Substrate processing method, semiconductor device manufacturing method, recording medium, and substrate processing apparatus

By forming and modifying the carbonitride film on the substrate, the problem of residual hydrogen and chlorine in the carbonitride film affecting film properties is solved, and the effect of improving film density and resistance is achieved.

CN118854259APending Publication Date: 2024-10-29KOKUSAI DENKI KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410325290.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-03-21
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the carbonitride film formed on the substrate, impurities such as hydrogen and chlorine remaining in the carbonitride film will affect the characteristics of the film, resulting in a reduction in the density and resistance of the film.

Method used

A first film containing carbon, nitrogen and hydrogen bonded to carbon is formed on the substrate through a cyclic process, and different modifiers are used to modify it to reduce the hydrogen and chlorine content ratio in the carbonitride film to form a third film. Second film. This process includes multiple treatments of the substrate, using a first modifier and a second modifier for nitriding and modification respectively to reduce impurity residues.

Benefits of technology

The film's ashing resistance and etching resistance are improved, forming a film with high density and reduced impurities, ensuring that the concentration of carbon and hydrogen in the film is within an appropriate range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854259A_ABST
    Figure CN118854259A_ABST
Patent Text Reader

Abstract

The invention provides a substrate processing method capable of improving characteristics of a film formed on a substrate, a method of manufacturing a semiconductor device, a recording medium, and a substrate processing apparatus. The present invention relates to a method for forming a first film on a substrate, the method comprising the steps of: (a) forming a first film on the substrate, the first film containing a predetermined element, nitrogen, carbon, and hydrogen bonded to the carbon, by performing a predetermined number of cycles including a step of supplying a raw material containing the predetermined element, carbon, and hydrogen to the substrate, and a step of supplying a first modifier containing nitrogen to the substrate; and (b) modifying the first film to a second film containing the predetermined element, carbon, and nitrogen, in which the content ratio of hydrogen bonded to the carbon is reduced compared to that of the first film by supplying a second modifying agent different from the first modifying agent to the substrate on which the first film has been formed, the second modifier is a compound or a derivative thereof that contains a bond between nitrogen and hydrogen and a bond between nitrogen and each other in one molecule.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a substrate processing method, a method for manufacturing a semiconductor device, a recording medium, and a substrate processing device. Background Art

[0002] As one of the steps in the process of manufacturing a semiconductor device, a process of supplying a plurality of processing gases to a substrate to form a carbonitride film on the substrate is sometimes performed (see, for example, Patent Document 1).

[0003] Prior art literature

[0004] Patent Document 1: Japanese Patent Application Publication No. 2015-153825 Summary of the invention

[0005] Problems to be solved by the invention

[0006] As described above, when a carbonitride film is formed on a substrate, impurities such as hydrogen (H) bonded to carbon (C) may remain in the carbonitride film and may affect the characteristics of the film.

[0007] The present disclosure provides a technology capable of improving the characteristics of a film formed on a substrate.

[0008] Means for solving problems

[0009] According to one embodiment of the present disclosure, a technology is provided, comprising the following steps:

[0010] (a) forming a first film including the predetermined element, nitrogen, carbon, and hydrogen bonded to the carbon on a substrate by performing a predetermined number of cycles, the cycle including a step of supplying a raw material including the predetermined element, carbon, and hydrogen to the substrate, and a step of supplying a first modifier including nitrogen to the substrate; and

[0011] (b) A process of modifying the first film into a second film containing the specified element, carbon and nitrogen in which the content ratio of hydrogen bonded to the carbon is reduced compared to the first film by supplying a second modifier different from the first modifier to the substrate on which the first film is formed, wherein the second modifier is a compound or a derivative thereof containing a bond between nitrogen and hydrogen and a bond between nitrogen in one molecule.

[0012] Effects of the Invention

[0013] According to the present disclosure, the characteristics of a film formed on a substrate can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a schematic structural diagram of a vertical processing furnace of a substrate processing apparatus preferably used in one embodiment of the present disclosure, and is a diagram showing a processing furnace portion in a longitudinal cross-sectional view.

[0015] Figure 2 This is a schematic diagram of a vertical processing furnace of a substrate processing device preferably used in one embodiment of the present invention. Figure 1 The AA line cross-sectional view shows a portion of the processing furnace.

[0016] Figure 3 This is a schematic configuration diagram of a controller of a substrate processing apparatus preferably used in one embodiment of the present disclosure, and is a diagram showing a control system of the controller in the form of a block diagram.

[0017] Figure 4 This is a flowchart showing a substrate processing step preferably used in one embodiment of the present disclosure.

[0018] Figure 5 (A) is a diagram for explaining the state on the surface of the substrate when the first modifying agent is supplied to the substrate on which the raw material is adsorbed. Figure 5 (B) is a diagram for explaining the state on the surface of the substrate when the second modifying agent is supplied to the substrate on which the raw material is adsorbed.

[0019] Figure 6 This is a flowchart showing a modified example of a substrate processing step preferably used in one embodiment of the present disclosure. DETAILED DESCRIPTION

[0020] <One aspect of the present disclosure>

[0021] The following mainly refers to Figure 1 to Figure 5 One mode of the present disclosure is described. In addition, the drawings used in the following description are all schematic, and the relationship between the dimensions of the elements shown in the drawings, the ratio of the elements, etc. may not be consistent with the actual situation. In addition, the relationship between the dimensions of the elements, the ratio of the elements, etc. may not be consistent between multiple drawings.

[0022] (1) Structure of substrate processing apparatus

[0023] like Figure 1 As shown, the processing furnace 202 has a heater 207 as a heating mechanism (temperature adjustment unit). The heater 207 is cylindrical and is vertically mounted by being supported by a holding plate. The heater 207 also functions as an activation mechanism (excitation unit) that activates (excites) the gas using heat.

[0024] A reaction tube 203 is disposed concentrically with the heater 207 on the inner side of the heater 207. The reaction tube 203 is made of a heat-resistant material such as quartz (SiO2) or silicon carbide (SiC), and is formed into a cylindrical shape with a closed upper end and an open lower end. A processing chamber 201 is formed in the hollow portion of the reaction tube 203. The processing chamber 201 is configured to accommodate a wafer 200 as a substrate. The wafer 200 is processed in the processing chamber 201.

[0025] Nozzles 249a and 249b are provided in the processing chamber 201 so as to penetrate the lower side wall of the reaction tube 203. The nozzles 249a and 249b are connected to the gas supply pipes 232a and 232b, respectively.

[0026] In the gas supply pipes 232a and 232b, mass flow controllers (MFCs) 241a and 241b as flow controllers (flow control units) and valves 243a and 243b as opening and closing valves are respectively provided in order from the upstream side of the gas flow. A gas supply pipe 232c is connected to the gas supply pipe 232a at a downstream side of the valve 243a. Gas supply pipes 232d and 232e are respectively connected to the gas supply pipe 232b at a downstream side of the valve 243b. In the gas supply pipes 232c, 232d, and 232e, MFCs 241c, 241d, and 241e and valves 243c, 243d, and 243e are respectively provided in order from the upstream side of the gas flow.

[0027] like Figure 2 As shown, the nozzles 249a and 249b are respectively arranged in a circular ring-shaped space between the inner wall of the reaction tube 203 and the wafer 200 in a top view, so as to stand up from the lower part of the inner wall of the reaction tube 203 along the upper part toward the arrangement direction of the wafer 200. That is, the nozzles 249a and 249b are respectively arranged along the wafer arrangement area in the area on the side of the wafer arrangement area where the wafers 200 are arranged and horizontally surround the wafer arrangement area. Gas supply holes 250a and 250b for supplying gas are respectively provided on the side of the nozzles 249a and 249b. The gas supply holes 250a and 250b are respectively opened in a manner toward the center of the reaction tube 203, and can supply gas toward the wafer 200. A plurality of gas supply holes 250a and 250b are provided from the lower part to the upper part of the reaction tube 203.

[0028] A raw material gas including a predetermined element, carbon (C), and hydrogen (H) is supplied into the processing chamber 201 from the gas supply pipe 232 a via the MFC 241 a , the valve 243 a , and the nozzle 249 a .

[0029] In this specification, raw material gas refers to a raw material in a gaseous state, for example, a gas obtained by gasifying a raw material in a liquid state at normal temperature and pressure, a raw material in a gaseous state at normal temperature and pressure, etc. When the term "raw material" is used in this specification, there are cases where it means "liquid raw material in a liquid state", cases where it means "raw material gas in a gaseous state", or cases where it means both.

