Vermiculite insulating brick NG800-1200 DEG C 0.4-1.0, and preparation method and application thereof
By using vermiculite insulation bricks fired from kaolin and other materials to form a layered and cross-distributed porous structure with small round holes, it solves the problems of traditional insulation materials being anti-seepage, leak-proof and fast thermal conductivity, and achieves efficient thermal insulation. And pressure resistance, it is suitable for the energy saving and consumption reduction requirements of new electrolyzers with a production capacity of more than 400KA.
Patent Information
- Application Number
- CN202411108662.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-29
AI Technical Summary
The insulation materials of existing electrolytic cells are leak-proof and seepage-proof after extended use, resulting in weakening the function of the insulation layer and increasing energy consumption costs. Moreover, the process of traditional insulation bricks is not environmentally friendly and has fast thermal conductivity, which cannot meet the needs of new electrolytic cells above 400KA. Demand for energy saving and consumption reduction of production capacity.
Vermiculite insulation bricks are made of kaolin, Al2O3/porous glass balls, light refractory clay, high alumina cement, modified vermiculite mixed powder, clay brick powder, aluminum silicate fiber powder and polymer as raw materials. By rationally adjusting the raw material ratio and firing conditions, a layered pore structure combined with cross-distribution of small round pores is formed to improve the thermal insulation and pressure resistance properties.
Vermiculite insulation bricks with good thermal insulation effect, high load softening temperature and good strength have been achieved. They have poor thermal conductivity and are suitable for ultra-light insulation materials on the sides and bottom of electrolytic cells, extending the service life of electrolytic cells and reducing energy consumption. cost.
Smart Images

Figure BDA0004991537360000121 
Figure BDA0004991537360000131 
Figure BDA0004991537360000141
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory bricks, and particularly relates to a vermiculite insulation brick NG800-1200°C-0.4-1.0, a preparation method and application thereof. Background Art
[0002] As low temperature, low voltage and high current efficiency technology have become the development direction of energy conservation and consumption reduction in the electrolytic aluminum industry in recent years, domestic and foreign manufacturers have gradually eliminated low current production capacity. In recent years, most of the design capacity of new projects has exceeded 400Ka. On this basis, the overall design direction of the electrolytic cell body is towards energy conservation and consumption reduction, and it is optimized and improved on the original basis. For example, the anti-seepage layer material has been changed from the previous "dry anti-seepage material" to "dry anti-seepage material with composite anti-seepage bricks"; the design of the thermal insulation refractory material at the bottom and side of the electrolytic cell has been changed from the original material "clay insulation refractory bricks" to "vermiculite insulation bricks and insulation boards"; dry anti-seepage material, which has been widely used in aluminum plants in recent years, has also been gradually replaced by dry anti-seepage material and composite anti-seepage brick combination. The proportion of composite anti-seepage brick manufacturers and single tanks is increasing year by year. Dry anti-seepage materials have excellent anti-seepage effects, but their disadvantage is that they are not leak-proof. After more than 2 years of use, their anti-seepage performance will gradually weaken, and the molten cryolite will break through the anti-seepage layer and continue to leak downward, which will cause the insulation layer to gradually solidify and the insulation layer function to gradually weaken. As the use time increases, the insulation effect is greatly reduced, increasing the owner's energy consumption cost. For example, the Chinese patent application number 201710097206.4 discloses a composite anti-seepage brick for electrolytic cells, which uses coke, coke raw powder, potassium feldspar, water and active additives as raw materials. The composite anti-seepage brick is obtained by mixing, pressing and high-temperature drying. After use, it effectively improves the original material's anti-seepage but not anti-leakage properties, thereby solving the leakage problem of the electrolytic cell's anti-seepage layer and increasing the service life of the electrolytic cell. In addition, the electrolytic cell insulation material has also undergone tremendous evolution in recent years. The production process of the first generation of insulation bricks mainly uses high-aluminum materials and polylight balls for sintering. During high-temperature sintering, the polylight balls in the bricks are not resistant to high temperatures, and dioxins are formed after burning to emit gas. The insulation effect and flexural and compressive strength of the first generation of insulation bricks can meet the insulation layer needs of various high-temperature industries at that time. However, due to its environmentally unfriendly process, its production capacity has been gradually eliminated for nearly 10 years, and the number of users has decreased year by