present invention is to weigh 4 mg on a balance and disperse it in 1 mL of a mixed solution (235 uL of deionized water, 735 uL of isopropanol and 15 uL of a 5 wt% Nafion solution) to prepare a catalyst ink. Then, 28 uL of the ink is gradually added to the surface of a glassy carbon electrode (catalyst loading 0.25 mg cm-2), and the electrocatalytic performance is tested after natural drying.
[0049] All electrocatalytic performance tests described in the present invention are carried out in 0.1M KOH (pH = 13.62) electrolyte, and the potential measured in the experiment can be converted to the potential relative to the reversible hydrogen electrode (RHE) by the following formula:
[0050] E(RHE)=E(Ag / AgCl)+0.059*pH+0.2224
[0051] The potential values involved in the present invention are all potentials relative to a reversible hydrogen electrode.
[0052] The catalyst of the present invention needs to be activated by CV for 3 cycles before electrochemical testing.
[0053] The catalysts described in the present invention are all tested at room temperature to prevent large temperature changes from affecting the catalyst performance.
[0054] The present invention is further described below in conjunction with specific examples. In order to further understand the present invention, preferred embodiments of the present invention are described in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention. In addition, it should be understood that after reading the contents disclosed in the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope of protection defined by the present invention.
[0055] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.
[0056] Embodiment 1:
[0057] This example demonstrates a method for preparing a metal polyphenol-modified boron-nitrogen co-doped carbon-based oxygen reduction fuel cell electrocatalyst C@CrB-BT-N.
[0058] (1) Weigh 1g of white skin powder and dissolve it in 60ml of a mixed solution of sodium hydroxide and sodium chloride, wherein the mixed solution is a mixture of 30ml of 0.1mol / l sodium hydroxide and 20ml of 2mol / l sodium chloride solution, and then stir it on a magnetic stirrer, set the temperature to 60 degrees Celsius, and stir for 7 hours to form a gelatin solution. Then filter and precipitate impurities, and then neutralize it with acid to a pH between 6-8. Finally, freeze it in a refrigerator for 12 hours, and then put it in a freeze dryer and dry it for 24 hours to obtain a gelatin solid;
[0059] (2) Weigh 1 g of bayberry tannin and 0.06 mol of Cr(NO3)3·9(H2O), respectively dissolve them in 30 ml of deionized water, treat them ultrasonically for 1 hour, and then stir them magnetically for 2 hours to obtain a metal polyphenol network precursor solution constructed by tannin.
[0060] (3) Weigh 0.3 mol of boric acid and dissolve it in 200 ml of deionized water at 80° C., stir to form a uniform boric acid solution, and pour 2 g of gelatin prepared in step (1) into the boric acid solution;
[0061] (4) pouring the metal polyphenol precursor solution in step 2 into the mixed solution in step (3), placing it on a magnetic stirrer at 80° C. and stirring it thoroughly to evaporate all the water;
[0062] (5) Wash the product of step 4 with deionized water and anhydrous ethanol 2 to 3 times, filter the product and dry it in an oven at 60° C. for 18 h;
[0063] (6) The dried precursor product is evenly spread in a porcelain ark, and in a pure nitrogen atmosphere, the temperature is increased to 400°C at a heating rate of 5°C / min and stabilized for 30 minutes, and then the temperature is increased to 800°C at a heating rate of 5°C / min and maintained for 2 hours, and finally cooled to room temperature in the furnace to obtain a fuel cell cathode material.
[0064] (7) The calcined sample is refluxed in boiling water for 2 h, and then the sample is washed and dried to obtain a fuel cell cathode material.
[0065] The C@CrB-BT-N material obtained in this example was subjected to phase identification and micromorphology and structure characterization: an XPS analyzer, a powder X-ray diffractometer and an X-ray photoelectron spectrometer were used to identify the phase of the prepared material, and a scanning electron microscope was used to characterize the micromorphology and structure of the obtained material.
[0066] Figure 1 This is a scanning electron microscope image of the C@CrB-BT-N nanocomposite material. As can be seen from the figure, the catalyst of the metal polyphenol network of bayberry tannin and chromium nitrate composite loaded on B / N co-doped carbon nanosheets formed by pyrolysis of gelatin and boric acid has a porous structure, and its sheet structure gives the material higher toughness and is not easy to break. The rich microscopic porous structure of the catalyst allows the catalytic active sites to be better exposed, thereby obtaining better ORR catalytic performance.