[0030] A first modifying agent including nitrogen (N) is supplied from the gas supply pipe 232b via the MFC 241b, the valve 243b, and the nozzle 249b into the processing chamber 201. The first modifying agent may also be referred to as a first modifying gas or a first nitriding agent.

[0031] The term "agent" used in this specification includes at least one of a gaseous substance and a liquid substance. A liquid substance includes a mist substance. That is, a film-forming agent, a modifier, or an etching agent may include a gaseous substance, a liquid substance such as a mist substance, or both.

[0032] Inert gas is supplied from gas supply pipes 232c and 232d into the processing chamber 201 via MFCs 241c and 241d, valves 243c and 243d, gas supply pipes 232a and 232b, and nozzles 249a and 249b. The inert gas functions as a purge gas, a carrier gas, a dilution gas, and the like.

[0033] A second modifier different from the first modifier and having higher reactivity than the first modifier is supplied from the gas supply pipe 232e via the MFC 241e, the valve 243e, the gas supply pipe 232b, and the nozzle 249b into the processing chamber 201. The second modifier can also be called a second modifying gas or a second nitriding agent.

[0034] The raw material gas supply system (raw material supply system) for supplying raw material gas is mainly composed of the gas supply pipe 232a, MFC241a, and valve 243a. The first modifier supply system (first modified gas supply system, first nitriding agent supply system) for supplying the first modifier is mainly composed of the gas supply pipe 232b, MFC241b, and valve 243b. The inert gas supply system for supplying inert gas is mainly composed of the gas supply pipes 232c, 232d, MFC241c, 241d, valves 243c, 243d. The second modifier supply system (second modified gas supply system, second nitriding agent supply system) for supplying the second modifier is mainly composed of the gas supply pipe 232e, MFC241e, and valve 243e.

[0035] Any one or all of the various supply systems described above may also be configured as an integrated supply system 248 that integrates valves 243a to 243e, MFCs 241a to 241e, etc. The integrated supply system 248 is connected to the gas supply pipes 232a to 232e, respectively, and the supply operation of various gases in the gas supply pipes 232a to 232e, that is, the opening and closing operation of the valves 243a to 243e, the flow rate adjustment operation of the MFCs 241a to 241e, etc., is controlled by the controller 121 described later. The integrated supply system 248 is configured as an integrated unit of an integral type or a split type, and can be loaded and unloaded relative to the gas supply pipes 232a to 232e, etc. as an integrated unit, and the integrated supply system 248 can be maintained, replaced, and added as an integrated unit.

[0036] An exhaust pipe 231 for exhausting the atmosphere in the processing chamber 201 is connected to the lower side wall of the reaction tube 203. The exhaust pipe 231 is connected to a vacuum pump 246 as a vacuum exhaust device via a pressure sensor 245 as a pressure detector (pressure detection unit) for detecting the pressure in the processing chamber 201 and an APC (Auto Pressure Controller) valve 244 as a pressure regulator (pressure adjustment unit). The APC valve 244 is configured to open and close the valve while the vacuum pump 246 is in operation, so that the vacuum exhaust in the processing chamber 201 and the vacuum exhaust stop can be performed. Furthermore, the pressure in the processing chamber 201 can be adjusted by adjusting the valve opening according to the pressure information detected by the pressure sensor 245 while the vacuum pump 246 is in operation. The exhaust system is mainly composed of the exhaust pipe 231, the pressure sensor 245, and the APC valve 244. The vacuum pump 246 can also be included in the exhaust system.

[0037] A sealing cover 219 as a furnace port cover that can hermetically seal the lower end opening of the reaction tube 203 is provided below the reaction tube 203. The sealing cover 219 is made of a metal material such as SUS and is formed into a disc shape. An O-ring 220 as a sealing member that abuts against the lower end of the reaction tube 203 is provided on the upper surface of the sealing cover 219. A rotating mechanism 267 for rotating the wafer boat 217 described later is provided below the sealing cover 219. The rotating shaft 255 of the rotating mechanism 267 passes through the sealing cover 219 and is connected to the wafer boat 217. The rotating mechanism 267 is configured to rotate the wafer 200 by rotating the wafer boat 217. The sealing cover 219 is configured to be lifted and lowered in the vertical direction by the wafer boat elevator 115 as a lifting mechanism provided outside the reaction tube 203. The boat elevator 115 is configured as a transport device (transport mechanism) that carries the wafer 200 in and out (transports) the wafer 200 in and out of the processing chamber 201 by raising and lowering the sealing cap 219 .

[0038] The wafer boat 217 as a substrate support is configured to support multiple wafers 200, for example, 25 to 200 wafers 200, in a horizontal posture and arranged in a vertical direction in a state where the centers are aligned with each other, that is, arranged at intervals. The wafer boat 217 is made of a heat-resistant material such as quartz or SiC. At the bottom of the wafer boat 217, a heat insulation plate 218 made of a heat-resistant material such as quartz or SiC is supported in multiple layers in a horizontal posture.

[0039] A temperature sensor 263 as a temperature detector is provided in the reaction tube 203. By adjusting the power supply to the heater 207 based on the temperature information detected by the temperature sensor 263, the temperature in the processing chamber 201 has a desired temperature distribution. The temperature sensor 263 is provided along the inner wall of the reaction tube 203.

[0040] like Figure 3 As shown, the controller 121 as a control unit (control unit) is configured as a computer having a CPU (Central Processing Unit) 121a, a RAM (Random Access Memory) 121b, a storage device 121c, and an I / O port 121d. The RAM 121b, the storage device 121c, and the I / O port 121d are configured to be able to exchange data with the CPU 121a via an internal bus 121e. The controller 121 is connected to an input-output device 122 such as a touch panel. In addition, an external storage device 123 can be connected to the controller 121. In addition, the substrate processing device can be configured to have one control unit or multiple control units. That is, for the control of the processing sequence described later, one control unit can be used or multiple control units can be used. In addition, the multiple control units can be configured as a control system interconnected by a wired or wireless communication network, or the control system as a whole can be used to control the processing sequence described later. When the term "control unit" is used in this specification, it may include not only one control unit but also a plurality of control units and a control system including a plurality of control units.

[0041] The storage device 121c is composed of, for example, a flash memory, a HDD (Hard Disk Drive), etc. A control program for controlling the actions of the substrate processing device, and a process recipe that records the process, conditions, etc. of the substrate processing process described later are stored in a readable manner in the storage device 121c. The process recipe is a combination of processes that enable the controller 121 to execute each process in the substrate processing process described later to obtain a specified result, and functions as a program. Hereinafter, process recipes, control programs, etc. are also collectively referred to as programs. In addition, process recipes are also collectively referred to as processes. When the term "program" is used in this specification, there is a case where only a process body is included, a case where only a control program body is included, or a case where both are included. RAM121b is configured as a storage area (work area) for temporarily holding programs, data, etc. read out by CPU121a.

[0042] The I / O port 121 d is connected to the above-mentioned MFCs 241 a to 241 e , valves 243 a to 243 e , pressure sensor 245 , APC valve 244 , vacuum pump 246 , temperature sensor 263 , heater 207 , rotation mechanism 267 , boat elevator 115 , and the like.

[0043] The CPU 121a is configured to read out a control program from the storage device 121c and execute it, and to read out a recipe from the storage device 121c according to input of an operation command from the input / output device 122. The CPU 121a is configured to control, according to the contents of the read recipe, flow rate adjustment operations of various gases by the MFCs 241a to 241e, opening and closing operations of the valves 243a to 243e, opening and closing operations of the APC valve 244 and pressure adjustment operations of the APC valve 244 by the pressure sensor 245, start and stop of the vacuum pump 246, temperature adjustment operations of the heater 207 by the temperature sensor 263, rotation of the wafer boat 217 by the rotation mechanism 267 and rotation speed adjustment operations, and lifting and lowering operations of the wafer boat 217 by the wafer boat elevator 115.

[0044] The controller 121 can be configured by installing the above-mentioned program stored in the external storage device 123 on a computer. The external storage device 123 includes, for example, a disk such as an HDD, an optical disk such as a CD, an optical magneto-optical disk such as an MO, a semiconductor memory such as a USB memory, etc. The storage device 121c and the external storage device 123 are configured as a computer-readable recording medium that records the program. Hereinafter, they are also collectively referred to as recording media. In the case where the term recording medium is used in this specification, there is a case where only the storage device 121c monomer is included, a case where only the external storage device 123 monomer is included, or a case where both are included. In addition, the provision of the program to the computer can also be carried out without using the external storage device 123, but using a communication unit such as the Internet or a dedicated line.