year. On the other hand, the pores formed after the combustion of the polylight balls in the first generation of insulation bricks are through-holes, and the heat The second-generation insulating bricks are manufactured using a semi-dry-wet process, primarily using clay powder, high-alumina powder, and floating beads, fired at medium temperature. They offer excellent thermal insulation, superior strength to the first-generation, with improved flexural and compressive strength, and lower thermal conductivity, resulting in improved insulation and energy savings. Examples include the NG120-0.6 clay insulating refractory brick, patented in CN201610606602; the NG125-0.8 clay insulating refractory brick and its preparation, patented in CN201610606607; and the NG130-1 clay insulating refractory brick, patented in CN201610606608.0 and its preparation. The aforementioned invention patents are all from the development period of the second-generation insulation bricks. With the progress of environmental protection, energy conservation and consumption reduction, the market application of the second-generation insulation bricks - clay-based insulating refractory bricks has surpassed the market share of the first generation. With the unstoppable development of new electrolytic cells with production capacity above 400KA, the subject of a new type of refractory insulation brick with lower thermal conductivity, better insulation effect, smaller body density and lighter weight has emerged. Therefore, it is very necessary to provide a vermiculite insulation brick NG800℃~1200℃-0.4~1.0 with excellent thermal insulation effect, high load refractoriness temperature, good strength, and low reheat line change rate, as well as a preparation method and application. Summary of the Invention
[0003] In response to existing needs, the present invention provides a vermiculite insulation brick NG800℃~1200℃-0.4~1.0, a preparation method and its application, and provides a new generation of thermal insulation refractory materials with better performance to meet the current energy-saving and emission reduction goals of electrolytic cells above 400KA.
[0004] The purpose of the present invention is to overcome the shortcomings of the existing technology and provide a vermiculite insulation brick NG800℃~1200℃-0.4~1.0 with good thermal insulation effect, high load softening temperature, good strength and small re-firing line change rate, a preparation method and its application.
[0005] The object of the present invention is achieved in that a vermiculite insulation brick NG800℃~1200℃-0.4~1.0 is formed by firing the following raw materials in proportion: kaolin 10-50%, Al2O3 / porous glass balls 5-70%, lightweight refractory clay 5-30%, high alumina cement 1-50%, modified vermiculite mixed powder 5-35%, clay brick powder 3-20%, water 3-12%, aluminum silicate fiber powder 1-5%, and polymer 1-5%.
[0006] The Al2O3 / porous glass spheres have a particle size of less than 6 mm and a bulk density of less than 0.18.
[0007] The kaolin and lightweight refractory clay have a bulk density of less than 1.0.
[0008] The particle size of the clay brick powder is greater than 600 mesh.
[0009] The modified vermiculite mixed powder is a mixture of particles with a bulk density of 1-3 mm and particles with a bulk density of 3-5 mm.
[0010] The high-alumina cement is 625 grade cement, the aluminum silicate fiber powder is 200 mesh; and the polymer is water glass.
[0011] A method for preparing vermiculite insulation bricks NG800°C-1200°C-0.4-1.0, comprising the following steps:
[0012] Step 1: batch, mix and wet-mix the raw materials according to the proportion to obtain mud;
[0013] Step 2: The clay obtained in step 1 is pressed into shape by a brick press and then dried to obtain a green body;
[0014] Step 3: The green body obtained in step 2 is fired, and the finished products are sorted, inspected and put into storage to obtain vermiculite insulation bricks.
[0015] The pressure of the brick press in step 2 is 80-500 tons, preferably 200 tons; the firing conditions in step 3 are: 600-1200°C, firing for 8-24 hours, preferably 900°C for 14 hours.
[0016] The invention discloses an application of vermiculite insulation bricks NG800℃~1200℃-0.4~1.0. The application comprises preparing the vermiculite insulation bricks NG800℃~1200℃-0.4~1.0 by reasonably adjusting the raw material ratio and using the above-mentioned preparation method to prepare ultra-light vermiculite insulation bricks suitable for the side of the electrolytic cell, vermiculite insulation bricks suitable for the insulation layer of the bottom of the electrolytic cell, and various special-shaped vermiculite insulation bricks and vermiculite insulation boards not limited to the standard brick size according to the size of the electrolytic cell.
[0017] The ultra-light vermiculite insulation bricks suitable for the side of the electrolytic cell have a body density of 0.4-0.5, a compressive strength at room temperature ≥1.3MPa, a compressive strength at high temperature ≥1.2MPa, an operating temperature of ≥900°C, and a thermal conductivity of 200°C ≤0.11; 300°C ≤0.123; 600°C ≤0.142; and 800°C ≤0.155. The vermiculite insulation bricks suitable for the insulation layer at the bottom of the electrolytic cell have a body density of 0.5-1.0, a compressive strength at room temperature ≥2.5MPa, a compressive strength at high temperature ≥2.5MPa, an operating temperature of ≥900°C, and a thermal conductivity of 500°C ≤0.2; and 800°C ≤0.23.
