Colloidal electrolyte of silicon-based lithium ion battery as well as preparation method and application of colloidal electrolyte
By using the Py-BPy-Br colloidal electrolyte of covalent organic framework nanosheets in silicon-based lithium batteries, the deficiencies in fast charging and calendar life of silicon-based lithium-ion batteries are solved, and efficient lithium ion desolvation is achieved. and HF adsorption, significantly improving the cycle stability and life of the battery.
Patent Information
- Application Number
- CN202410857769.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
AI Technical Summary
Silicon-based lithium-ion batteries have shortcomings in fast charging and calendar life, mainly due to the low equilibrium potential of the graphite component leading to metallic lithium deposition and lithium ion desolvation kinetics at the liquid-solid interface, resulting in reduced cycle stability and safety issues. At the same time, the HF in the electrolyte corrodes the positive and negative electrodes, resulting in a short calendar life.
Covalent organic framework (COFs) nanosheets are used as the dispersion of the electrolyte, and the pyrene ring on the structure produces non-covalent interactions with lithium ions to change the solvation structure of lithium ions, and interacts with HF through pyridine. Suppress the corrosion of the positive and negative electrodes to form Py-BPy-Br colloidal electrolyte. The electrolyte is synthesized by a solvothermal method and dispersed in a commercial electrolyte for ultra-fast charging and long calendar life silicon-based lithium batteries.
It significantly improves the desolvation process of lithium ions and the fast charging performance of the battery. At the same time, it extends the calendar life of the battery through the adsorption of HF through the porous structure and high specific surface area, maintains cycle stability, and is suitable for large-scale production.
Smart Images

Figure CN118867367A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of silicon-based lithium-ion batteries, and in particular relates to a covalent organic framework colloid electrolyte for ultrafast charging and long calendar life silicon-based lithium batteries, and a preparation method and application thereof. Background Art
[0002] Power supply technology is of great significance in responding to the global energy crisis. It helps to efficiently utilize renewable but intermittent energy such as solar energy and wind energy, and ensure the stability and sustainability of energy supply. With the rapid development of society and economy, the demand for energy storage systems with high energy density has become more and more urgent to meet the growing energy demand. At present, lithium-ion batteries with graphite as negative electrodes can no longer meet the requirements of long battery life in application scenarios such as electric vehicles and portable electronic devices due to their low theoretical energy density. The development of battery systems with higher energy density has become an urgent need of today's society. Among them, silicon-based negative electrodes (theoretical specific capacity: 3592mAh g -1 ) due to its high specific capacity relative to graphite anode (theoretical specific capacity: 372 mAh g -1 ) has a higher theoretical specific capacity and has received extensive attention from academia and industry. However, silicon-based lithium-ion batteries still have problems such as poor fast charging capability and short calendar life.
[0003] Although the state-of-the-art commercial silicon-carbon (Si / C) anode has made significant progress, the goal of achieving fast charging remains elusive. On the one hand, the dominant graphite component (90-95%) in Si / C anode has a low equilibrium potential (~100 mV vs. Li / Li + ). Therefore, during fast charging, metallic lithium is easily deposited on the negative electrode surface, resulting in reduced cycle stability and safety issues. On the other hand, the sluggish desolvation kinetics of lithium ions at the liquid-solid interface hinders efficient lithium ion transport kinetics. The above two reasons lead to the poor fast charging performance of silicon-based lithium-ion batteries.
[0004] In silicon-based lithium-ion batteries, the main problem affecting the calendar life is that the HF in the electrolyte will corrode the positive electrode and the silicon-based negative electrode, resulting in the loss of active materials and significant deterioration of electrochemical performance. First, fluoroethylene carbonate (FEC), a commonly used electrolyte additive for silicon-based lithium-ion batteries, can form a strong and ideal solid electrolyte interphase (solid-state electrolyte interphase, SEI) on the silicon-based negative electrode, but FEC will also generate HF through defluorination. Secondly, trace water in the electrolyte reacts with PF6 - The reaction will also generate HF. Finally, the poor thermal stability of the electrolyte will cause FEC and PF6 -The above three reasons lead to the short calendar life of silicon-based lithium-ion batteries, which cannot meet the requirements of long-term static storage and operation of the batteries. Summary of the invention
[0005] In order to overcome the shortcomings and deficiencies of the above-mentioned prior art, the primary purpose of the present invention is to provide a covalent organic framework colloidal electrolyte for ultra-fast charging and long calendar life silicon-based lithium batteries, wherein the colloidal electrolyte uses covalent organic framework (COFs) nanosheets as dispersoids. The colloidal electrolyte provided by the present invention, in which the COFs nanosheets as dispersoids can utilize the pyrene rings in their structures to produce strong non-covalent interactions with lithium ions, thereby changing the solvation structure of lithium ions and promoting the desolvation process of lithium ions. On the other hand, the non-covalent interaction of pyridine on COFs with HF can inhibit the corrosion of HF to the positive and negative electrodes, thereby extending the calendar life of the battery.