[0045] (2) Substrate processing steps

[0046] Main Use Figure 4 , Figure 5 The following example is described: using the processing furnace 202 of the above-mentioned substrate processing apparatus, as one process of manufacturing a semiconductor device, a process of forming a first film containing a predetermined element, N, C, and H bonded to C on a wafer 200 having a silicon film (Si film) formed on the surface, and a process of modifying the first film into a second film containing the predetermined element, C, and N in which the content ratio of H bonded to C is reduced compared to the first film. In the following description, the operation of each unit constituting the substrate processing apparatus can be controlled by the controller 121.

[0047] The term "wafer" used in this specification may refer to the wafer itself or a stack of a wafer and a predetermined layer or film formed on the surface thereof. The term "surface of the wafer" used in this specification may refer to the surface of the wafer itself or the surface of a predetermined layer, etc. formed on the wafer. When the term "a predetermined layer is formed on the wafer" is stated in this specification, it may refer to directly forming the predetermined layer on the surface of the wafer itself or to forming the predetermined layer on the layer, etc. formed on the wafer. The use of the term "substrate" in this specification is also synonymous with the use of the term "wafer".

[0048] [First film forming step (also referred to as film forming step)]

[0049] (Wafer loading and wafer boat loading, step S11)

[0050] A plurality of wafers 200 are loaded (wafer loading) into the wafer boat 217. Then, as Figure 1As shown, the boat 217 supporting the plurality of wafers 200 is lifted by the boat elevator 115 and carried into the processing chamber 201 (boat loading). In this state, the sealing cap 219 seals the lower end of the reaction tube 203 via the O-ring 220 .

[0051] (Pressure adjustment and temperature adjustment, step S12)

[0052] The vacuum pump 246 performs vacuum exhaust (decompression exhaust) so that the pressure in the processing chamber 201, that is, the pressure of the space where the wafer 200 exists, becomes the desired pressure (vacuum degree). At this time, the pressure in the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 244 is feedback-controlled based on the measured pressure information. The vacuum pump 246 is maintained in a state of always operating at least until the processing of the wafer 200 is completed. In addition, the heater 207 performs heating so that the wafer 200 in the processing chamber 201 reaches the desired temperature. At this time, the power supply to the heater 207 is feedback-controlled based on the temperature information detected by the temperature sensor 263 so that the processing chamber 201 has the desired temperature distribution. The heating in the processing chamber 201 based on the heater 207 is continuously performed at least until the processing of the wafer 200 is completed. In addition, the rotation of the wafer boat 217 and the wafer 200 based on the rotation mechanism 267 is started. The rotation of the wafer boat 217 and the wafers 200 by the rotation mechanism 267 is continuously performed at least until the processing of the wafers 200 is completed.

[0053] (Pre-flow Gas Supply, Step S13)

[0054] First, a pre-flow gas is supplied to the wafer 200 in the processing chamber 201. As the pre-flow gas, a first modifier as a gas containing N can be used. The details of the first modifier will be described later. Regarding this step, in the step S15 described later, it is performed as a pre-flow for making the raw material gas easily adsorbed on the surface of the wafer 200. Specifically, the valve 243b is opened to allow the first modifier to flow into the gas supply pipe 232b. The first modifier is flow-regulated by MFC241b, supplied into the processing chamber 201 via the nozzle 249b, and discharged from the exhaust pipe 231. At this time, the valve 243d is opened at the same time to allow the inert gas to flow into the gas supply pipe 232d. The inert gas is flow-regulated by MFC241d, supplied into the processing chamber 201 together with the first modifier, and discharged from the exhaust pipe 231.

[0055] In order to prevent the first modifying agent from entering the nozzle 249a, the valve 243c is opened to allow the inert gas to flow into the gas supply pipe 232c. The inert gas is supplied into the processing chamber 201 through the gas supply pipe 232a and the nozzle 249a, and is exhausted from the exhaust pipe 231.

[0056] By supplying a gas containing, for example, a hydrogen nitride compound as a pre-flow gas to the wafer 200, the natural oxide layer on the wafer 200 is nitrided, and NH terminals are formed on the wafer 200. As a result, the density of NH terminals on the surface of the wafer 200, which serve as adsorption sites for the raw material, can be increased, forming a uniform adsorption surface and improving the film formation rate. A preferred example of the pre-flow gas used in this step will be described later.

[0057] As the inert gas, in addition to nitrogen (N 2 ) gas, rare gases such as argon (Ar) gas, helium (He) gas, neon (Ne) gas, and xenon (Xe) gas can be used. As the inert gas, one or more of these can be used.

[0058] (Residual gas removal, step S14)

[0059] Next, the residual gas in the processing chamber 201 is removed. Specifically, after the NH terminus is formed on the surface of the wafer 200, the valve 243b is closed to stop the supply of the first modifier. At this time, the APC valve 244 remains open, and the processing chamber 201 is evacuated by the vacuum pump 246 to remove the first modifier and byproducts that remain in the processing chamber 201 and are not reacted or help form the NH terminus. In this case, the valves 243c and 243d remain open to maintain the supply of inert gas to the processing chamber 201. The inert gas acts as a purge gas.

[0060] Thereafter, the following steps S15 to S19 are executed in sequence.

[0061] (Raw material gas supply, step S15)

[0062] In this step, the raw material gas is supplied to the processing chamber 201. Specifically, while the APC valve 244 is opened to a predetermined opening, the valve 243a is opened to allow the raw material gas to flow into the gas supply pipe 232a. The raw material gas is flow-regulated by the MFC 241a, supplied from the gas supply hole 250a to the processing chamber 201, and exhausted from the exhaust pipe 231. At this time, the raw material gas is supplied to the wafer 200. At this time, while the valve 243c is opened, the inert gas is flowed into the gas supply pipe 232c. The inert gas is flow-regulated by the MFC 241c, supplied to the processing chamber 201 together with the raw material gas, and exhausted from the exhaust pipe 231.

[0063] In order to prevent the source gas from entering the nozzle 249b, the inert gas is flowed into the gas supply pipe 232d with the valve 243d open. The inert gas is supplied into the processing chamber 201 through the gas supply pipe 232b and the nozzle 249b and exhausted from the exhaust pipe 231.

[0064] The processing conditions when supplying the raw material gas in this step are exemplified as follows:

[0065] Treatment temperature: 150-800°C, preferably 180-700°C, more preferably 400-700°C,

[0066] Processing pressure: 1-2666Pa, preferably 67-1333Pa,

[0067] Raw material gas supply flow rate: 1 to 2000 sccm, preferably 10 to 1000 sccm,

[0068] Raw material gas supply time: 1 to 120 seconds, preferably 1 to 60 seconds,

[0069] Inert gas supply flow rate: 100~10000sccm.

[0070] Furthermore, from the viewpoint of increasing the processing speed, it is particularly preferred that the processing temperature be substantially the same in any step of the first film forming step.

[0071] In addition, the expression of a numerical range such as "150-800°C" in the present disclosure indicates that the lower limit and the upper limit are included in the range. Therefore, for example, "150-800°C" means "above 150°C and below 800°C". The same applies to other numerical ranges. The processing temperature in the present disclosure means the temperature of the wafer 200 or the temperature in the processing chamber 201, and the processing pressure means the pressure in the processing chamber 201. In addition, the processing time means the time for which the processing continues. This also applies to the following description.

[0072] If the temperature of the wafer 200 is lower than 150°C, it is difficult for the raw material to be chemically adsorbed on the wafer 200, and sometimes a practical film formation rate cannot be obtained. This can be eliminated by setting the temperature of the wafer 200 to 150°C or higher. By setting the temperature of the wafer 200 to 180°C or higher, the raw material can be sufficiently adsorbed on the wafer 200, and a sufficient film formation rate can be obtained. By setting the temperature of the wafer 200 to 400°C or higher, the raw material can be more sufficiently adsorbed on the wafer 200, and a more sufficient film formation rate can be obtained.

[0073] If the temperature of the wafer 200 exceeds 800°C, the CVD reaction becomes stronger (the gas phase reaction becomes dominant), and thus the film thickness uniformity is easily deteriorated, and its control becomes difficult. By setting the temperature of the wafer 200 to below 800°C, the deterioration of the film thickness uniformity can be suppressed and its control can be performed. By setting the temperature of the wafer 200 to below 700°C, the surface reaction becomes dominant, and it is easy to ensure the uniformity of the film thickness, and its control becomes easy.

[0074] That is, by setting the temperature of the wafer 200 in this process to 150 to 800° C., for example, the raw material can be adsorbed on the wafer 200, the film formation rate can be increased, and the film thickness uniformity can be improved. In addition, the generation of excessive gas phase reactions can be suppressed, and the generation of particles caused by the reaction can be suppressed.