[0067] Figure 2 The XRD diagram of C@CrB-BT-N nanocomposite material at different calcination temperatures (700℃, 800℃, 900℃) is shown in the figure. As can be seen from the figure, the purity of the obtained sample is relatively high, no obvious impurities are generated, and the sharper diffraction peaks indicate that the synthesized material has good crystallinity. The material has six obvious diffraction peaks at 2θ=27.769°, 30.591°, 39.855°, 54.581°, 57.257°, and 66.337°, which correspond to the (310), (232), (420), (442), (620), and (711) crystal planes of B2O3 (PDF#06-0297).
[0068] Figure 3This is the XPS graph of the C@CrB-BT-N nanocomposite. As can be seen from the figure, the surface element composition of the material is further confirmed. (a) is the XPS full spectrum analysis of the material, which confirms the presence of five elements, C, N, O, B, and Cr, on the surface of the material. It can be seen from the C1S spectrum that it is mainly divided into three peaks, corresponding to the two peaks of the C–Cr (283.027eV) bond and sp2C–C (284.8eV), and the small peak of the C–O (287.48eV) bond. The CC absorption peak shows that the composite material has a carbon matrix of graphitized carbon with good conductivity. It can be seen from the O1S spectrum that oxygen-containing functional groups CO (532.20eV) and COC (531.06eV) appear. This is consistent with the analysis results of XRD. From the high-resolution N1s spectrum, it can be seen that it is formed by four obvious peak fittings, indicating the existence of four forms of N, namely pyridinic N (397.92eV), quaternary N (400.73eV), pyridine-N-oxide (404.82eV) and nitrate (409.39eV). From the high-resolution B1s spectrum, it can be seen that there are two different signals with dissociation binding energies of 191.65eV and 192.52eV, corresponding to B-C2O / BN and B-CO2, respectively. From the elemental spectrum of Cr 2p, it can be found that it is also formed by four obvious peak fittings. The peaks at 586.09eV and 576.32eV correspond to Cr 2p1 / 2 and Cr 2p3 / 2 of hexavalent chromium, respectively, while the other two peaks correspond to trivalent chromium.
[0069] Embodiment 2:
[0070] This example demonstrates the electrochemical performance of a boron-nitrogen co-doped three-dimensional porous carbon nanofuel cell cathode material modified with bayberry tannin extract.
[0071] The present invention uses a carbon rod as a counter electrode, a saturated silver chloride electrode (Ag / AgCl) as a reference electrode, and a glassy carbon electrode as a working electrode.
[0072] The concentration of Nafion added in the catalyst preparation process of the present invention is 5wt% and the dosage is 15ul.
[0073] The electrode pretreatment in the test process of the present invention is to add α-Al2O3 electrode polishing powder and a small amount of deionized water on a nylon polishing cloth base, polish the rotating disk electrode back and forth in an "8" shape on it for 10 minutes, then clean the residual powder on the electrode with deionized water, and finally naturally air dry it to complete the treatment.
[0074] The catalyst preparation of the present invention is to weigh 4 mg on a balance and disperse it in a 1 mL centrifuge tube, add 235 uL of deionized water, 735 uL of isopropanol and 15 uL of 5 wt% Nafion solution, and then ultrasonicate at room temperature for 50 minutes to prepare catalyst ink. Then, 28 uL of ink is gradually added to the surface of the glassy carbon electrode (catalyst loading 0.25 mg cm-2), and the electrocatalytic performance is tested after natural drying.
[0075] All electrocatalytic performance tests described in the present invention are carried out in 0.1M KOH (pH = 13.62) electrolyte, and the potential measured in the experiment can be converted to the potential relative to the reversible hydrogen electrode (RHE) by the following formula:
[0076] E(RHE)=E(Ag / AgCl)+0.059*pH+0.2224
[0077] The potential values involved in the present invention are all potentials relative to a reversible hydrogen electrode.
[0078] The catalyst of the present invention needs to be activated by CV for 3 cycles before electrochemical testing.