[0006] Another object of the present invention is to provide a method for preparing the above-mentioned covalent organic framework colloidal electrolyte for ultra-fast charging and long calendar life silicon-based lithium batteries. The method first synthesizes a covalent organic framework material as a colloidal electrolyte dispersant by a solvothermal method. The method is applicable to all COFs synthesized with aldehyde monomers and amino monomers as raw materials, and the COFs synthesized by the method have a lateral / vertical size of less than 100nm, which is an ideal material for a colloidal electrolyte dispersant; then, the above-synthesized covalent organic framework material is used as a dispersant, and the covalent organic framework material is dispersed in a commercial electrolyte to obtain a covalent organic framework colloidal electrolyte that can be applied to ultra-fast charging and long calendar life lithium batteries.
[0007] Another object of the present invention is to provide the use of the above-mentioned covalent organic framework colloidal electrolyte for ultra-fast charging and long calendar life silicon-based lithium batteries in lithium batteries.
[0008] The purpose of the present invention is achieved through the following solutions:
[0009] A colloidal electrolyte for a silicon-based lithium battery is a colloidal electrolyte using covalent organic framework (COFs) nanosheets as a dispersant, and comprises a covalent organic framework material and a basic electrolyte.
[0010] The basic electrolyte is a lithium-ion battery electrolyte, preferably a commercial ester electrolyte, more preferably (0.5-6)M LiPF6-EC / EMC+(1-10)wt% FEC, wherein the mass ratio of EC to EMC in EC / EMC is 3:7 or 1:1;
[0011] The covalent organic framework material is a COFs synthesized with aldehyde monomers and amino monomers as raw materials, wherein the amino monomer is an amino monomer containing at least one of the functional groups such as pyrene ring, triazine, carbonyl, carboxyl, etc., and the aldehyde monomer is an aldehyde monomer containing at least one of the functional groups such as pyridine, furan, oxazole, imidazole, thiophene, etc. The covalent organic framework can produce non-covalent interactions with lithium ions, change the solvation structure of lithium ions, and improve the fast charging performance of the battery. On the other hand, the covalent organic framework can also produce non-covalent interactions with hydrofluoric acid, thereby improving the calendar life of the battery.
[0012] The covalent organic framework material can be designed according to the functionalization effect on the electrolyte, and the covalent organic framework material is preferably a structure shown in Formula I:
[0013]
[0014] The dosage of the covalent organic framework material and the basic electrolyte satisfies: the concentration of the covalent organic framework material in the basic electrolyte is 0.1-10 g / L.
[0015] A method for preparing a colloidal electrolyte for a silicon-based lithium battery, characterized by comprising the following steps:
[0016] The covalent organic framework material is uniformly dispersed in the basic electrolyte to obtain the colloidal electrolyte of the silicon-based lithium battery.
[0017] The uniform dispersion refers to dispersion by stirring and / or ultrasonication under the protection of argon atmosphere, preferably, the mixed solution is stirred for 1 to 3 hours and then ultrasonicated for 2 to 6 hours.
[0018] The obtained colloidal electrolyte was named Py-BPy-Br colloidal electrolyte (abbreviated as Py-BPy-Br CE).
[0019] The covalent organic framework material is prepared by the following method:
[0020] (1) Preparation of neutral COFs material: aldehyde monomer, amino monomer and solvent are mixed and stirred to obtain a mixed solution, argon is filled into the mixed solution, and the mixed solution is sealed and heated. After the reaction is completed, a neutral COFs material is obtained;
[0021] (2) Preparation of cationic COFs material: The neutral COFs material is dispersed in a dibromoethane / acetonitrile mixed solution, and the mixed solution is heated and stirred. After the reaction is completed, a cationic COFs material, i.e., a covalent organic framework material shown in Formula I, is obtained.
[0022] The aldehyde monomer described in step (1) is 2,2'-bipyridine-5,5'-dicarboxaldehyde (2,2'-BPy-DCA), and the amino monomer is 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene (Py-TA). The specific structure is shown below:
[0023]
[0024] The reaction molar ratio of the aldehyde monomer to the amino monomer in step (1) is 2:1.