[0075] By supplying a raw material gas to the wafer 200, a first layer containing, for example, a predetermined element, C, and H with a thickness ranging from less than 1 atomic layer to several atomic layers is formed as the first layer on the wafer 200 having NH terminals formed on the surface. That is, when a gas containing Si, C, and H as the predetermined elements is used as the raw material gas, the first layer contains H from the raw material in addition to the Si-C bond. H in the first layer forms bonds such as a CH bond and a Si-H bond. The Si-containing layer containing C and H becomes a layer containing Si-C bonds, Si-H bonds, and CH bonds. The Si-containing layer containing C and H may be a Si layer containing C and H, may be an adsorption layer of the raw material gas, or may contain both.

[0076] The Si layer containing C and H is a general term for a Si thin film containing C and H formed by overlapping a discontinuous Si layer in addition to a continuous Si layer containing C and H. The continuous Si layer containing C and H is sometimes referred to as a Si thin film containing C and H. The Si constituting the Si layer containing C and H includes not only a portion in which the bonds with C and H are not completely disconnected, but also a portion in which the bonds with C and H are completely disconnected.

[0077] The adsorption layer of the raw material gas includes a discontinuous adsorption layer in addition to a continuous adsorption layer of molecules of the raw material gas, that is, the adsorption layer of the raw material gas includes an adsorption layer having a thickness of one molecular layer or less than one molecular layer composed of molecules constituting the raw material gas.

[0078] Here, a layer with a thickness of less than 1 atomic layer means an atomic layer formed discontinuously, and a layer with a thickness of 1 atomic layer means an atomic layer formed continuously. A layer with a thickness of less than 1 molecular layer means a molecular layer formed discontinuously, and a layer with a thickness of 1 molecular layer means a molecular layer formed continuously.

[0079] Under the condition that the raw material gas self-decomposes (e.g., thermal decomposition), a Si layer containing C and H is formed by depositing, for example, Si on the wafer 200. Under the condition that the raw material gas does not self-decompose, the raw material gas is adsorbed on the wafer 200, thereby forming an adsorption layer of the raw material gas. Regardless of the conditions, at least a portion of the Si-C bond, Si-H bond, CH bond, etc. in the raw material gas is not cut but maintained (maintained) and directly taken into the Si-containing layer containing C and H.

[0080] As the raw material gas, a gas containing a predetermined element, C, and H can be used. As the gas containing the predetermined element, C, and H, for example, a gas containing Si, C, and H as the predetermined element can be used. As the gas containing Si, C, and H, for example, a gas containing a hydrocarbon group such as an alkylsilane gas or an alkylenesilane gas, that is, a compound containing a CH bond can be used.

[0081] In addition, as the gas containing the prescribed element, C and H, a gas containing the prescribed element, C, H and a halogen element can be used. As the gas containing the prescribed element, C, H and a halogen element, for example, a gas containing Si, C, H as the prescribed element and chlorine (Cl) as the halogen element can be used. As the gas containing Si, C, H and Cl, for example, an alkylene halosilane gas containing Si, an alkylene group and a halogen group and having a chemical bond between Si and C (Si-C bond) or an alkyl halosilane gas containing Si, an alkyl group and a halogen group and having a Si-C bond can be used.

[0082] Here, alkylene refers to n H 2n+2 The functional group after removing two hydrogen atoms from the chain saturated hydrocarbon (alkane) shown in the figure is the general formula C n H 2n The alkylene group includes methylene, ethylene, propylene, butylene, etc. In addition, the alkyl group is a group consisting of the general formula C n H 2n+2 The functional group after removing one hydrogen from the chain saturated hydrocarbon shown is the general formula C n H 2n+1 The alkyl group includes a methyl group, an ethyl group, a propyl group, a butyl group, etc. In addition, the halogen group includes a chlorine group, a fluorine group, a bromine group, etc. That is, the halogen group includes halogen elements such as chlorine (Cl), fluorine (F), and bromine (Br).

[0083] As the alkylene halosilane gas, for example, a gas containing Si, a methylene group (-CH2-) as an alkylene group, and a chloro group (Cl) as a halogen group, that is, a chlorosilane gas containing a methylene group, and a gas containing Si, an ethylene group (-C2H4-) as an alkylene group, and a chloro group (Cl) as a halogen group, that is, a chlorosilane gas containing an ethylene group can be used. As the chlorosilane gas containing a methylene group, for example, a methylenebis(trichlorosilane) gas, that is, a bis(trichlorosilyl)methane ((SiCl3)2CH2, abbreviated as: BTCSM) gas, etc. can be used. As the chlorosilane gas containing an ethylene group, for example, an ethylenebis(trichlorosilane) gas, that is, a 1,2-bis(trichlorosilyl)ethane ((SiCl3)2C2H4, abbreviated as: BTCSE) gas, etc. can be used.

[0084] As the alkyl halosilane gas, for example, a gas containing Si, a methyl group (-CH3) as an alkyl group, and a chlorine group (Cl) as a halogen group, that is, a chlorosilane gas containing a methyl group can be used. As the chlorosilane gas containing a methyl group, for example, 1,1,2,2-tetrachloro-1,2-dimethyldisilane ((CH3)2Si2Cl4, abbreviated as: TCDMDS) gas, 1,2-dichloro-1,1,2,2-tetramethyldisilane ((CH3)4Si2Cl2, abbreviated as: DCTMDS) gas, 1-monochloro-1,1,2,2,2-pentamethyldisilane ((CH3)5Si2Cl, abbreviated as: MCPMDS) gas, etc. can be used. Unlike alkylene halosilane gases such as BTCSE gas and BTCSM gas, TCDMDS gas, etc., alkyl halosilane gases such as DCTMDS gas and MCPMDS gas are also gases having Si-Si bonds, that is, raw material gases containing a predetermined element and a halogen element and having chemical bonds between the predetermined elements.

[0085] Alkyl halosilane gases such as BTCSM gas and BTCSE gas, and alkyl halosilane gases such as TCDMDS gas, DCTMDS gas, and MCPMDS gas can also be said to be raw gas containing at least 2 Si in one molecule, and further containing Cl, and having Si-C bonds and CH bonds. These gases act as Si sources and also as C sources in this process. BTCSM gas, BTCSE gas, etc. can also be called alkyl chlorosilane gas. TCDMDS gas, DCTMDS gas, MCPMDS gas, etc. can also be called alkyl chlorosilane gas.

[0086] When a gas containing a predetermined element, C, H, and a halogen element is used as a raw material gas, the first layer may contain a halogen element derived from the raw material gas as an impurity in addition to the predetermined element, C, and H. For example, when Cl is contained as a halogen element in the raw material gas, a bond such as a Si-Cl bond is also contained in the first layer.

[0087] (Residual gas removal, step S16)

[0088] Next, the residual gas in the processing chamber 201 is removed. Specifically, after the first layer is formed, the valve 243a is closed to stop the supply of the raw material gas. At this time, the APC valve 244 remains open, and the processing chamber 201 is evacuated by the vacuum pump 246 to remove the raw material gas and by-products that remain in the processing chamber 201 and that have not reacted or contributed to the formation of the first layer from the processing chamber 201. At this time, the valves 243c and 243d remain open to maintain the supply of the inert gas into the processing chamber 201. The inert gas acts as a purge gas.

[0089] (Supply of first modifying agent, step S17)

[0090] Next, the first modifying agent is supplied to the wafer 200 in the processing chamber 201 .

[0091] Specifically, similarly to the above-mentioned step S13, the valve 243b is opened to allow the first modifier to flow into the gas supply pipe 232b. The first modifier is flow-regulated by the MFC 241b, supplied into the processing chamber 201 via the nozzle 249b, and discharged from the exhaust pipe 231. At this time, while the valve 243d is opened, the inert gas is flowed into the gas supply pipe 232d. The inert gas is flow-regulated by the MFC 241d, supplied into the processing chamber 201 together with the first modifier, and discharged from the exhaust pipe 231.

[0092] In order to prevent the first modifying agent from entering the nozzle 249a, the inert gas is flowed into the gas supply pipe 232c with the valve 243c opened. The inert gas is supplied into the processing chamber 201 through the gas supply pipe 232a and the nozzle 249a and exhausted from the exhaust pipe 231.

[0093] As the treatment conditions when the first modifying agent is supplied in this step, the following are exemplified:

[0094] Processing pressure: 1-4000Pa, preferably 10-1000Pa,

[0095] First modifier supply flow rate: 0.1-20slm, preferably 1-10slm,

[0096] First modifier supply time: 1 to 120 seconds, preferably 10 to 60 seconds,

[0097] Inert gas supply flow rate: 0~10slm.