[0018] Beneficial effects of the present invention: The present invention provides a vermiculite insulation brick NG800℃~1200℃-0.4~1.0, a preparation method and its application. In use, the present invention introduces Al2O3 / porous glass balls in the preparation process. On the one hand, the gas in the porous glass balls forms circular closed pores in the brick body, which has excellent thermal insulation properties; secondly, the present invention adds modified vermiculite composite powder. The modified vermiculite composite powder has a unique flaky structure. After expanding in a high temperature environment, it can be tightly combined with Al2O3 / porous glass balls and clay to form a The pore structure is layered and cross-distributed with small circular holes. Compared with the through-holes of the first-generation insulation bricks - polylight bricks, the performance of heat insulation and heat dissipation is better than that of the second-generation insulation bricks - clay insulation refractory bricks. The internal structure of the new insulation is that when heat is conducted, it is transferred layer by layer from the high-temperature side to the outermost brick body. The thermal conductivity is relatively poor, but the thermal insulation performance is better than that of the second-generation insulation bricks - clay insulation refractory bricks. By reasonably adjusting the ratio of raw materials, it can be made into vermiculite insulation bricks suitable for the side of the electrolytic cell, with a body density of 0.4-0.5 and a compressive strength of ≥1.3M at room temperature. Ultra-light vermiculite insulation bricks with a high temperature compressive strength (500℃) ≥1.2MPa, an operating temperature of ≥900℃, and a thermal conductivity coefficient (W / m·K) of 200℃≤0.11; 300℃≤0.123; 600℃≤0.142; 800℃≤0.155; for the design of the vermiculite insulation bricks for the bottom insulation layer, considering the overall weight and pressure of the electrolytic cell, the vermiculite insulation products at the bottom need to ensure better anti-bending and anti-compression performance while meeting lower thermal conductivity. After testing, vermiculite insulation bricks suitable for the bottom of the electrolytic cell were made. , vermiculite insulation bricks with a body density of 0.5-1.0, compressive strength at room temperature ≥2.5MPa, compressive strength at high temperature (500℃) ≥2.5MPa, operating temperature ≥900℃, thermal conductivity 500℃≤0.2; 800℃≤0.23; at the same time, according to the design of the manufacturer's electrolytic cell size, various types of special-shaped vermiculite insulation bricks and vermiculite insulation boards with length, height and width that are not limited to the standard brick size of 230*114*65mm can be customized; the present invention has the advantages of good thermal insulation effect, high load softening temperature, good strength and small re-firing line change rate. DETAILED DESCRIPTION
[0019] The present invention aims to provide a side and bottom insulation product that is better adapted to a production capacity of more than 400KA, better match the electrolytic cell design after the silicon nitride combined with silicon carbide side modification and the dry anti-seepage material combined with the composite anti-seepage brick optimization, and provide a vermiculite insulation brick NG800℃~1200℃-0.4~1.0, preparation method and application thereof for the energy-saving field of electrolytic aluminum production.
[0020] The present invention will be further described below.
[0021] Example 1
[0022] A vermiculite insulation brick NG800-1200°C-0.4-1.0 is prepared by firing raw materials in the following proportions: 25% kaolin, 35% Al2O3 / porous glass balls, 8% lightweight refractory clay, 5% high-alumina cement, 15% modified vermiculite mixed powder, 3% clay brick powder, 5% water, 2% aluminum silicate fiber powder, and 2% polymer.
[0023] The raw materials of the present invention, namely, kaolin, light refractory clay, Al2O3 / porous glass balls, and modified vermiculite composite powder, are all commercially available products. The Al2O3 / porous glass balls have a particle size of less than 6 mm and a bulk density of less than 0.18. The kaolin and light refractory clay have a bulk density of less than 1.0, the clay brick powder has a particle size of greater than 600 meshes, the modified vermiculite mixed powder is a mixture of particles with bulk densities of 1-3 mm and 3-5 mm, the high-alumina cement is 625 grade cement, the aluminum silicate fiber powder is 200 meshes, the water is normal industrial water, and the polymer is water glass.