[0025] The solvent described in step (1) is a mixed solvent of mesitylene / dioxane / 6M acetic acid; the volume ratio of mesitylene, dioxane and 6M acetic acid is 5 / 5 / 1, and the amount of the mixed solvent is such that 1.1 to 7.7 mL of the mixed solvent of mesitylene / dioxane / 6M acetic acid is used for every 0.16 mmol of the aldehyde monomer.
[0026] The heating reaction temperature in step (1) is 100-120° C., and the reaction time is 2-14 days.
[0027] After the reaction in step (1) is completed, the following purification step is further included: the prepared COFs nanosheets are washed with water and acetone and dried to obtain a neutral COFs material. The drying conditions after washing are vacuum 60-80°C, the drying time is 8-12h, and the neutral COFs powder obtained after drying is named Py-BPy.
[0028] The amount of the dibromoethane / acetonitrile mixed solution in step (2) satisfies the following requirement: every 60 mg of the neutral COFs material is added to the dibromoethane / acetonitrile mixed solution containing 10 to 30 mL of acetonitrile and 0.5 to 1.5 mL of dibromoethane.
[0029] The heating reaction time in step (2) is 1 to 24 hours, and the heating temperature is 100 to 140° C., wherein the stirring is only for the purpose of ensuring sufficient contact between the raw materials, and therefore there is no need to limit the stirring speed.
[0030] After the reaction in step (2) is completed, the following purification step is further included: the prepared COFs nanosheets are washed and dried with tetrahydrofuran (THF) to obtain a cationic COFs material. The drying conditions after washing are vacuum 60-80°C, the drying time is 8-12h, and the cationic COFs powder obtained after drying is named Py-BPy-Br.
[0031] In step (2), before dispersing the prepared COFs material into the basic electrolyte, it is preferably first placed in a high-speed planetary ball mill for ball milling until the lateral size of Py-BPy-Br is less than 100 nm, wherein the ball milling speed is 500 to 3000 r / min, and the ball milling time is 1 to 24 h; after ball milling, the obtained COFs powder is dried again to remove the moisture adsorbed during the drying process, wherein the drying conditions are vacuum drying at 80 to 100° C. for 12 to 24 h.
[0032] The colloidal electrolyte of the silicon-based lithium battery mentioned above is used in silicon-based lithium batteries, especially in ultra-fast charging and long calendar life silicon-based lithium batteries.
[0033] Preferably, the silicon-based lithium battery is preferably a silicon-based lithium-ion battery based on a high-nickel layered positive electrode.
[0034] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0035] 1) The Py-BPy-Br COFs prepared by the present invention are dispersed in the electrolyte in a mesoscopic form, and can produce strong non-covalent interactions with the microscopic components in the electrolyte, which can effectively change the solvation structure of lithium ions, accelerate the desolvation process of lithium ions, and improve the fast charging performance of the battery;
[0036] 2) The Py-BPy-Br COFs prepared by the present invention have the characteristics of porous structure and high specific surface area, and can strongly adsorb harmful HF in the electrolyte, thereby reducing the corrosion of HF on the positive and negative electrodes, thereby extending the calendar life of the battery;
[0037] 3) The colloidal electrolyte of the present invention can simultaneously improve the fast charging performance and calendar life of the battery. The mesoscopic Py-BPy-Br COFs can have a positive effect on the microscopic electrolyte components through multi-scale interactions, which has not been reported in the reported literature and patents, and is highly creative. Thanks to this, the colloidal electrolyte can effectively maintain the cycle stability of silicon-based lithium-ion batteries for a long time. Under the condition of 8C ultra-fast charging, the capacity retention rate is 78.6% to 82.3% within 200 cycles. The electrolyte also has the characteristics of rapid preparation and low cost, and has very good prospects for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The infrared spectrum of Py-BPy-Br prepared in Example 1;
[0039] Figure 2 is a photograph of the colloidal electrolyte obtained in Example 1;
[0040] Figure 3This is a cycle test diagram of a silicon-based lithium-ion battery assembled with the colloidal electrolyte prepared in Example 1;
[0041] Figure 4 This is a cycle test diagram of a silicon-based lithium-ion battery assembled with the colloidal electrolyte prepared in Example 2;
[0042] Figure 5 This is a cycle test diagram of a silicon-based lithium-ion battery assembled with the colloidal electrolyte prepared in Example 3. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0044] Unless otherwise specified, the reagents used in the examples can be purchased from the market.