[0098] The other processing conditions may be the same as those when the raw material gas is supplied in the raw material gas supply step.

[0099] As the first modifier, a N-containing gas can be used. As the N-containing gas, for example, nitrogen (N2) gas, ammonia (NH3) gas, diazine (N2H2) gas, hydrazine (N2H4) gas, N3H5 gas and other hydrogen nitride gases can be used. As the N-containing gas, one or more of them can be used.

[0100] In addition, as described later, in this step, as the first modifier, it is preferred to use a gas containing a nitride-based compound that contains N and does not contain a bond between N atoms, i.e., a N-N bond, in one molecule. As the gas containing a nitride-based compound that contains N and does not contain a bond between N atoms, i.e., a N-N bond, in one molecule, for example, NH3 gas can be used.

[0101] In addition, the first modifier used in the above-mentioned pre-flow gas supply step S13 may be a modifier different from the first modifier used in this step. For example, in the pre-flow gas supply step, a gas containing a nitride-based compound containing N and a bond between N in one molecule, i.e., an N-N bond, may be used, and in this step, a gas containing a nitride-based compound containing N and not containing a bond between N in one molecule, i.e., an N-N bond, may be used. For example, in the pre-flow gas supply step, the second modifier described later may be supplied as the pre-flow gas.

[0102] By supplying the first modifier containing N to the wafer 200, at least a portion of the first layer formed on the wafer 200 is nitrided (modified). By modifying the first layer, in addition to, for example, Si-C bonds, Si-N bonds, and CN bonds, a second layer containing impurities such as H and Cl remaining in the first layer is formed. H in the second layer forms bonds such as CH bonds, Si-H bonds, and NH bonds. That is, by using the first modifier, the first layer containing the specified elements, C, and H is modified into a second layer containing the specified elements, C, H, and N, forming, for example, a silicon carbonitride layer (SiCN layer).

[0103] Here, by supplying the first modifier, a part of H and Cl in the first layer is desorbed, but H and Cl exceeding the desired concentration remain in the second layer. Impurities such as H and Cl exceeding the desired concentration remain in the film, thereby sometimes reducing the film density and the ashing resistance.

[0104] In addition, in this step, when a gas containing a highly reactive hydrogen nitride compound or a derivative thereof such as a second modifier described in detail later is used, during the period when the nitridation reaction is carried out until the N concentration in the first layer reaches the desired concentration, C in the first layer may be excessively separated. That is, it is sometimes impossible to maintain the C concentration in the second layer at the desired concentration. Therefore, as the first modifier in this step, it is preferable to use a gas containing a low-reactive hydrogen nitride compound. As a gas containing a low-reactive hydrogen nitride compound, a gas containing a hydrogen nitride compound that contains N and does not contain a bond between Ns, i.e., a N-N bond, in one molecule can be used as described above.

[0105] In addition, when the first modifier is activated by heat in a non-plasma environment and supplied, the above reaction can be performed gently, and the formation of the second layer becomes easy. When the second layer is formed, impurities such as Cl contained in the first layer constitute a gaseous substance containing at least Cl during the modification reaction of the first layer by the first modifier, and are discharged from the processing chamber 201. That is, impurities such as Cl in the first layer are extracted or separated from the first layer, thereby separating from the first layer. As a result, the second layer becomes a layer with less impurities such as Cl than the first layer.

[0106] (Residual gas removal, step S18)

[0107] Next, the residual gas in the processing chamber 201 is removed. Specifically, after the second layer is formed, the valve 243b is closed to stop the supply of the first modifier. At this time, the APC valve 244 remains open, and the processing chamber 201 is evacuated by the vacuum pump 246 to remove the first modifier and byproducts that remain in the processing chamber 201 and are not reacted or help form the second layer from the processing chamber 201. At this time, the valves 243c and 243d remain open to maintain the supply of the inert gas to the processing chamber 201. The inert gas acts as a purge gas.

[0108] (Implement the first specified number of times, step S19)

[0109] The cycle of performing the above steps S15 to S18 non-simultaneously is performed a first predetermined number of times (n times, n is an integer greater than 1). Thus, a first film containing a predetermined element, N, C, and H bonded to C (i.e., a C-H bond) can be formed on the wafer 200. The above cycle is preferably performed multiple times until the first film reaches a desired thickness. As the first film, for example, a silicon carbonitride film (SiCN film) containing Si, N, C, and a C-H bond can be formed.

[0110] At this time, the thickness of the first film is set to, for example, Preferably If the thickness of the first film is set to be less than Sometimes, a film having the desired properties cannot be obtained. In addition, if the thickness of the first film exceeds Sometimes, the modification effect of the modification step described later cannot be fully spread over the entire thickness direction of the first film. Hereinafter, the modification effect by the modification step described later can be brought about over the entire thickness direction of the first film. Thereby, the modification effect by the modification step described later can be more reliably brought about over the entire thickness direction of the first film.

[0111] Here, in addition to Si-C bonds, Si-N bonds, and CN bonds, the first film also contains impurities such as H and Cl remaining from the first layer. H in the first film forms bonds such as CH bonds, Si-H bonds, and NH bonds. In this way, if CH bonds, Si-H bonds, and NH bonds remain in the film, the ashing resistance deteriorates. However, in order to improve the ashing resistance, if it is desired to perform plasma treatment on the first film to remove impurities such as H and Cl, not only impurities such as H and Cl, but also C may be extracted from the film. Therefore, in this method, in order to suppress the extraction of C from the film and reduce impurities such as H and Cl, the next modification process is performed after the above-mentioned film forming process.

[0112] In this method, after the first film is formed by performing the above-mentioned film forming process (step S12 to step S19), the wafer 200 is not exposed to an oxygen-containing atmosphere, and the subsequent modification process (step S20 to step S22) is performed. After the first film is formed, when the wafer 200 is exposed to an oxygen-containing atmosphere, an oxide layer is sometimes formed on the surface of the first film. If an oxide layer is formed on the surface of the first film, the modification effect in the depth direction of the first film in the later-described step S21, that is, the effect of reducing H, etc., is hindered, and sometimes the modification effect cannot be fully obtained. That is, after the first film forming process is performed, the subsequent second film forming process is performed without being exposed to an oxygen-containing atmosphere, thereby improving the modification effect in step S21. That is, the subsequent second film forming process is performed in a state where no oxide layer is formed on the surface of the first film.

[0113] The second film forming process is performed after the first modifier is supplied in step S17 of the first film forming process, and then the residual gas is removed in step S18 to purge the space where the wafer 200 is located (also called inert gas purge). That is, the space where the wafer 200 is located is purged after the film forming process and before the modifying process. Thus, impurities such as Cl can be removed to some extent before the modifying process is performed.

[0114] [Second film forming step (also referred to as modification step)]

[0115] (Pressure adjustment and temperature adjustment, step S20)

[0116] The pressure in the processing chamber 201 is set to a desired pressure by performing vacuum exhaust by the vacuum pump 246. In addition, the wafer 200 in the processing chamber 201 is heated to a desired temperature by the heater 207.

[0117] (Second Modifying Agent Supply, Step S21)

[0118] Next, the second modifier is supplied to the wafer 200 on which the first film is formed. Specifically, the valve 243e is opened to allow the second modifier to flow into the gas supply pipe 232b. The second modifier is flow-regulated by the MFC 241e, supplied into the processing chamber 201 via the nozzle 249b, and discharged from the exhaust pipe 231. At this time, while the valve 243d is opened, an inert gas is flowed into the gas supply pipe 232d. The inert gas is flow-regulated by the MFC 241d, supplied into the processing chamber 201 together with the second modifier, and discharged from the exhaust pipe 231.

[0119] In order to prevent the second modifying agent from entering the nozzle 249a, the inert gas is flowed into the gas supply pipe 232c with the valve 243c opened. The inert gas is supplied into the processing chamber 201 through the gas supply pipe 232a and the nozzle 249a and exhausted from the exhaust pipe 231.

[0120] As the treatment conditions when the second modifying agent is supplied in this step, the following are exemplified:

[0121] Treatment temperature: room temperature to 700°C, preferably 150 to 700°C, more preferably 150 to 400°C,

[0122] Processing pressure: 1-2666Pa, preferably 67-1333Pa,

[0123] The second modifier supply flow rate: 1 to 2000 sccm, preferably 10 to 1000 sccm,

[0124] Second modifier supply time: 1 to 120 seconds, preferably 1 to 60 seconds,

[0125] Inert gas supply flow rate: 0~10000sccm.

[0126] However, from the viewpoint of increasing the processing speed, it is preferable to set the processing temperature in this step to substantially the same temperature as the processing temperature in the first film forming step.