[0024] A method for preparing vermiculite insulation bricks NG800°C-1200°C-0.4-1.0, comprising the following steps:
[0025] Step 1: batch, mix and wet-mix the raw materials according to the proportion to obtain mud;
[0026] Step 2: The clay obtained in step 1 is pressed into shape by a brick press and then dried to obtain a green body;
[0027] Step 3: The green body obtained in step 2 is fired, and the finished products are sorted, inspected and put into storage to obtain vermiculite insulation bricks.
[0028] The pressure of the brick press in step 2 is 200 tons; the firing conditions in step 3 are: 900° C., and firing for 14 hours.
[0029] The present invention relates to a vermiculite insulation brick NG800℃~1200℃-0.4~1.0, a preparation method and an application thereof. In use, the present invention introduces Al2O3 / porous glass balls in the preparation process. On the one hand, the gas existing in the porous glass balls forms circular closed pores in the brick body, which has excellent thermal insulation properties; secondly, the present invention adds modified vermiculite composite powder. The modified vermiculite composite powder has a unique flaky structure and can be tightly bonded to Al2O3 / porous glass balls and clay after expansion in a high temperature environment. The invention has the advantages of good thermal insulation effect, high load softening temperature, good strength and small reheating line change rate, and has a good heat insulation performance.
[0030] Example 2
[0031] A vermiculite insulation brick NG800-1200°C-0.4-1.0 is prepared by firing raw materials in the following proportions: 10% kaolin, 50% Al2O3 / porous glass balls, 8% lightweight refractory clay, 13% high-alumina cement, 10% modified vermiculite mixed powder, 3% clay brick powder, 4% water, 2% aluminum silicate fiber powder, and 1% polymer.
[0032] The raw materials of the present invention, namely, kaolin, light refractory clay, Al2O3 / porous glass balls, and modified vermiculite composite powder, are all commercially available products. The Al2O3 / porous glass balls have a particle size of less than 6 mm and a bulk density of less than 0.18. The kaolin and light refractory clay have a bulk density of less than 1.0, the clay brick powder has a particle size of greater than 600 meshes, the modified vermiculite mixed powder is a mixture of particles with bulk densities of 1-3 mm and 3-5 mm, the high-alumina cement is 625 grade cement, the aluminum silicate fiber powder is 200 meshes, the water is normal industrial water, and the polymer is water glass.
[0033] A method for preparing vermiculite insulation bricks NG800°C-1200°C-0.4-1.0, comprising the following steps:
[0034] Step 1: batch, mix and wet-mix the raw materials according to the proportion to obtain mud;
[0035] Step 2: The clay obtained in step 1 is pressed into shape by a brick press and then dried to obtain a green body;
[0036] Step 3: The green body obtained in step 2 is fired, and the finished products are sorted, inspected and put into storage to obtain vermiculite insulation bricks.
[0037] The pressure of the brick press in step 2 is 120 tons; the firing conditions in step 3 are: 750° C., and firing for 20 hours.
[0038] The present invention relates to a vermiculite insulation brick NG800℃~1200℃-0.4~1.0, a preparation method and an application thereof. In use, the present invention introduces Al2O3 / porous glass balls in the preparation process. On the one hand, the gas existing in the porous glass balls forms circular closed pores in the brick body, which has excellent thermal insulation properties; secondly, the present invention adds modified vermiculite composite powder. The modified vermiculite composite powder has a unique flaky structure and can be tightly bonded to Al2O3 / porous glass balls and clay after expansion in a high temperature environment. The invention has the advantages of good thermal insulation effect, high load softening temperature, good strength and small reheating line change rate, and has a good heat insulation performance.
[0039] Example 3
[0040] A vermiculite insulation brick NG800-1200°C-0.4-1.0 is prepared by firing raw materials in the following proportions: 25% kaolin, 18% Al2O3 / porous glass balls, 8% lightweight refractory clay, 18% high-alumina cement, 20% modified vermiculite mixed powder, 4% clay brick powder, 5% water, 1% aluminum silicate fiber powder, and 1% polymer.
[0041] The raw materials of the present invention, namely, kaolin, light refractory clay, Al2O3 / porous glass balls, and modified vermiculite composite powder, are all commercially available products. The Al2O3 / porous glass balls have a particle size of less than 6 mm and a bulk density of less than 0.18. The kaolin and light refractory clay have a bulk density of less than 1.0, the clay brick powder has a particle size of greater than 600 meshes, the modified vermiculite mixed powder is a mixture of particles with bulk densities of 1-3 mm and 3-5 mm, the high-alumina cement is 625 grade cement, the aluminum silicate fiber powder is 200 meshes, the water is normal industrial water, and the polymer is water glass.