[0045] The high nickel layered positive electrode (LiNi 0.6 Co 0.2 Mn 0.2 O2) can be purchased from Shenzhen Kejing Zhida Technology Co., Ltd.
[0046] Example 1
[0047] (1) Preparation of Py-BPy: 34 mg of 2,2'-bipyridine-5,5'-dicarboxaldehyde and 45.2 mg of 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene were added to a round-bottom flask, and 1.1 mL of a mixed solvent of mesitylene / dioxane / 6 M acetic acid was added at the same time, wherein the volume ratio of the three components of the mixed solvent was 5:5:1; the mixture was sealed after being filled with argon gas and heated at 100°C for 2 days; after the reaction, the mixture was washed with deionized water and acetone, and dried at 60°C in vacuum for 8 h to obtain a neutral Py-BPy powder.
[0048] (2) Preparation of Py-BPy-Br: 60 mg of the neutral Py-BPy material obtained above was dispersed in a dibromoethane / acetonitrile mixed solution, with 10 mL of acetonitrile and 0.5 mL of dibromoethane. The mixed solution was heated and stirred at 100°C for 1 h. After the reaction, it was washed with tetrahydrofuran and dried to obtain a cationic COFs material. The drying conditions after washing were vacuum at 60°C for 8 h, and the cationic Py-BPy-Br was obtained after drying.
[0049] (3) Preparation of Py-BPy-Br colloidal electrolyte: The prepared Py-BPy-Br powder was placed in a high-speed planetary ball mill for ball milling at a speed of 500 r / min for 1 h. After ball milling, the obtained COFs powder was dried again under vacuum at 80 °C for 12 h. The Py-BPy-Br powder was transferred to a glove box with an argon atmosphere, and the concentration of Py-BPy-Br dispersed in a commercial ester electrolyte (1.2M LiPF6 EC:EMC (w / w 3:7) + 10wt% FEC) was 0.1 g / L. After dispersion, the colloidal electrolyte was stirred for 1 h and ultrasonicated for 2 h. The resulting electrolyte was a Py-BPy-Br colloidal electrolyte.
[0050] (4) Assembling the colloidal electrolyte obtained in step (3) into a high nickel layered positive electrode (LiNi 0.6 Co 0.6 Mn 0.6 O2) and silicon-carbon anode silicon-based lithium-ion batteries.
[0051] The structural formula of Py-BPy-Br prepared in this embodiment is shown in Formula I. The pyrene ring in the structure can adsorb lithium ions, and pyridine can adsorb HF. Figure 1 This is the infrared spectrum of Py-BPy-Br prepared in this example. Figure 2 This is a photo of the electrolyte obtained in this example. It can be seen from the figure that the electrolyte produces an obvious Tyndall effect and is a colloidal electrolyte. Figure 3 The figure is a cycle test diagram of a silicon-based lithium-ion battery assembled with the colloidal electrolyte prepared in this embodiment. Figure 3 It can be seen that the silicon-based lithium-ion battery using colloidal electrolyte can still maintain good cycle stability at a current density of 8C (charging time of 7.5 minutes), and the capacity retention rate is 78.6% after 200 cycles. Figure 3 The BE in the experiment is a commercial ester electrolyte (1.2M LiPF6 EC:EMC (w / w 3:7) + 10wt% FEC) without Py-BPy-Br, and the capacity retention rate after 200 cycles is only 70.1%. Compared with the commercial ester electrolyte (1.2M LiPF6 EC:EMC (w / w 3:7) + 10wt% FEC) without any modification, the colloidal electrolyte prepared in this example shows better cycle stability, which indicates that the Py-BPy-Br CE colloidal electrolyte has a significant effect on improving the fast charging capability of the battery and the calendar life of the battery.
[0052] Example 2
[0053] (1) Preparation of Py-BPy: 34 mg of 2,2'-bipyridine-5,5'-dicarboxaldehyde and 45.2 mg of 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene were added to a round-bottom flask, and 4.4 mL of a mixed solution of mesitylene / dioxane / 6 M acetic acid was added at the same time, wherein the volume ratio of the mixed solution of mesitylene / dioxane / 6 M acetic acid was 5:5:1; the mixture was sealed after being filled with argon gas and heated at 110°C for 8 days; after the reaction, the mixture was washed with deionized water and acetone, and dried at 70°C in vacuum for 10 h to obtain a neutral Py-BPy powder.