[0127] If the temperature of the wafer 200 is lower than room temperature, the second modifier is hardly activated, and sometimes the modification effect cannot be fully obtained when modifying the first film. By setting the temperature of the wafer 200 to be higher than room temperature, the second modifier can be activated, and the modification effect can be brought about throughout the entire thickness direction of the first film. In addition, by setting the temperature of the wafer 200 to be higher than 150°C, the activation of the second modifier can be further promoted, and the modification effect can be brought about more reliably throughout the entire thickness direction of the first film.

[0128] If the temperature of the wafer 200 exceeds 700°C, the thermal decomposition of the second modifier proceeds excessively, and sometimes the modification effect on the first film cannot be obtained. For example, when N2H4 is used as the second modifier, due to its excessive thermal decomposition, sometimes NH3 with low reactivity is generated by the second modifier instead of NH2 as a highly reactive intermediate, and the modification effect on the first film cannot be obtained. In addition, if the temperature of the wafer 200 exceeds 400°C, the thermal decomposition of the second modifier proceeds partially, and for the same reason, the modification effect on the first film is sometimes reduced. By setting the temperature of the wafer to below 700°C, a modification effect can be obtained. In addition, by setting the temperature of the wafer 200 to below 400°C, a modification effect can be obtained more reliably.

[0129] By setting the temperature of the wafer 200 in this process to room temperature to 700°C, the reactivity of the second modifier can be easily controlled so that the second modifier or its intermediate reacts with H bonded to C in the first film, H bonded to Si, Cl bonded to Si, etc., and the detachment of H, Cl, etc. is suppressed while the detachment of C is suppressed.

[0130] In addition, by setting the temperature of the wafer 200 in this process to be lower than the temperature of the wafer 200 in the first film forming process described above, it is easy to adjust the degree of thermal decomposition and activation of the second modifier, and control the reactivity of the second modifier and / or its intermediate. Therefore, it is easier to control the reactivity of the second modifier so as to detach H bonded to C while suppressing the detachment of C from the first film. In addition, by performing this process at a lower temperature, the influence of the thermal history generated in this process on the wafer 200 can also be reduced. On the other hand, by setting the processing temperature to a temperature substantially the same as the processing temperature in the first film forming process, the processing speed of the wafer 200 can be increased.

[0131] At this time, the partial pressure of the second modifier is smaller than the partial pressure of the first modifier in the above step S17. In addition, at this time, the flow rate of the second modifier can also be smaller than the flow rate of the first modifier in the above step S17. Thereby, it is easy to control the reaction rate of the second modifier having a higher reactivity than the first modifier.

[0132] Here, when the first film is modified using the second modifying agent excited by plasma, the radicals and the like generated by the plasma excitation have excessively high reactivity, and thus, not only H bonded to C in the film by these radicals and the like, but also C bonded to N of a predetermined element is released. In the present disclosure, the second modifying agent having a higher reactivity than the first modifying agent is supplied to the wafer 200 in a non-plasma state. Thus, H and the like bonded to C can be selectively released while suppressing the release of C.

[0133] As the second modifying agent, a gas containing a hydrogen nitride-based compound or a derivative thereof containing a bond between N and H (ie, NH bond) and a bond between N atoms (ie, NN bond) in one molecule can be used.

[0134] As the second modifier, for example, a gas containing at least one compound selected from diazene (N2H2), hydrazine (N2H4), triazene (N3H3), triazine (N3H5), etc., which are nitride compounds containing NH bonds and NN bonds in one molecule, can be used. In addition, as the second modifier, for example, a gas containing derivatives such as monomethylhydrazine (CH3(NH)NH2), 1,1-dimethylhydrazine (asymmetric dimethylhydrazine) ((CH3)2-N-NH2), 1,2-dimethylhydrazine (tetramethylhydrazine) (N2(CH3)4), which are derivatives of nitride compounds containing NH bonds and NN bonds in one molecule, can be used. As the second modifier, one or more of them can be used.

[0135] (Residual Gas Removal, Step S22)

[0136] Next, the residual gas in the processing chamber 201 is removed. Specifically, after the first film is modified to form the second film, the valve 243e is closed to stop the supply of the second modifier. At this time, the APC valve 244 remains open, and the processing chamber 201 is evacuated by the vacuum pump 246 to remove the second modifier and byproducts that remain in the processing chamber 201 and are not reacted or contribute to the modification of the first film from the processing chamber 201. At this time, the supply of the inert gas to the processing chamber 201 is maintained while the valves 243c and 243d are open. The inert gas acts as a purge gas.

[0137] By supplying the second modifier to the wafer 200 in a non-plasma manner, at least a portion of the first film formed on the wafer 200 is nitrided (modified) and densified. By modifying the first film, a second film, i.e., a SiCN film, is formed on the wafer 200, for example, containing Si, C, and N. When the second modifier is activated and supplied by heat in a non-plasma, the above-mentioned reaction can be carried out gently, and the formation of the second film becomes easy. When the second film is formed, the impurities such as H and Cl contained in the first film constitute a gaseous substance containing at least H and Cl in this process and are discharged from the processing chamber 201. That is, for the CH bond, Si-H bond, NH bond, etc. in the first film, a second modifier with a higher reactivity than the above-mentioned first modifier is used to modify the first film. As a result, the intermediate of the second modifier reacts with the H and Cl of the CH bond, Si-H bond, NH bond, etc. in the first film, so that H and Cl are separated from the first film. That is, impurities such as H and Cl are removed while maintaining the C concentration in the first film within a desired range. In other words, the first film on the wafer 200 can be modified into a second film containing a predetermined element, C, and N, in which the content ratio of H bonded to C is reduced compared to the first film.

[0138] By reducing impurities such as H and Cl in the film, the ashing resistance of the film can be improved. In addition, by maintaining the C concentration in the film within a desired range, the etching resistance of the film can be improved. That is, by modifying the first film using the second modifier as described above, the first film can be modified into a second film that has both ashing resistance and etching resistance.

[0139] (Implement the second specified number of times, step S23)

[0140] In this step, when the cycle of steps S15 to S22 is performed non-simultaneously for less than the second predetermined number of times (m times, m is an integer greater than or equal to 1), the pressure in the processing chamber 201 and the wafer 200 in the processing chamber 201 are adjusted to the desired pressure and desired temperature in the first film forming step described above by the same process as the above-mentioned step S12 (step S24), and the process returns to the above-mentioned step S15. By performing the cycle including steps S15 to S22 for the second predetermined number of times, a film containing the predetermined elements, C and N having a desired film thickness can be formed on the wafer 200. That is, in this method, by performing the cycle including the film forming step (excluding the pre-flow gas supply step) and the modification step for the second predetermined number of times, a film containing the predetermined elements, C and N having a desired film thickness is formed on the wafer 200. In addition, the pre-flow gas supply step may be performed not only once before this cycle as in this method, but also in a cycle.

[0141] By performing steps S20 to S22 once each time the loop of performing steps S15 to S18 non-simultaneously described above is performed a plurality of times, the number of times steps S20 to S22 are performed can be reduced, thereby improving throughput.

[0142] Here, in this modification step (second film forming step), the first film is modified into the second film in such a manner that the amount of reduction in the content ratio of H contained in the first film is greater than the amount of reduction in the content ratio of C contained in the first film. That is, in this step, the first film is modified into the second film in such a manner that the amount of reduction in the content ratio of C in the first film is suppressed and the content ratio of H is reduced.

[0143] Figure 5 (A) in FIG. 1 is a diagram showing a state of the surface of the wafer 200 when NH 3 gas is supplied to the first film formed on the wafer 200 . Figure 5 (B) in FIG. 1 is a diagram showing a state of the surface of the wafer 200 when N 2 H 4 gas is supplied to the first film formed on the wafer 200 .

[0144] like Figure 5 As shown in (A), NH3 consists only of NH bonds with relatively large activation energy, so it is difficult to thermally decompose into highly reactive intermediates. In addition, the activation energy required for NH3 to react with each of the CH bonds, Si-H bonds, and Si-Cl bonds remaining in the first film is large, so it is difficult to produce a reaction that cuts these bonds. That is, NH3 has a weak effect on removing these bonds in the first film. For example, the activation energy (Ea(H)) required for NH3 to react with the Si-H bond contained in the first film to separate H is 1.95, and the activation energy (Ea(Cl)) required for NH3 to react with the Si-Cl bond to separate Cl is 1.33.