[0079] The catalysts described in the present invention are all tested at room temperature to prevent large temperature changes from affecting the catalyst performance.
[0080] The Nafion added in the catalyst preparation process of the present invention is produced by Aldrich Sigma Company and has a concentration of 5%.
[0081] Use a pipette to draw 7ul of the catalyst and drop it onto the working electrode. Wait for it to dry naturally and repeat this step 3 times. Then slowly immerse the working electrode into the oxygen-saturated 0.1M KOH electrolyte. In this step, prevent bubbles from forming on the working electrode. During the entire test process, oxygen should be continuously introduced into the electrolyte to ensure oxygen saturation.
[0082] The catalyst obtained in the present embodiment is subjected to cyclic voltammetry and linear cyclic voltammetry test: the electrochemical workstation produced by Pine, USA, is used to carry out cyclic voltammetry experiment, and the test voltage scanning range is -0.9-0.1V, and the scanning speed is 50mV / s. During the test, the current density of 50mV / s is used to activate it for 3 circles before carrying out cyclic voltammetry test. Linear cyclic voltammetry test is also carried out using Pine electrochemical workstation, and the test voltage scanning range is -0.9-0.1V, and the scanning speed is 50mV / s. The speed test can obtain the current density of catalyst material under different speeds, and the number of transferred electrons can be known using KL equation, and the test current density is 10mV / s, and the rotating speed is 400, 625, 900, 1225, 1600, 2025rmp. Stability and methanol tolerance are also important indicators of catalyst performance. The test was also completed on an electrochemical workstation. The stability test voltage was -0.189 V and the test time was 20,000 s. The methanol tolerance test voltage was -0.189 V and the test time was 1,000 s. A 2M methanol solution was dripped in at 300 s.
[0083] Figure 4 This is the cyclic voltammetric characteristic curve of the C@CrB-BT-N catalyst (test voltage scanning range: -0.9-0.1V, scanning rate: 50mV / s). In the O2-saturated electrolyte, there is a cathode oxygen reduction peak at 0.71V, indicating that a catalytic oxygen reduction reaction has occurred. The response to oxygen shows that C@CrB-BT-N has obvious oxygen reduction catalytic activity in alkaline solution.
[0084] Figure 5 The linear cyclic voltammograms of C@CrB-BT-N catalyst at different temperatures are as follows (test voltage range: -0.9-0.1V, scanning speed: 10mV / s). When the calcination temperature is 800℃, the performance of C@CrB-BT-N catalyst is optimal.
[0085] Figure 6 This is the linear cyclic voltammogram of chromium and boron at different ratios in O2-saturated 0.1M KOH (scanning range is -0.9-0.1V, scanning rate is 10mv / s). The molar ratios of boron to chromium are 0:1, 0.05:1, 0.1:1, 0.2:1, and 0.5:1, respectively. It can be seen from the figure that at a heat treatment temperature of 800°C, when the molar ratio of boron to chromium is 0.2:1, the oxygen reduction ORR performance of the nanocomposite material reaches the optimal level, and the limiting current density increases from 2.89mA cm2 to 6.05mA cm2.
[0086] Figure 7This is the linear cyclic voltammogram of C@CrB-BT-N catalyst under different rotation speeds (400, 625, 900, 1225, 1600, 2025, 2500rmp) (scanning speed: 10mV / s). It can be seen that with the increase of rotation speed, the limiting diffusion current density of the catalyst gradually increases. This is because the faster the rotation speed, the faster the diffusion rate of oxygen, indicating that the oxygen reduction catalytic process is controlled by mass transfer and conforms to the first-order kinetic reaction.
[0087] Figure 8 The methanol tolerance of the best sample C@CrB-BT-N and the commercial 20% Pt / C catalyst was measured by adding 2mL of methanol to 0.1M KOH electrolyte at 1600rmp at 300s using IT technology. It can be observed from the figure that the limiting current density of C@CrB-BT-N has only slight changes, while the Pt / C catalyst shows significant changes in current density due to methanol oxidation. After continuing to run for 700s, the current density of C@CrB-BT-N still maintains a stable trend, while the retention rate of Pt / C decays to below 50%. This shows that C@CrB-BT-N is better than Pt / C in methanol tolerance.