[0054] (2) Preparation of Py-BPy-Br: 60 mg of the neutral Py-BPy material obtained above was dispersed in a dibromoethane / acetonitrile mixed solution, with 20 mL of acetonitrile and 1 mL of dibromoethane. The mixed solution was heated and stirred at 120°C for 12 h. After the reaction, it was washed with tetrahydrofuran and dried to obtain a cationic COFs material. The drying conditions after washing were vacuum at 70°C for 10 h, and the cationic Py-BPy-Br was obtained after drying.
[0055] (3) Preparation of Py-BPy-Br colloidal electrolyte: The prepared Py-BPy-Br powder was placed in a high-speed planetary ball mill for ball milling at a speed of 2000 r / min for 12 h. After ball milling, the obtained COFs powder was dried again under vacuum at 90 °C for 18 h. The Py-BPy-Br powder was transferred to a glove box with an argon atmosphere, and the concentration of Py-BPy-Br was dispersed in a commercial ester electrolyte (1.2M LiPF6 EC:EMC (w / w 3:7) + 10wt% FEC) at a concentration of 5 g / L. After dispersion, the colloidal electrolyte was stirred for 2 h and ultrasonicated for 4 h. The resulting electrolyte was a Py-BPy-Br colloidal electrolyte.
[0056] (4) Assembling the colloidal electrolyte obtained in step (3) into a high nickel layered positive electrode (LiNi 0.6 Co 0.6 Mn 0.6 O2) and silicon-carbon anode silicon-based lithium-ion batteries.
[0057] Figure 4 The figure is a cycle test diagram of a silicon-based lithium-ion battery assembled with the colloidal electrolyte prepared in this embodiment. Figure 4 It can be seen that the silicon-based lithium-ion battery using colloidal electrolyte can still maintain good cycle stability at a current density of 8C (charging time of 7.5 minutes), and the capacity retention rate is 82.3% after 200 cycles, which is significantly better than Figure 3 Commercial ester electrolytes in.
[0058] Example 3
[0059] (1) Preparation of Py-BPy: 34 mg of 2,2'-bipyridine-5,5'-dicarboxaldehyde and 45.2 mg of 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene were added to a round-bottom flask, and 7.7 mL of a mixed solvent of mesitylene / dioxane / 6 M acetic acid was added at the same time, wherein the volume ratio of the three components of the mixed solvent was 5:5:1; the mixture was sealed after being filled with argon gas and heated at 120°C for 14 days; after the reaction, the mixture was washed with deionized water and acetone, and dried at 80°C in vacuum for 12 h to obtain a neutral Py-BPy powder.
[0060] (2) Preparation of Py-BPy-Br: 60 mg of the neutral Py-BPy material obtained above was dispersed in a dibromoethane / acetonitrile mixed solution, with 30 mL of acetonitrile and 1.5 mL of dibromoethane. The mixed solution was heated and stirred at 140°C for 24 h. After the reaction, it was washed with tetrahydrofuran and dried to obtain a cationic COFs material. The drying conditions after washing were vacuum at 80°C for 12 h, and the cationic Py-BPy-Br was obtained after drying.
[0061] (3) Preparation of Py-BPy-Br colloidal electrolyte: The prepared Py-BPy-Br powder was placed in a high-speed planetary ball mill for ball milling at a speed of 3000 r / min for 24 h. After ball milling, the obtained COFs powder was dried again under vacuum at 100 °C for 24 h. The Py-BPy-Br powder was transferred to a glove box with an argon atmosphere, and the concentration of Py-BPy-Br dispersed in a commercial ester electrolyte (1.2M LiPF6 EC:EMC (w / w 3:7) + 10wt% FEC) was 10 g / L. After dispersion, the colloidal electrolyte was stirred for 3 h and ultrasonicated for 6 h. The obtained electrolyte was a Py-BPy-Br colloidal electrolyte.
[0062] (4) Assembling the colloidal electrolyte obtained in step (3) into a high nickel layered positive electrode (LiNi 0.6 Co 0.6 Mn 0.6 O2) and silicon-carbon anode silicon-based lithium-ion batteries.
[0063] Figure 5 The figure is a cycle test diagram of a silicon-based lithium-ion battery assembled with the colloidal electrolyte prepared in this embodiment. Figure 5It can be seen that the silicon-based lithium-ion battery using colloidal electrolyte can still maintain good cycle stability at a current density of 8C (charging time of 7.5 minutes), and the capacity retention rate is 80.4% after 200 cycles, which is significantly better than Figure 3 Commercial ester electrolytes in.