[0145] On the other hand, Figure 5 As shown in (B), N2H4 contains a NN bond with relatively low activation energy, and therefore, it is easy to thermally decompose into a highly reactive intermediate NH2. In addition, the intermediate NH2 contains N with a dangling bond, and therefore, the activation energy required to react with each of the CH bond, Si-H bond, and Si-Cl bond remaining in the first film is small, and it is easy to produce a reaction that cuts these bonds. That is, N2H4 (intermediate NH2) has a strong effect in removing these bonds in the first film. According to an example of the calculation results of molecular simulation performed by the publisher, the activation energy (Ea(H)) required for NH2 to react with the Si-H bond contained in the first film to dissociate H is 0.01, and the activation energy (Ea(Cl)) required to react with the Si-Cl bond to dissociate Cl is 0.16.

[0146] That is, the activation energy of NH2, an intermediate generated by decomposition of N2H4, as the second modifier, for reacting and releasing H bonded to C contained in the first film is smaller than the activation energy of NH3, as the first modifier, for releasing H bonded to C contained in the first film. That is, by reacting NH2, an intermediate of N2H4 having a higher reactivity than NH3, with H bonded to C in the first film, H can be released from the first film.

[0147] In addition, the activation energy of NH2 for causing Cl bonded to Si contained in the first film to react and desorb is smaller than the activation energy of NH3 for causing Cl bonded to Si contained in the first film to desorb. That is, by causing NH2, which is an intermediate of N2H4 having a higher reactivity than NH3, to react with Cl bonded to Si in the first film, etc., Cl can be desorbed from the first film.

[0148] That is, in this modification process, the first film is modified into the second film by using the second modifier to modify the first film in such a way as to reduce the content ratio of H bonded to a predetermined element, H bonded to C, H bonded to N, etc. contained in the first film. That is, the content ratio (concentration) of H bonded to Si, H bonded to C, H bonded to N, etc. in the first film is reduced. Specifically, by supplying the second modifier, the above-mentioned intermediate generated from the second modifier reacts with, for example, Si-H bonds, CH bonds, NH bonds, etc. contained in the first film, thereby causing H to be detached from the first film. By reducing the content ratio of H in the film, film properties such as ashing resistance can be improved.

[0149] In addition, in this process, the first film is modified into the second film in such a way that the halogen element such as Cl contained in the first film is separated. That is, the content ratio of Cl bonded to C, Cl bonded to Si, Cl bonded to N, etc. remaining in the first film is reduced. Specifically, by supplying the second modifier, the above-mentioned intermediate generated from the second modifier reacts with the C-Cl bond, Si-Cl bond, N-Cl bond, etc. contained in the first film, thereby separating Cl from the first film. By reducing the content ratio of halogen elements such as Cl in the film, film properties such as ashing resistance can be improved.

[0150] In addition, the H concentration contained in the first film before the modification process is, for example, 20 to 30 atomic%, and the H concentration contained in the second film after the modification process is, for example, 0 to 10 atomic%. When the H concentration contained in the second film exceeds 10 atomic%, ashing resistance within a practical range may not be obtained. By making the H concentration contained in the second film 10 atomic% or less, the ashing resistance of the second film in plasma ashing using oxygen (O2) plasma or the like can be improved to a practical range.

[0151] Here, the C concentration contained in the second film after the modification step is maintained in a desired range for maintaining etching resistance, for example, 5 to 30 atomic %, preferably 10 to 30 atomic %.

[0152] When the C concentration contained in the second film is less than 5 atomic%, the etching resistance is sometimes greatly reduced. By setting the C concentration contained in the second film to 5 atomic% or more, the etching resistance can be improved when the second film is wet-etched using, for example, a diluted hydrogen fluoride (HF) aqueous solution. In addition, by setting the C concentration contained in the second film to 10 atomic% or more, the etching resistance of the second film can be improved to a practical range.

[0153] In addition, when the C concentration contained in the second film exceeds 30 atomic %, etching resistance within a practical range may not be obtained. By setting the C concentration contained in the second film to 30 atomic % or less, the etching resistance of the second film can be improved to a practical range.

[0154] That is, according to this aspect, both the C concentration and the H concentration in the film can be modified to the above-mentioned desired ranges, and a film having both ashing resistance and etching resistance can be formed.

[0155] (Purge and atmospheric pressure recovery, step S25)

[0156] The valves 243c and 243d are opened, and inert gas is supplied from the gas supply pipes 232c and 232d to the processing chamber 201, respectively, and discharged from the exhaust pipe 231. The inert gas functions as a purge gas. Thus, the processing chamber 201 is purged, and the gas and by-products remaining in the processing chamber 201 are removed from the processing chamber 201 (purge). After that, the atmosphere in the processing chamber 201 is replaced with the inert gas (inert gas replacement), and the pressure in the processing chamber 201 is restored to normal pressure (atmospheric pressure recovery).

[0157] (Wafer boat unloading and wafer removal, step S26)

[0158] The sealing cover 219 is lowered by the wafer boat elevator 115, and the lower end of the reaction tube 203 is opened. Then, the processed wafers 200 are carried out from the lower end of the reaction tube 203 to the outside of the reaction tube 203 while being supported by the wafer boat 217 (wafer boat unloading). The processed wafers 200 are taken out from the wafer boat 217 (wafer taking out).

[0159] (3) Effects of this method

[0160] According to this aspect, one or more of the following effects can be obtained.

[0161] (a) Impurities such as H and Cl contained in the film are reduced, the film density is high, and a film excellent in ashing resistance can be formed.

[0162] (b) It is possible to form a film having excellent etching resistance while reducing impurities such as H and Cl while maintaining the C concentration contained in the film within a desired range.

[0163] (c) That is, the film formed on the wafer 200 can be modified to have both ashing resistance and etching resistance.

[0164] (d) The above-mentioned effects can also be obtained in the case of forming and modifying a CN-containing film other than a SiCN film.

[0165] <Other aspects of the present disclosure>

[0166] The embodiments of the present disclosure have been specifically described above. However, the present disclosure is not limited to the above embodiments, and various modifications can be made without departing from the gist of the present disclosure.

[0167] (Variation Example)

[0168] Next, use Figure 6 A modification of the above-mentioned substrate processing step will be described.

[0169] In this modified example, the film forming process includes a modification process. That is, after steps S31 to S38 are performed in the same manner as steps S11 to S18, steps S39 and S40 are performed, and the steps S39 and S40 are performed in the same manner as steps S21 and S22 in the modification process. Then, as step S41, the cycle of steps S35 to S40 is performed a third predetermined number of times (p times, where p is an integer greater than 1).

[0170] By performing the second cycle for a predetermined number of times, as with the second film described above, a third film of a desired thickness with reduced impurities such as H and Cl can be formed while maintaining the C concentration within a desired range. That is, in this modification, the same effect as in the above method can be obtained. In addition, in this modification, by further performing a modification treatment of forming the first film formed on the surface of the wafer 200 and removing H, Cl, etc., the density of NH terminals on the surface of the wafer 200 that serve as adsorption sites for the raw material can be increased, thereby increasing the formation speed of the first film, i.e., the film formation rate. In addition, the processing time can be shortened and the throughput can be improved.

[0171] (Other methods)

[0172] For example, in the above-mentioned method, the case where the prescribed element contained in the raw material gas is Si is used as an example for explanation. However, the present disclosure is not limited to such a method. For example, the prescribed element may also be a metal element such as titanium (Ti), zirconium (Zr), hafnium (Hf), tantalum (Ta), niobium (Nb), aluminum (Al), molybdenum (Mo), tungsten (W), germanium (Ge), etc. In these cases, a titanium carbonitride film (TiCN film), a zirconium carbonitride film (ZrCN film), a hafnium carbonitride film (HfCN film), a tantalum carbonitride film (TaCN film), a niobium carbonitride film (NbCN film), an aluminum carbonitride film (AlCN film), a molybdenum carbonitride film (MoCN film), a tungsten carbonitride film (WCN film), a germanium carbonitride film (GeCN film), and other metal carbonitride films are formed. In these cases, the same effect as in the above-mentioned method can also be obtained.

[0173] In addition, in the above-mentioned method, in the film forming process, the case where a first film including a specified element, N, C, and H bonded to C is formed on a wafer 200 having a Si film formed on the surface thereof is described, but the present disclosure is not limited to this. It can also be preferably used when an oxide film such as a silicon oxide film (SiO film) or a nitride film such as a silicon nitride film (SiN film) is formed on the surface thereof, or when a first film is formed on the surface of the wafer 200 itself.