[0088] Fig. 9 C@Cr is tested by chronoamperometry 0.2 B-BT-800℃ and Pt / C, after testing for 20000s, the initial current density of the Pt / C catalyst obviously lost about 23%, while that of the C@CrB-BT-N catalyst decreased by 19%, which indicates that the stability of the catalyst is better than that of the commercial Pt / C catalyst.
[0089] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a carbon-based oxygen reduction fuel cell negative electrode material based on chromium-containing leather residue from leathermaking solid waste as a carbon source precursor and modified by bayberry tannin extract and co-doped with boron and nitrogen, characterized in that: The preparation method comprises the following steps: Step 1: Weigh a certain amount of chromium-containing waste leather residue, prepare a certain amount of sodium hydroxide and sodium chloride solution and mix them together, dissolve the chromium-containing waste leather residue in the mixed solution, and then stir it on a magnetic stirrer to form a gelatin solution, then filter and precipitate the impurities, and then neutralize it with acid to a pH between 6-8. Finally, freeze it in a refrigerator, and then put it in a freeze dryer to dry for 24 hours to obtain gelatin solid; Step 2: Weigh a certain amount of bayberry tannin extract, dissolve it in deionized water, perform ultrasonic treatment, and then perform magnetic stirring to obtain a bayberry tannin extract solution; Step 3: Weigh a certain amount of boric acid and dissolve it in deionized water, stir to form a uniform boric acid solution, and pour the gelatin prepared in step 1 into the boric acid solution; Step 4: Pour the bayberry tannin extract solution in step 2 into the mixed solution in step 3, and then place it on a magnetic stirrer for full stirring to evaporate the water; Step 5: Wash the product of step 4 with deionized water and anhydrous ethanol 2 to 3 times, filter and dry the product in an oven to obtain C@CrB-BT-N; Step 6: Place the dried precursor product in a tubular furnace in a nitrogen atmosphere for high-temperature pyrolysis, and cool naturally to room temperature. Step 7: Reflux the calcined sample in boiling water, then wash and dry the sample to obtain a fuel cell cathode material.
2. The preparation method according to claim 1, characterized in that: The amount of chromium-containing waste leather residue and the mixed solution in step 1 is 1g / 50ml; the mixed solution is prepared by mixing 0.1mol / l sodium hydroxide and 2mol / l sodium chloride solution in a volume ratio of 3:2, the temperature of the magnetic stirrer is 60 degrees Celsius, the speed is 700rpm, the time is 7h, the refrigerator freezing time is 12h, and the freeze dryer temperature is -78°C for 24h.
3. The preparation method according to claim 1, characterized in that: In the step 2, the concentration of the prepared bayberry tannin extract solution is 0.05 g / mol.
4. The preparation method according to claim 1, characterized in that: In step 3, the concentration of the boric acid solution is 1.5 mol / l, and the required amount is 200 ml.
5. The preparation method according to claim 1, characterized in that: In the step 4, the temperature of the magnetic stirrer is 80° C. and the stirring time is 24 h.
6. The preparation method according to claim 1, characterized in that: In the step 5, the oven drying temperature is 60° C. and the time is 18 hours.
7. The preparation method according to claim 1, characterized in that: In step six, the specific operation of high-temperature pyrolysis is: in a pure nitrogen atmosphere, the temperature is increased to 400°C at a heating rate of 5°C / min and stabilized for 30 minutes, then the temperature is increased to 800°C at a heating rate of 5°C / min and maintained for 2 hours, and finally cooled to room temperature with the furnace.
8. The preparation method according to claim 1, characterized in that: The reflux time was 2 h.
9. A method for preparing a carbon-based oxygen reduction fuel cell negative electrode material based on the preparation method according to claims 1-8, using chromium-containing leather residue from leather-making solid waste as a carbon source precursor and modified by bayberry tannin extract and co-doped with boron and nitrogen.
Citation Information
Patent Citations
Heteroatom-doped porous carbon material as well as preparation method and application thereof
CN113942995A
Preparation of hierarchical porous collagen-based metal nickel organic framework composite carbon nanofiber fuel cell cathode material
CN115440992A
Electrode catalyst
JP2008047472A