[0042] A method for preparing vermiculite insulation bricks NG800°C-1200°C-0.4-1.0, comprising the following steps:
[0043] Step 1: batch, mix and wet-mix the raw materials according to the proportion to obtain mud;
[0044] Step 2: The clay obtained in step 1 is pressed into shape by a brick press and then dried to obtain a green body;
[0045] Step 3: The green body obtained in step 2 is fired, and the finished products are sorted, inspected and put into storage to obtain vermiculite insulation bricks.
[0046] The pressure of the brick press in step 2 is 80 tons; the firing conditions in step 3 are: 850° C., and firing for 14 hours.
[0047] The present invention relates to a vermiculite insulation brick NG800℃~1200℃-0.4~1.0, a preparation method and an application thereof. In use, the present invention introduces Al2O3 / porous glass balls in the preparation process. On the one hand, the gas existing in the porous glass balls forms circular closed pores in the brick body, which has excellent thermal insulation properties; secondly, the present invention adds modified vermiculite composite powder. The modified vermiculite composite powder has a unique flaky structure and can be tightly bonded to Al2O3 / porous glass balls and clay after expansion in a high temperature environment. The invention has the advantages of good thermal insulation effect, high load softening temperature, good strength and small reheating line change rate, and has a good heat insulation performance.
[0048] Comparative Example 1
[0049] Compared with Example 1, other raw materials remain unchanged, only the parameters of kaolin 25% and Al2O3 / porous glass balls 35% are replaced with kaolin 35% and Al2O3 / porous glass balls 25%. The remaining steps refer to Example 1;
[0050] That is, a vermiculite insulation brick NG800℃~1200℃-0.4~1.0 is made by firing raw materials in the following proportions: 35% kaolin, 25% Al2O3 / porous glass balls, 8% lightweight refractory clay, 5% high alumina cement, 15% modified vermiculite mixed powder, 3% clay brick powder, 5% water, 8% aluminum silicate fiber powder, and 2% polymer.
[0051] The raw materials of the present invention, namely, kaolin, light refractory clay, Al2O3 / porous glass balls, and modified vermiculite composite powder, are all commercially available products. The Al2O3 / porous glass balls have a particle size of less than 6 mm and a bulk density of less than 0.18. The kaolin and light refractory clay have a bulk density of less than 1.0, the clay brick powder has a particle size of greater than 600 meshes, the modified vermiculite mixed powder is a mixture of particles with bulk densities of 1-3 mm and 3-5 mm, the high-alumina cement is 625 grade cement, the aluminum silicate fiber powder is 200 meshes, the water is normal industrial water, and the polymer is water glass.
[0052] Specifically: a preparation method of vermiculite insulation brick NG800℃~1200℃-0.4~1.0, comprising the following steps:
[0053] Step 1: batch, mix and wet-mix the raw materials according to the proportion to obtain mud;
[0054] Step 2: The clay obtained in step 1 is pressed into shape by a brick press and then dried to obtain a green body;
[0055] Step 3: The green body obtained in step 2 is fired, and the finished products are sorted, inspected and put into storage to obtain vermiculite insulation bricks.
[0056] The pressure of the brick press in step 2 is 200 tons; the firing conditions in step 3 are: 9000° C., and firing for 14 hours.
[0057] Comparative Example 2
[0058] Compared with Example 1, the ratio of aluminum silicate fiber powder was adjusted to 8%, and the rest of the process was the same as in Example 1;
[0059] That is, a vermiculite insulation brick NG800℃~1200℃-0.4~1.0 is made by firing raw materials in the following proportions: 25% kaolin, 35% Al2O3 / porous glass balls, 8% lightweight refractory clay, 5% high alumina cement, 15% modified vermiculite mixed powder, 3% clay brick powder, 5% water, 8% aluminum silicate fiber powder, and 2% polymer.
[0060] The raw materials of the present invention, namely, kaolin, light refractory clay, Al2O3 / porous glass balls, and modified vermiculite composite powder, are all commercially available products. The Al2O3 / porous glass balls have a particle size of less than 6 mm and a bulk density of less than 0.18. The kaolin and light refractory clay have a bulk density of less than 1.0, the clay brick powder has a particle size of greater than 600 meshes, the modified vermiculite mixed powder is a mixture of particles with bulk densities of 1-3 mm and 3-5 mm, the high-alumina cement is 625 grade cement, the aluminum silicate fiber powder is 200 meshes, the water is normal industrial water, and the polymer is water glass.