[0174] In addition, in the above-mentioned method, the case where the first film forming process and the modification process are continuously performed (in-situ) in the same processing chamber 201 is used for explanation. The present invention is not limited to this, and the first film forming process and the modification process can also be performed separately in different processing chambers (processing containers) (in ex-situ). In this case, the same effect as the above-mentioned method is also obtained. In addition, when these processes are performed in an in-situ manner, it is possible to suppress the contamination of the substrate, the change of the surface state of the substrate, etc. that may be caused by the substrate being carried out of the processing room or carried in from the processing room between the processes. In addition, when these processes are performed in an in-situ manner, the migration time between the processes can be shortened. On the other hand, when these processes are performed in an ex-situ manner, each process can be performed in parallel in different processing chambers, and the productivity can be improved accordingly.

[0175] In addition, it is preferred that the process used for substrate processing is prepared individually according to the processing content, and is stored in the storage device 121c via the electrical communication line and the external storage device 123. And, it is preferred that when starting the substrate processing, the CPU 121a appropriately selects a suitable process from the multiple processes stored in the storage device 121c according to the processing content. Thus, a film of various film types, composition ratios, film qualities, and film thicknesses can be formed with good reproducibility using one substrate processing device. In addition, the burden on the operator can be reduced, operational errors can be avoided, and the substrate processing can be started quickly.

[0176] The above-mentioned process is not limited to the case of newly making, and can also be prepared by, for example, changing an existing process already installed in a substrate processing device. When changing a process, the changed process can also be installed in the substrate processing device via an electrical communication line or a recording medium recording the process. In addition, the input / output device 122 of the existing substrate processing device can also be operated to directly change the existing process already installed in the substrate processing device.

[0177] In the above-mentioned method, an example of using a batch-type substrate processing device that processes multiple substrates at a time to process a film is described. The present disclosure is not limited to the above-mentioned method, and for example, it can also be appropriately applied to the case where a single-piece substrate processing device that processes one or more substrates at a time is used to process a film. In addition, in the above-mentioned method, an example of using a substrate processing device with a hot-wall type processing furnace to process a film is described. The present disclosure is not limited to the above-mentioned method, and it can also be appropriately applied to the case where a substrate processing device with a cold-wall type processing furnace is used to process a film.

[0178] When these substrate processing apparatuses are used, film formation processing can be performed in the same processing procedures and processing conditions as those in the above-mentioned embodiment, and the same effects as those in the above-mentioned embodiment can be obtained.

[0179] In addition, the above-mentioned forms and modified examples can be used in combination as appropriate. The processing procedure and processing conditions in this case can be, for example, the same as the processing procedure and processing conditions of the above-mentioned forms and modified examples.

[0180] Description of Reference Numerals

[0181] 200 wafers (substrates).

Claims

1. A substrate processing method, characterized in that: The process is as follows: (a) forming a first film including a predetermined element, nitrogen, carbon, and hydrogen bonded to carbon on a substrate by performing a predetermined number of cycles, the cycle including a step of supplying a raw material including the predetermined element, carbon, and hydrogen to the substrate, and a step of supplying a first modifier including nitrogen to the substrate; and (b) The first film is modified into a second film containing the specified element, carbon and nitrogen and having a lower content ratio of hydrogen bonded to the carbon than that of the first film by supplying a second modifier different from the first modifier to the substrate on which the first film is formed, wherein the second modifier is a compound or a derivative thereof containing a bond between nitrogen and hydrogen and a bond between nitrogen in one molecule.

2. The substrate processing method according to claim 1, characterized in that: After (a), (b) is initiated without exposing the substrate to an oxygen-containing atmosphere.

3. The substrate processing method according to claim 1, characterized in that: In (b), the first film is modified so that the content ratio of the bonds between carbon and hydrogen is reduced throughout the entire thickness direction of the first film.

4. The substrate processing method according to claim 1, characterized in that: In (b), the first film is modified into the second film so that the amount of reduction in the content ratio of hydrogen contained in the first film is greater than the amount of reduction in the content ratio of carbon contained in the first film.

5. The substrate processing method according to claim 1, characterized in that: The cycle is performed multiple times until the first film has a desired thickness.

6. The substrate processing method according to claim 1, characterized in that: In (b), the second modifier is supplied to the substrate in a non-plasma state.

7. The substrate processing method according to claim 1, characterized in that: The first modifier does not contain any bond between nitrogen atoms in one molecule.

8. The substrate processing method according to claim 7, characterized in that: The first modifier is a hydrogen nitride compound.

9. The substrate processing method according to claim 1, characterized in that: In (b), the intermediate containing nitrogen having a dangling bond in one molecule generated from the second modifier is reacted with hydrogen bonded to the carbon contained in the first film, thereby desorbing the hydrogen from the first film.

10. The substrate processing method according to claim 1, characterized in that: The activation energy of the intermediate generated by decomposition of the second modifier for desorption of hydrogen bonded to the carbon contained in the first film is smaller than the activation energy of the first modifier for desorption of hydrogen bonded to the carbon contained in the first film.

11. The substrate processing method according to any one of claims 1 to 10, characterized in that: The second modifier comprises at least one compound or derivative selected from the group consisting of diazene, hydrazine, triazene, triazine, monomethylhydrazine, 1,1-dimethylhydrazine, and 1,2-dimethylhydrazine.

12. The substrate processing method according to any one of claims 1 to 10, characterized in that: The raw material includes a compound containing the predetermined element, carbon, hydrogen, and a halogen element in one molecule, and in (b), the first film is modified into the second film in such a manner that the halogen element contained in the first film is removed.

13. The substrate processing method according to any one of claims 1 to 10, characterized in that: In (b), the first film is modified into the second film so that the content ratio of hydrogen bonded to the predetermined element contained in the first film is reduced.

14. The substrate processing method according to any one of claims 1 to 10, characterized in that: The partial pressure of the second modifier in (b) is less than the partial pressure of the first modifier in (a).

15. The substrate processing method according to any one of claims 1 to 10, characterized in that: The temperature of the substrate in (b) is lower than the temperature of the substrate in (a).

16. The substrate processing method according to any one of claims 1 to 10, characterized in that: After (a) and before (b), there is further included a step of purging the space where the substrate exists.

17. The substrate processing method according to any one of claims 1 to 10, characterized in that: The prescribed number of times is set to one, The second loop including (a) and (b) is executed multiple times.

18. A method for manufacturing a semiconductor device, characterized in that: The process is as follows: (a) forming a first film including a predetermined element, nitrogen, carbon, and hydrogen bonded to carbon on a substrate by performing a predetermined number of cycles, the cycle including a step of supplying a raw material including the predetermined element, carbon, and hydrogen to the substrate, and a step of supplying a first modifier including nitrogen to the substrate; and (b) A process of modifying the first film into a second film containing the specified element, carbon and nitrogen in which the content ratio of hydrogen bonded to the carbon is reduced compared to the first film by supplying a second modifier different from the first modifier to the substrate on which the first film is formed, wherein the second modifier is a compound or a derivative thereof that contains a bond between nitrogen and hydrogen and a bond between nitrogen in one molecule.

19. A computer-readable recording medium having a program recorded thereon, characterized in that: The program enables the substrate processing device to execute the following process through a computer: (a) forming a first film including a predetermined element, nitrogen, carbon, and hydrogen bonded to carbon on a substrate by performing a predetermined number of cycles, the cycle including a process of supplying a raw material including the predetermined element, carbon, and hydrogen to the substrate, and a process of supplying a first modifier including nitrogen to the substrate; as well as (b) by supplying a second modifier different from the first modifier to the substrate on which the first film is formed, the first film is modified into a second film containing the specified element, carbon and nitrogen, in which the content ratio of hydrogen bonded to the carbon is reduced compared to the first film, wherein the second modifier is a compound or a derivative thereof that contains bonds between nitrogen and hydrogen and bonds between nitrogen in one molecule.

20. A substrate processing device, characterized in that: have: a raw material supply system for supplying a raw material including a predetermined element, carbon and hydrogen to the substrate; a first modifier supply system for supplying a first modifier including nitrogen to the substrate; a second modifying agent supplying system for supplying a second modifying agent different from the first modifying agent to the substrate, the second modifying agent being a compound containing a bond between nitrogen and hydrogen and a bond between nitrogen in one molecule or a derivative thereof; and A control unit capable of controlling the raw material supply system, the first modifier supply system, and the second modifier supply system so as to perform the following processing: (a) forming a first film including the predetermined element, nitrogen, carbon, and hydrogen bonded to carbon on the substrate by performing a predetermined number of cycles, the cycle including a process of supplying the raw material to the substrate and a process of supplying the first modifier to the substrate; (b) supplying the second modifying agent to the substrate on which the first film is formed, thereby modifying the first film into a second film containing the predetermined element, carbon, and nitrogen and having a lower content ratio of hydrogen bonded to the carbon than that of the first film.