[0064] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A colloidal electrolyte for a silicon-based lithium battery, characterized in that: It is a colloidal electrolyte with covalent organic framework nanosheets as dispersants, which includes covalent organic framework materials and basic electrolytes, wherein the covalent organic framework materials are COFs synthesized with aldehyde monomers and amino monomers as raw materials, wherein the amino monomer is an amino monomer containing at least one functional group of pyrene ring, triazine, carbonyl, and carboxyl, and the aldehyde monomer is an aldehyde monomer containing at least one functional group of pyridine, furan, oxazole, imidazole, and thiophene.
2. The colloidal electrolyte of a silicon-based lithium battery according to claim 1, characterized in that: The covalent organic framework material has a structure shown in Formula I:
3. The colloidal electrolyte of a silicon-based lithium battery according to claim 1, characterized in that: The dosage of the covalent organic framework material and the basic electrolyte satisfies: the concentration of the covalent organic framework material in the basic electrolyte is 0.1-10 g / L.
4. The colloidal electrolyte of a silicon-based lithium battery according to claim 1, characterized in that: The basic electrolyte is a lithium-ion battery electrolyte; preferably a commercial ester electrolyte; more preferably (0.5-6) mol / L LiPF6-EC / EMC+(1-10) wt% FEC, wherein the mass ratio of EC to EMC in EC / EMC is 3:7 or 1:
1.
5. A method for preparing a colloidal electrolyte for a silicon-based lithium battery according to any one of claims 1 to 4, characterized in that The following steps are involved: The covalent organic framework material is uniformly dispersed in the basic electrolyte to obtain the colloidal electrolyte of the silicon-based lithium battery.
6. The method for preparing the colloidal electrolyte of a silicon-based lithium battery according to claim 5, characterized in that: The uniform dispersion refers to dispersion by stirring and / or ultrasound under the protection of argon atmosphere.
7. The method for preparing the colloidal electrolyte of a silicon-based lithium battery according to claim 5, characterized in that: The covalent organic framework material is prepared by the following method: (1) Preparation of neutral COFs material: aldehyde monomer, amino monomer and solvent are mixed and stirred to obtain a mixed solution, argon is filled into the mixed solution, and the mixed solution is sealed and heated. After the reaction is completed, a neutral COFs material is obtained; (2) Preparation of cationic COFs material: The neutral COFs material is dispersed in a dibromoethane / acetonitrile mixed solution, and the mixed solution is heated and stirred. After the reaction is completed, a cationic COFs material, i.e., a covalent organic framework material shown in Formula I, is obtained.
8. The method for preparing the colloidal electrolyte of a silicon-based lithium battery according to claim 7, characterized in that: The aldehyde monomer described in step (1) is 2,2'-bipyridine-5,5'-dicarboxaldehyde, and the amino monomer is 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene; The reaction molar ratio of the aldehyde monomer to the amino monomer in step (1) is 2:1; The solvent described in step (1) is a mixed solvent of mesitylene / dioxane / 6M acetic acid; The heating reaction temperature in step (1) is 100-120° C., and the reaction time is 2-14 days; The amount of the dibromoethane / acetonitrile mixed solution in step (2) satisfies the following requirement: every 60 mg of the neutral COFs material is added to the dibromoethane / acetonitrile mixed solution containing 10 to 30 mL of acetonitrile and 0.5 to 1.5 mL of dibromoethane; The heating reaction time in step (2) is 1 to 24 hours, and the heating temperature is 100 to 140° C.; After the reaction in step (2) is completed, the following purification step is also included: the prepared COFs nanosheets are washed with tetrahydrofuran and dried to obtain cationic COFs materials.
9. The method for preparing the colloidal electrolyte of a silicon-based lithium battery according to claim 5, characterized in that: In step (2), before dispersing the prepared COFs material into the basic electrolyte, it is first placed in a high-speed planetary ball mill for ball milling until the lateral size of Py-BPy-Br is less than 100 nm, wherein the ball milling speed is 500 to 3000 r / min and the ball milling time is 1 to 24 h; after ball milling, the obtained COFs powder is dried again to remove the water adsorbed during the drying process.
10. Use of the colloidal electrolyte for silicon-based lithium batteries according to any one of claims 1 to 4 in silicon-based lithium batteries.
Citation Information
Cited By
Preparation method of liquid lithium bis (fluorosulfonyl) imide
CN121247740A