[0061] Specifically: a preparation method of vermiculite insulation brick NG800℃~1200℃-0.4~1.0, comprising the following steps:
[0062] Step 1: batch, mix and wet-mix the raw materials according to the proportion to obtain mud;
[0063] Step 2: The clay obtained in step 1 is pressed into shape by a brick press and then dried to obtain a green body;
[0064] Step 3: The green body obtained in step 2 is fired, and the finished products are sorted, inspected and put into storage to obtain vermiculite insulation bricks.
[0065] The pressure of the brick press in step 2 is 200 tons; the firing conditions in step 3 are: 900° C., and firing for 14 hours.
[0066] Comparative Example 3
[0067] Compared with Example 1, the ratio of vermiculite powder was adjusted to 30%, and the rest of the process was referred to Example 1;
[0068] That is, a vermiculite insulation brick NG800℃~1200℃-0.4~1.0 is made by firing raw materials in the following proportions: kaolin 25%, Al2O3 / porous glass balls 35%, lightweight refractory clay 8%, high alumina cement 5%, modified vermiculite mixed powder 30%, clay brick powder 3%, water 5%, aluminum silicate fiber powder 2%, and polymer 2%.
[0069] The raw materials of the present invention, namely, kaolin, light refractory clay, Al2O3 / porous glass balls, and modified vermiculite composite powder, are all commercially available products. The Al2O3 / porous glass balls have a particle size of less than 6 mm and a bulk density of less than 0.18. The kaolin and light refractory clay have a bulk density of less than 1.0, the clay brick powder has a particle size of greater than 600 meshes, the modified vermiculite mixed powder is a mixture of particles with bulk densities of 1-3 mm and 3-5 mm, the high-alumina cement is 625 grade cement, the aluminum silicate fiber powder is 200 meshes, the water is normal industrial water, and the polymer is water glass.
[0070] Specifically: a preparation method of vermiculite insulation brick NG800℃~1200℃-0.4~1.0, comprising the following steps:
[0071] Step 1: batch, mix and wet-mix the raw materials according to the proportion to obtain mud;
[0072] Step 2: The clay obtained in step 1 is pressed into shape by a brick press and then dried to obtain a green body;
[0073] Step 3: The green body obtained in step 2 is fired, and the finished products are sorted, inspected and put into storage to obtain vermiculite insulation bricks.
[0074] The pressure of the brick press in step 2 is 200 tons; the firing conditions in step 3 are: 900° C., and firing for 14 hours.
[0075] Comparative Example 4
[0076] Compared with Example 1, the proportion of polymer was increased by 5%, and the rest of the process was the same as in Example 1;
[0077] That is, a vermiculite insulation brick NG800℃~1200℃-0.4~1.0 is made by firing raw materials in the following proportions: kaolin 25%, Al2O3 / porous glass balls 35%, lightweight refractory clay 8%, high alumina cement 5%, modified vermiculite mixed powder 15%, clay brick powder 3%, water 5%, aluminum silicate fiber powder 2%, and polymer 5%.
[0078] The raw materials of the present invention, namely, kaolin, light refractory clay, Al2O3 / porous glass balls, and modified vermiculite composite powder, are all commercially available products. The Al2O3 / porous glass balls have a particle size of less than 6 mm and a bulk density of less than 0.18. The kaolin and light refractory clay have a bulk density of less than 1.0, the clay brick powder has a particle size of greater than 600 meshes, the modified vermiculite mixed powder is a mixture of particles with bulk densities of 1-3 mm and 3-5 mm, the high alumina cement is 625 grade cement, the aluminum silicate fiber powder is 200 meshes, the water is normal industrial water, and the polymer is water glass.
[0079] Specifically: a preparation method of vermiculite insulation brick NG800℃~1200℃-0.4~1.0, comprising the following steps:
[0080] Step 1: batch, mix and wet-mix the raw materials according to the proportion to obtain mud;
[0081] Step 2: The clay obtained in step 1 is pressed into shape by a brick press and then dried to obtain a green body;
[0082] Step 3: The green body obtained in step 2 is fired, and the finished products are sorted, inspected and put into storage to obtain vermiculite insulation bricks.
[0083] The pressure of the brick press in step 2 is 200 tons; the firing conditions in step 3 are: 900° C., and firing for 14 hours.
[0084] Relevant tests are used to further illustrate the performance and other related indicators of the vermiculite insulation brick NG800℃~1200℃-0.4~1.0 of the present invention, so as to verify the excellent performance of the vermiculite insulation brick NG800℃~1200℃-0.4~1.0 of the present invention;
[0085] The products prepared in Examples 1-3 and Comparative Examples 1-4 were tested for physical and chemical indicators: ① Physical aspects: bulk density, room temperature compressive strength, high temperature compressive strength, heating permanent line change, thermal conductivity test, loss on ignition; ② Chemical aspects: alumina, silica, iron content, magnesium oxide, calcium oxide, sodium oxide, titanium dioxide, potassium oxide.
[0086] The physical inspection markings refer to national standards and industry inspection standards. The specific results are shown in the following table.
[0087]
[0088] Chemical testing uses spectrometer-X fluorescence chemical analysis, and the test results are shown in the following table.
[0089]
[0090]
[0091] It can be seen from the data in the table above that the bulk density of the insulation bricks prepared in Example 2 and Comparative Example 3 is relatively small, and the difference in thermal conductivity is not much. However, compared with Example 2, the room temperature compressive strength and high temperature compressive strength of Comparative Example 3 are not as good as those in Example 2. Adding too much modified vermiculite composite powder may reduce the compressive effect of vermiculite insulation bricks. Compared with Example 2, the loss on ignition is significantly higher than other loss on ignition data. There may be a low sintering temperature, which may cause the sintering to be not fully burned through during sintering. Adding more high alumina cement, all other experimental examples and the comparative example all adopt higher sintering temperature; in addition, the experimental results show no obvious optimization of thermal conductivity with the increase of the proportion of aluminum silicate fiber powder, but may lead to a slight decrease in room temperature pressure resistance and high temperature pressure resistance; according to the physical data of Examples 1-3 and Comparative Example 1, kaolin, Al2O3 / porous glass balls and modified vermiculite mixed powder are the key to determining the final product body density and room temperature pressure resistance and high temperature pressure resistance parameters. By changing the ratio of the three, a new vermiculite thermal insulation material suitable for the side and bottom of the electrolytic cell is made.
[0092] To sum up, compared with the prior art, the present invention introduces Al2O3 / porous glass balls in the preparation process. On the one hand, the existing gas in the porous glass balls forms circular closed pores in the brick body, which has excellent thermal insulation properties; secondly, the present invention adds modified vermiculite composite powder. The modified vermiculite composite powder has a unique flaky structure and can be tightly combined with Al2O3 / porous glass balls and clay after expansion in a high-temperature environment to form a layered porous structure with small circular holes distributed crosswise. Compared with the through-type pores of the first-generation insulation bricks-polylight bricks, the heat-insulating and heat-dissipating properties and the non-through-type pores of the second-generation insulation bricks-clay insulating refractory bricks, the new insulation internal structure transfers heat layer by layer from the high-temperature side to the outermost brick body during heat conduction. The thermal conductivity is relatively poor, but the thermal insulation performance is better than the second-generation insulation bricks-clay insulating refractory bricks.
[0093] In addition, the present invention also discloses an application of vermiculite insulation bricks NG800℃~1200℃-0.4~1.0, which comprises preparing the vermiculite insulation bricks NG800℃~1200℃-0.4~1.0 by reasonably adjusting the raw material ratio and using the above-mentioned preparation method to prepare ultra-light vermiculite insulation bricks suitable for the side of the electrolytic cell, vermiculite insulation bricks suitable for the insulation layer of the bottom of the electrolytic cell, and various special-shaped vermiculite insulation bricks and vermiculite insulation boards not limited to the standard brick size according to the size of the electrolytic cell, specifically:
[0094] ① By rationally adjusting the ratio of raw materials, ultra-light vermiculite insulation bricks suitable for the side of the electrolytic cell can be made, with a body density of 0.4-0.5, a compressive strength at room temperature ≥1.3MPa, a high-temperature compressive strength (500℃) ≥1.2MPa, an operating temperature of ≥900℃, and a thermal conductivity (W / m·K) of 200℃≤0.11; 300℃≤0.123; 600℃≤0.142; 800℃≤0.155;
[0095] ② Regarding the design of vermiculite insulation bricks for the bottom insulation layer, considering the overall weight and pressure of the electrolytic cell, the vermiculite insulation products at the bottom need to ensure better anti-bending and anti-compression performance while also meeting lower thermal conductivity. After testing, vermiculite insulation bricks suitable for the bottom of the electrolytic cell were made, with a body density of 0.5-1.0, a compressive strength of ≥2.5MPa at room temperature, a compressive strength of ≥2.5MPa at high temperature (500℃), an operating temperature of ≥900℃, and a thermal conductivity of ≤0.2 at 500℃ and ≤0.23 at 800℃.
[0096] ③At the same time, according to the design of the manufacturer's electrolytic cell size, various types of special-shaped vermiculite insulation bricks and vermiculite insulation boards can be made, and the length, height and width can be customized, not limited to the standard brick size of 230*114*65mm.
Claims
1. A vermiculite insulation brick NG800℃~1200℃-0.4~1.0, characterized by: It is made by firing raw materials in the following proportions: 10-50% kaolin, 5-70% Al2O3 / porous glass balls, 5-30% lightweight refractory clay, 1-50% high-alumina cement, 5-35% modified vermiculite mixed powder, 3-20% clay brick powder, 3-12% water, 1-5% aluminum silicate fiber powder, and 1-5% polymer.
2. The vermiculite insulation brick NG800℃~1200℃-0.4~1.0 as claimed in claim 1, characterized in that: The Al2O3 / porous glass sphere has a particle size of less than 6 mm and a bulk density of less than 0.
18.
3. The vermiculite insulation brick NG800℃~1200℃-0.4~1.0 as claimed in claim 2, characterized in that: The kaolin and light refractory clay have a bulk density of less than 1.
0.
4. The vermiculite insulation brick NG800℃~1200℃-0.4~1.0 as claimed in claim 3, characterized in that: The particle size of the clay brick powder is greater than 600 mesh.
5. The vermiculite insulation brick NG800℃~1200℃-0.4~1.0 as claimed in claim 4, characterized in that: The modified vermiculite mixed powder is a mixture of particles with a bulk density of 1-3 mm and particles with a bulk density of 3-5 mm.
6. The vermiculite insulation brick NG800℃~1200℃-0.4~1.0 as claimed in claim 5, characterized in that: The high-alumina cement is 625 grade cement, the aluminum silicate fiber powder is 200 mesh; and the polymer is water glass.
7. A method for preparing vermiculite insulation brick NG800℃~1200℃-0.4~1.0 according to any one of claims 1-6, characterized in that: The following steps are involved: Step 1: batch, mix and wet-mix the raw materials according to the proportion to obtain mud; Step 2: The clay obtained in step 1 is pressed into shape by a brick press and then dried to obtain a green body; Step 3: The green body obtained in step 2 is fired, and the finished products are sorted, inspected and put into storage to obtain vermiculite insulation bricks.
8. The method for preparing vermiculite insulation brick NG800℃~1200℃-0.4~1.0 as claimed in claim 7, characterized in that: The pressure of the brick press in step 2 is 80-500 tons; the firing conditions in step 3 are: 600-1200° C., and firing time is 8-24 hours.
9. An application of vermiculite insulation brick NG800℃~1200℃-0.4~1.0, characterized in that: The application includes making the vermiculite insulation brick NG800℃~1200℃-0.4~1.0 described in any one of claims 1 to 6 into ultra-light vermiculite insulation bricks suitable for the side of the electrolytic cell, vermiculite insulation bricks suitable for the insulation layer at the bottom of the electrolytic cell, and various special-shaped vermiculite insulation bricks and vermiculite insulation boards not limited to the standard brick size according to the size of the electrolytic cell by reasonably adjusting the raw material ratio and adopting the preparation method described in claim 7.
10. The application of the vermiculite insulation brick NG800℃~1200℃-0.4~1.0 as claimed in claim 9, characterized in that: The ultra-light vermiculite insulation brick suitable for the side of the electrolytic cell has a body density of 0.4-0.5, a compressive strength at room temperature ≥1.3MPa, a compressive strength at high temperature ≥1.2MPa, an operating temperature of ≥900°C, and a thermal conductivity of 200°C≤0.11; 300°C≤0.123; 600°C≤0.142; 800°C≤0.155; the vermiculite insulation brick suitable for the insulation layer at the bottom of the electrolytic cell has a body density of 0.5-1.0, a compressive strength at room temperature ≥2.5MPa, a compressive strength at high temperature ≥2.5MPa, an operating temperature of ≥900°C, and a thermal conductivity of 500°C≤0.2; 800°C≤0.23.
Citation Information
Patent Citations
Low-thermal conductivity modified vermiculite composite thermal insulation material and preparation method thereof
CN102503482A
Light cement foam insulation plate and production method thereof
CN103183521A
Mineral polymer material composition and preparation method and application thereof in thermal insulation material
CN112374801A
Composite vermiculite insulating brick for electrolytic cell and preparation method of composite vermiculite insulating brick
CN118405929A
Method of making ceramic-vermiculite articles
RU2819710C1